Manufacturing method and testing and evaluating method of main speed reducer casing pore defect sample
By preparing long-shaped ingot samples with different grades of air pore defects, the long-term, high cost and high failure risk of air pore defect testing and evaluation of main reducer magnesium alloy cassette in the prior art is solved, and efficient and reliable are achieved test evaluation.
Patent Information
- Application Number
- CN202411113250.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-08-14
AI Technical Summary
When testing and evaluating the air hole defect of the main reducer magnesium alloy casing, the test cycle is long, the cost is high, the efficiency is low, and there is a great risk of failure.
A manufacturing method is adopted to prepare cold iron and heat treatment, combine core sand and molded sand to prepare a sand mold, pour magnesium alloy solution and sprinkle round insoluble matter of different diameters after solidification, forming a long with different levels of pore defects. The strip ingot was then stamped, surface treatment and heat treatment to prepare a single-grade pore defect sample for finishing into typical test pieces for testing and evaluation.
It greatly shortens the test cycle, reduces the testing cost, reduces the risk of failure, improves the testing efficiency and reliability of results, and is suitable for widespread promotion and application.
Smart Images

Figure CN118913825A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of casing defect testing and evaluation, and in particular, to a method for manufacturing a main reducer casing pore defect sample. In addition, the present invention also relates to a method for testing and evaluating a main reducer casing pore defect sample by testing and evaluating a long strip ingot sample manufactured by the method for manufacturing a main reducer casing pore defect sample. Background Art
[0002] The casing of the helicopter main reducer is usually a magnesium alloy casting. Magnesium alloy castings will have different levels of porosity defects during the casting process. This is caused by the gas that cannot be discharged in time during the solidification of the molten metal. For example, damp or rusted furnace charges, unclean surface, water vapor and other gases in the furnace gas, furnace body and ladle that have not been dried after repair, gas in the mold cavity, gas drawn in during casting, poor air permeability of the mold or mud core, etc. may lead to porosity defects and are therefore difficult to prevent. Different levels of porosity defects have different effects on the strength and life of magnesium alloy castings. If all main reducer casings with porosity defects are treated as scrap, it may cause unnecessary waste. At present, Class I castings of magnesium alloy casings have high stress levels in key areas, so the level of porosity defects is relatively high. Once defects exceeding the range specified by the standard appear, it will often lead to crack failure in the defective part of the casing, thus failing to meet performance requirements. Therefore, since the higher the level, the larger the porosity defect, the existing magnesium alloy casing casting acceptance standards stipulate that only level 1 porosity defects are allowed in key areas, and level 2-4 porosity defects are allowed in non-critical areas.
[0003] However, when the existing magnesium alloy castings with porosity defects are classified into defect levels, they often simply follow the relevant conversion standards. There is a lack of reliable data to determine the impact of different levels of porosity defects on the strength and life of the casing. It may happen that the porosity defects on some magnesium alloy casing castings do not meet the acceptance standards, but their strength and life meet the acceptance requirements, resulting in unnecessary waste. If, in order to obtain reliable data, a sufficient number of casing ingots containing different levels of porosity defects are directly cut from the main reducer magnesium alloy casing casting for testing and evaluation, it will be impossible to cut casing ingots containing different levels of porosity defects from the same main reducer magnesium alloy casing casting due to the randomness of porosity defects in the casting process of the main reducer magnesium alloy casing, and the casing ingots containing different levels of porosity defects cannot be finely processed into typical test pieces, resulting in a long test cycle, high cost, low test efficiency, and a large risk of failure. Summary of the invention
[0004] The present invention provides a method for manufacturing a main reducer casing pore defect sample and a test and evaluation method to solve the technical problems of long test cycle, high cost, low test efficiency and great risk of failure in the existing test and evaluation of main reducer casings with pore defects of different grades.
[0005] According to one aspect of the present invention, a method for manufacturing a main reducer casing air hole defect sample is provided, comprising the following steps: A1, preparing chill and heat treating the chill for repeated use; A2, preparing core sand into a sand core, preparing molding sand into a sand mold, and then combining the sand core, the sand mold and the chill into a sand mold, wherein the sand mold comprises a runner, a casting cavity arranged in a long strip shape and a riser connected to the casting cavity, a plurality of casting cavities are arranged in the sand mold at intervals and connected through the runner, and the riser and the casting cavity are arranged one by one; A3, melting a magnesium alloy block into a magnesium alloy solution, and then pouring the magnesium alloy solution into the sand mold, and after the pouring is completed, evenly sprinkling a plurality of circular insolubles of different diameters from the upper end of the riser to form a magnesium alloy casting by casting, and the magnesium alloy There are multiple long strip ingots on the gold ingot, and each long strip ingot has different levels of porosity defects; A4, taking out the magnesium alloy casting from the sand mold, removing the molding sand and core sand on the magnesium alloy casting, and then cutting the pouring riser on the magnesium alloy casting to obtain multiple long strip ingots, and then marking, surface treating and heat treating the long strip ingots in turn; A5, inspecting the long strip ingots for porosity defects, marking the areas occupied by porosity defects of different levels, and then processing the long strip ingots according to the areas occupied by porosity defects of different levels to process a single long strip ingot into multiple long strip ingot samples, and marking the multiple long strip ingot samples respectively, wherein each long strip ingot sample only has porosity defects of the same level, and the porosity defects are located at the center of the long strip ingot sample.
[0006] As a further improvement of the above technical solution:
[0007] Furthermore, in step A1, the specific steps of heat treatment are as follows: put the cold iron into a drying furnace for drying, keep it at 260℃-300℃ for 3h-4h, take out the cold iron from the drying furnace, and cool it naturally.
[0008] Furthermore, in step A1, when the storage time of the heat-treated cold iron exceeds 2 days, the cold iron needs to be kept at 150° C.-180° C. for 30 min-40 min before use.
[0009] Furthermore, the plurality of circular insoluble objects with different diameters include φ1 mm steel balls, φ2 mm steel balls and φ3 mm steel balls, and the surfaces of the steel balls are coated with a high temperature resistant coating.
[0010] Further, in step A3, melting the magnesium alloy block into a magnesium alloy solution specifically includes the following steps: preheating the crucible to 680°C-720°C, adding the magnesium alloy block into the crucible, and covering the crucible with a gas protection cover to introduce a protective gas into the crucible, wherein the ventilation rate is 15L / min-25L / min, and the heating temperature is 760°C-780°C; after the magnesium alloy block is completely melted, adding a preset weight of Mg-Zr intermediate alloy and stirring for 8min-12min; setting the heating temperature to 765°C-775°C, increasing the ventilation rate of the protective gas to 25L / min-35L / min, and then placing a refiner in the crucible and introducing argon for refining, wherein the ventilation rate of argon is 10L / min-20L / min, and the ventilation time is 12min-15min. After the refining is completed, removing the slag on the liquid surface of the crucible to obtain a magnesium alloy solution.
[0011] Furthermore, the Mg-Zr master alloy needs to be preheated at 100°C-200°C for at least 30 minutes before use.
[0012] Furthermore, in step A3, pouring the magnesium alloy solution into the sand mold specifically includes the following steps: controlling the crucible temperature of the magnesium alloy solution at 800°C-830°C, and pouring the magnesium alloy solution into the sand mold when the magnesium alloy solution drops to 765°C-775°C, and controlling the pouring time within 5s-15s.
[0013] Furthermore, in step A4, the specific steps of heat treatment are as follows: the long strip ingot is heated to 390℃-410℃ and kept warm for 1.5h-2.5h, and then continued to heat to 515℃-525℃ and kept warm for 6h-8h, and then quenched with a quenching medium of 60℃-80℃, and the quenching transfer time does not exceed 20s, and finally the long strip ingot is kept at 195℃-205℃ for 18h-24h.
[0014] Furthermore, in step A4, the specific steps of surface treatment are as follows: cleaning the flash and burrs on the surface of the long strip ingot, then using a gas medium to remove sand particles on the surface and in the crevices of the long strip ingot, then removing excess materials on the surface of the long strip ingot, and performing chromate treatment on the long strip ingot.
[0015] According to another aspect of the present invention, a method for testing and evaluating a main reducer casing pore defect sample is provided, which tests and evaluates a long strip ingot sample manufactured by the above-mentioned method for manufacturing a main reducer casing pore defect sample, and comprises the following steps: B1, using sand casting and machining to obtain a plurality of standard parts without metallurgical defects, and manufacturing a plurality of batches of long strip ingot samples, each batch of long strip ingot samples having a different pore defect level, and then fine-machining the plurality of batches of long strip ingot samples into smooth round rod-shaped test pieces, and then performing a pore defect inspection on the test pieces to remove the test pieces whose pore defect level and position do not meet the requirements, wherein the test pieces include tensile test pieces; Test pieces and fatigue test pieces; B2, carry out tensile performance tests on standard parts and tensile test pieces to obtain tensile test data including yield strength, ultimate strength, yield strength attenuation coefficient and ultimate strength attenuation coefficient of pore defects of different levels, and carry out group method fatigue performance tests on standard parts and fatigue test pieces to obtain test data for fitting fatigue performance curves, and carry out lifting method fatigue performance tests on standard parts and test pieces to obtain fatigue test data including fatigue limit and fatigue limit attenuation coefficient of pore defects of different levels; B3, evaluate the static strength and fatigue strength of pore defect sites of different levels on the main reducer casing through tensile test data and fatigue performance data.
[0016] The present invention has the following beneficial effects:
[0017] The manufacturing method of the main reducer casing air hole defect sample of the present invention comprises the following steps: preparing a chill to enable rapid cooling of subsequent castings after pouring, thereby avoiding metallurgical defects such as porosity and shrinkage cavities inside the castings, and heat treating the repeatedly used chill to eliminate residual thermal stress and thermal deformation of the chill, thereby avoiding the chill affecting the quality of the castings; preparing core sand into a sand core, and then preparing molding sand into a sand mold, and then combining the sand core, the sand mold and the chill into a sand mold, so that the castings can be cast through the sand mold; melting a magnesium alloy block into a magnesium alloy solution, and then The gold solution is poured into the sand mold, and after the pouring is completed, a plurality of circular insolubles of different diameters are evenly sprinkled from the upper end of the riser to ensure that after the magnesium alloy solution solidifies, the circular insolubles are located at a specified position of the magnesium alloy casting, and a gap is formed between the circular insolubles and the magnesium alloy casting. The space occupied by the circular insolubles can be approximately regarded as a circular pore defect, and a magnesium alloy casting having a plurality of long strips of ingots is formed by pouring, and each of the long strips of ingots has pore defects of different grades, that is, long strips of ingots with pore defects of different grades are prepared in batches. The invention relates to a method for preparing a magnesium alloy casting by forming a magnesium alloy casting into a plurality of strip-shaped ingots; taking out the magnesium alloy casting from the sand mold, removing the molding sand and core sand on the magnesium alloy casting, and then cutting the pouring riser on the magnesium alloy casting to obtain a plurality of strip-shaped ingots; then marking, surface treating and heat treating the strip-shaped ingots in sequence to ensure the quality of the strip-shaped ingots; performing a porosity defect inspection on the strip-shaped ingots, and marking the areas occupied by porosity defects of different grades; then processing the strip-shaped ingots according to the areas occupied by porosity defects of different grades to process a single strip-shaped ingot into a plurality of strip-shaped ingot samples; and then performing a plurality of The long strip ingot samples are marked separately, wherein each long strip ingot sample only has the same level of porosity defects, and the porosity defects are located at the center of the long strip ingot sample, which is convenient for subsequent testing and evaluation. The present scheme can batch-produce long strip ingot samples with different levels of porosity defects, which is convenient for subsequent fine processing into typical test pieces and testing, so as to evaluate the casings with different levels of porosity defects. Compared with the existing technology, the test cycle is greatly shortened, the test cost is reduced, and the risk of failure is reduced. It has strong practicality and is suitable for wide promotion and application.
[0018] The test and evaluation method of the main reducer casing pore defect sample of the present invention manufactures standard parts and long strip ingot samples, and then fine-processes the long strip ingot samples into smooth round rod-shaped test pieces to truly simulate the real internal hole defects existing in the main reducer casing, and according to the requirements of the tensile performance test and the fatigue performance test, the tensile test pieces and the fatigue test pieces are respectively obtained during fine processing, and then the test pieces are inspected for pore defects to remove the test pieces whose pore defect levels and positions do not meet the requirements, so as to improve the reliability of the test results, and the yield strength, ultimate strength, yield strength attenuation coefficient and ultimate strength containing pore defects of different levels are obtained by carrying out tensile performance tests on standard parts and tensile test pieces and comparing the test data of standard parts and tensile test pieces. At the same time, group fatigue performance tests of standard parts and fatigue test pieces are carried out to obtain test data for fitting fatigue performance curves, and lifting fatigue performance tests of standard parts and test pieces are carried out. By comparing the test data of standard parts and fatigue test pieces, fatigue test data of fatigue limit and fatigue limit attenuation coefficient of different levels of pore defects are obtained. The static strength and fatigue strength of different levels of pore defects on the main reducer casing can be evaluated through the tensile test data and fatigue performance data, so as to quantitatively determine the tolerance of different levels of pore defects in the main reducer casing during factory acceptance, thereby improving the qualified rate of the casing, saving the manufacturing cost of the casing, shortening the manufacturing cycle of the casing, and having strong practicality and suitable for wide promotion and application.
[0019] In addition to the above-described purposes, features and advantages, the present invention has other purposes, features and advantages. The present invention will be further described in detail with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] The drawings constituting a part of this application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:
[0021] Figure 1 It is a flowchart of the steps of a method for manufacturing a main reducer casing air hole defect sample according to a preferred embodiment of the present invention;
[0022] Figure 2 It is a structural schematic diagram of a magnesium alloy casting in a method for manufacturing a sample of a main reducer casing pore defect in a preferred embodiment of the present invention;
[0023] Figure 3 It is a structural schematic diagram of a long strip ingot in a method for manufacturing a sample of a main reducer casing pore defect in a preferred embodiment of the present invention;
[0024] Figure 4It is a structural schematic diagram of a long strip ingot sample in a method for manufacturing a main reducer casing air hole defect sample in a preferred embodiment of the present invention;
[0025] Figure 5 It is a flowchart of the steps of a method for testing and evaluating a sample of a main reducer casing air hole defect according to a preferred embodiment of the present invention;
[0026] Figure 6 It is a structural schematic diagram of a tensile test piece in a test and evaluation method for a main reducer casing air hole defect specimen in a preferred embodiment of the present invention;
[0027] Figure 7 It is a structural schematic diagram of a fatigue test piece in a test and evaluation method for a main reducer casing air hole defect specimen according to a preferred embodiment of the present invention. DETAILED DESCRIPTION
[0028] The embodiments of the present invention are described in detail below with reference to the accompanying drawings. However, the present invention can be implemented in many different ways as defined and covered below.
[0029] like Figure 1-Figure 4As shown, the manufacturing method of the main reducer casing air hole defect sample of the present embodiment includes the following steps: A1, preparing chill and heat treating the chill for repeated use; A2, preparing core sand into sand core, preparing molding sand into sand mold, and then combining the sand core, sand mold and chill into a sand mold, wherein the sand mold includes a cross runner, a casting block cavity arranged in a long strip shape and a riser connected to the casting block cavity, a plurality of casting block cavities are arranged in the sand mold at intervals and connected through the cross runner, and the riser and the casting block cavity are arranged one by one; A3, melting the magnesium alloy block into a magnesium alloy solution, and then pouring the magnesium alloy solution into the sand mold, and after the pouring is completed, a plurality of circular insolubles of different diameters are evenly sprinkled from the upper end of the riser to form a magnesium alloy casting by casting, and the magnesium alloy casting A plurality of long strip castings are arranged on the casting, and each of the long strip castings has different levels of pore defects; A4, taking out the magnesium alloy casting from the sand mold, removing the molding sand and core sand on the magnesium alloy casting, and then cutting the pouring riser on the magnesium alloy casting to obtain a plurality of long strip castings, and then marking, surface treating and heat treating the long strip castings in turn; A5, inspecting the long strip castings for pore defects, and marking the areas occupied by pore defects of different levels, and then processing the long strip castings according to the areas occupied by pore defects of different levels, so as to process a single long strip casting into a plurality of long strip casting samples, and marking the plurality of long strip casting samples respectively, wherein only pore defects of the same level exist on each long strip casting sample, and the pore defects are located at the center of the long strip casting sample. Optionally, in step A4, the specific steps of marking are: using a vibration pen to mark the blank number, melt batch number and sequence number on the long strip casting. Optionally, in step A5, the specific steps of marking are: using a vibration pen to impact and mark the blank number, the batch number and the porosity defect grade at the designated position of the long strip ingot sample. It should be understood that the main reducer casing is a magnesium alloy casting, and therefore the strength of the different grades of porosity defect parts on the main reducer casing is truly simulated by manufacturing the long strip ingot samples of different grades of porosity defects of the magnesium alloy. Optionally, the sand mold also includes a sprue for pouring a magnesium alloy solution in communication with the runner.
[0030] like Figure 1-Figure 4As shown, specifically, the manufacturing method of the main reducer casing porosity defect sample of the present invention comprises the following steps: preparing a chill to enable rapid cooling of subsequent castings after pouring, thereby avoiding metallurgical defects such as porosity and shrinkage cavities inside the castings, and heat treating the repeatedly used chill to eliminate residual thermal stress and thermal deformation of the chill, thereby avoiding the chill affecting the quality of the castings; preparing the core sand into a sand core, and then preparing the molding sand into a sand mold, and then combining the sand core, the sand mold and the chill into a sand mold, so that the castings can be cast through the sand mold; and melting the magnesium alloy block into a magnesium alloy solution. , and then pouring the magnesium alloy solution into the sand mold, and after the pouring is completed, a plurality of circular insolubles of different diameters are evenly sprinkled from the upper end of the riser to ensure that after the magnesium alloy solution solidifies, the circular insolubles are located at the designated position of the magnesium alloy casting, and a gap is formed between the circular insolubles and the magnesium alloy casting. Then, the space occupied by the circular insolubles can be approximately regarded as a circular pore defect, and a magnesium alloy casting having a plurality of long strips of ingots is formed by pouring, and each long strip of ingot has pore defects of different grades, that is, pore defects of different grades are prepared in batches. The invention relates to a method for producing a long strip ingot; taking out the magnesium alloy casting from the sand mold, removing the molding sand and core sand on the magnesium alloy casting, and then cutting the pouring riser on the magnesium alloy casting to obtain a plurality of long strip ingots, and then marking, surface treating and heat treating the long strip ingots in turn to ensure the quality of the long strip ingots; inspecting the long strip ingots for pore defects, and marking the areas occupied by pore defects of different grades, and then processing the long strip ingots according to the areas occupied by pore defects of different grades to process a single long strip ingot into a plurality of long strip ingot samples, and then conducting a surface treatment on the plurality of long strip ingot samples; Each strip casting sample is marked and printed separately, wherein each strip casting sample only has the same level of porosity defects, and the porosity defects are located at the center of the strip casting sample, which is convenient for subsequent testing and evaluation. This scheme can batch prepare strip casting samples with different levels of porosity defects, which is convenient for subsequent fine processing into typical test pieces and testing, so as to evaluate the casings with different levels of porosity defects. Compared with the existing technology, this scheme greatly shortens the testing cycle, reduces the testing cost, and reduces the risk of failure. It has strong practicality and is suitable for wide promotion and application.
[0031] In this embodiment, in step A1, the specific steps of heat treatment are as follows: put the cold iron into a drying furnace for drying, keep it warm at 260℃-300℃ for 3h-4h, take out the cold iron from the drying furnace, and cool it naturally. Specifically, by keeping the cold iron warm at 260℃-300℃ for 3h-4h, the residual thermal stress and thermal deformation in the cold iron can be eliminated to the greatest extent. Optionally, after the heat treatment is completed, check whether there is oil, rust, water droplets and other dirt on the working surface of the cold iron. If there is any, it should be thoroughly cleaned; check the appearance quality of the cold iron. The surface should be dense and should not have defects such as slag inclusions and sand holes. The cold iron deformation that affects positioning should be prohibited from use.
[0032] In this embodiment, in step A1, when the storage time of the heat-treated chilled iron exceeds 2 days, the chilled iron needs to be kept at 150°C-180°C for 30min-40min before use. Specifically, when the storage time of the heat-treated chilled iron exceeds 2 days, its thermal conductivity will change, and by keeping the chilled iron at 150°C-180°C for 30min-40min, the thermal stress generated by the excessive temperature difference between the chilled iron and the casting temperature of the magnesium alloy casting can be reduced, and the heat of the magnesium alloy casting can be better absorbed, the cooling efficiency can be improved, the casting can be quickly solidified and a good organizational structure and cross-energy can be obtained, and metallurgical defects such as porosity and shrinkage holes inside the casting can be avoided, and the service life of the chilled iron can also be extended. It should be understood that once metallurgical defects such as porosity and shrinkage cavities are generated inside the long strip ingot on the magnesium alloy casting, it will be impossible to accurately determine the impact of the porosity defects on the strength of the casing during subsequent testing and evaluation, and the casting cannot be used. Therefore, in the manufacturing process of magnesium alloy castings, metallurgical defects other than porosity defects must be avoided in the long strip ingot on the magnesium alloy casting.
[0033] In this embodiment, the plurality of circular insolubles of different diameters include φ1mm steel balls, φ2mm steel balls and φ3mm steel balls, and the surfaces of the steel balls are coated with a high temperature resistant coating. Specifically, by sprinkling φ1mm steel balls, φ2mm steel balls and φ3mm steel balls, and coating the surfaces of the steel balls with a high temperature resistant coating, the steel balls and the magnesium alloy solution are separated to prevent the two from merging, so that the pore defect morphology in the long strip ingot on the magnesium alloy casting is consistent with the real pore defect morphology, thereby forming three different levels of pore defects in the long strip ingot on the magnesium alloy casting, which is convenient for subsequent testing and evaluation of the long strip ingot samples with three different levels of pore defects.
[0034] In this embodiment, in step A3, melting the magnesium alloy block into a magnesium alloy solution specifically includes the following steps: preheating the crucible to 680°C-720°C, adding the magnesium alloy block into the crucible, and covering the crucible with a gas protection cover to introduce a protective gas into the crucible, wherein the ventilation rate is 15L / min-25L / min, and the heating temperature is 760°C-780°C; after the magnesium alloy block is completely melted, adding a preset weight of Mg-Zr master alloy, and stirring for 8min-12min; setting the heating temperature to 765°C-775°C, increasing the ventilation rate of the protective gas to 25L / min-35L / min, and then placing a refiner in the crucible and introducing argon gas for refining, the ventilation rate of argon gas is 10L / min-20L / min, and the ventilation time is 12min-15min. After the refining is completed, removing the slag on the liquid surface of the crucible to obtain a magnesium alloy solution. Specifically. The crucible is preheated to 680℃-720℃ to reduce the temperature difference, promote heat transfer, reduce thermal stress, maintain stability, and help the magnesium alloy block to be heated evenly, reduce impurities, and improve the casting quality. A protective gas with a ventilation rate of 15L / min-25L / min is introduced to prevent metal oxidation and improve the casting quality. The heating temperature is controlled at 760℃-780℃ to melt the magnesium alloy block quickly. After the magnesium alloy block is completely melted, a preset weight of Mg-Zr master alloy is added and stirred for 8min-12min to refine the magnesium alloy block. grains, improve the mechanical properties of magnesium alloy solution, improve the organizational structure of magnesium alloy castings, and improve the process performance of magnesium alloy castings; by setting the heating temperature to 765℃-775℃, increasing the ventilation rate of the protective gas to 25L / min-35L / min, and then placing a refiner in the crucible and introducing argon for refining, the ventilation rate of argon is 10L / min-20L / min, and the ventilation time is 12min-15min, so as to further remove impurities in the magnesium alloy solution, reduce defects, and improve metal properties, and improve the quality of magnesium alloy castings. It should be understood that the temperature parameters, ventilation rate and time parameters in this embodiment can maximize the guarantee that the magnesium alloy solution has few impurities after the magnesium alloy block is melted, the melting efficiency is high, and it is beneficial to improve the quality of castings. Optionally, the volume content of the protective gas is 98% CO2 and 2% SF6.
[0035] In this embodiment, the Mg-Zr master alloy is preheated at 100°C-200°C for at least 30 minutes before use. Specifically, by preheating the Mg-Zr master alloy at 100°C-200°C for at least 30 minutes before use, the utilization rate and effect of the master alloy can be improved, and the preheated master alloy can better play its role in refining grains, further improve the organizational structure and performance of magnesium alloy castings, improve the quality and yield rate of magnesium alloy castings, and improve production efficiency, while preventing adverse reactions and safety problems.
[0036] In this embodiment, in step A3, pouring the magnesium alloy solution into the sand mold specifically includes the following steps: controlling the temperature of the magnesium alloy solution out of the crucible to 800°C-830°C, and pouring the magnesium alloy solution into the sand mold when the magnesium alloy solution drops to 765°C-775°C, and controlling the pouring time to be within 5s-15s. Specifically, by controlling the temperature of the magnesium alloy solution out of the crucible to 800°C-830°C to ensure that the pouring temperature is appropriate, metallurgical defects such as shrinkage cavities, pores and cracks in the magnesium alloy castings are avoided, and the magnesium alloy solution is also helped to maintain stable fluidity and filling properties during the pouring process, making the casting structure dense and the grains fine, thereby improving the mechanical properties and surface quality of the magnesium alloy castings, and reducing energy consumption and costs; when the pouring time is controlled within 5s-15s, the magnesium alloy solution can quickly fill the mold cavity, reducing the cold caused by insufficient fluidity. It is beneficial to the discharge of gas in the mold cavity and the uniform solidification of magnesium alloy castings, and can also improve production efficiency, reduce production cycle and cost; when the pouring time is less than 5s, the scouring effect of magnesium alloy solution on the mold cavity wall is enhanced, which may cause defects such as sand swelling and sand washing, and is not conducive to the discharge of gas in the mold cavity and the uniform solidification of magnesium alloy castings; when the pouring time is more than 15s, the magnesium alloy solution cannot fill the mold cavity quickly, which may cause defects such as cold shut and insufficient pouring, and the production efficiency is relatively low, which increases the production cycle and cost.
[0037] In this embodiment, in step A4, the specific steps of heat treatment are as follows: the long strip ingot is heated to 390℃-410℃ and kept warm for 1.5h-2.5h, and then the temperature is further heated to 515℃-525℃ and kept warm for 6h-8h, and then quenched with a quenching medium of 60℃-80℃, and the quenching transfer time does not exceed 20s, and finally the long strip ingot is kept warm at 195℃-205℃ for 18h-24h. Specifically, the long strip ingot is heated to 390°C-410°C and kept warm for 1.5h-2.5h, and then continued to heat to 515°C-525°C and kept warm for 6h-8h, and then quenched with a quenching medium at 60°C-80°C to achieve solid solution treatment of the long strip ingot. The second phase in the long strip ingot is melted into the solid solution through solid solution treatment, and the re-precipitation of these phases is inhibited in the subsequent rapid cooling, thereby obtaining a refined grain structure, which is helpful to improve the mechanical properties and corrosion resistance of the long strip ingot, and at the same time can eliminate the component segregation in the long strip ingot, make the alloy elements more evenly distributed in the solid solution, and improve the strength and hardness of the casting, and improve the plasticity and toughness. Finally, the long strip ingot is kept at 195°C-205°C for 18h-24h to achieve aging treatment of the casting, and the residual stress of the long strip ingot is eliminated through aging treatment, and the strength and hardness of the long strip ingot are further improved, and the toughness and impact toughness of the long strip ingot are improved, the fatigue performance is improved, the corrosion resistance is improved, the material organization is stabilized, and the processing performance is improved. Optionally, the quenching medium is an aqueous solution.
[0038] In this embodiment, in step A4, the specific steps of surface treatment are as follows: cleaning the flash and burrs on the surface of the long strip ingot, then using a gas medium to remove the sand on the surface of the long strip ingot and the cracks, then removing the excess on the surface of the long strip ingot, and performing a chromate treatment on the long strip ingot. Specifically, by cleaning the flash and burrs on the surface of the long strip ingot, then using a gas medium to remove the sand on the surface of the long strip ingot and the cracks to improve the surface quality of the long strip ingot, then removing the excess on the surface of the long strip ingot, and performing a chromate treatment on the long strip ingot, a chromium oxide film is formed on the surface of the long strip ingot, the corrosion resistance of the long strip ingot is improved, the adhesion is enhanced, the gloss and color of the surface of the long strip ingot are improved, and the surface hardness of the long strip ingot is increased, and the dirt and grease on the surface of the long strip ingot are further cleaned.
[0039] like Figure 5-Figure 7As shown, the test and evaluation method of the main reducer casing porosity defect sample of the present embodiment is to test and evaluate the long strip ingot sample manufactured by the above-mentioned manufacturing method of the main reducer casing porosity defect sample, and comprises the following steps: B1, adopting sand casting and machining to obtain a plurality of standard parts without metallurgical defects, and manufacturing a plurality of batches of long strip ingot samples, each batch of long strip ingot samples having a different porosity defect grade, and then finely processing the plurality of batches of long strip ingot samples into smooth round rod-shaped test pieces, and then performing porosity defect inspection on the test pieces to remove the test pieces whose porosity defect grade and position do not meet the requirements, wherein the test pieces include tensile test pieces and Fatigue test pieces; B2, carry out tensile performance tests on standard parts and tensile test pieces to obtain tensile test data including yield strength, ultimate strength, yield strength attenuation coefficient and ultimate strength of pore defects of different levels, and at the same time carry out group fatigue performance tests on standard parts and fatigue test pieces to obtain test data for fitting fatigue performance curves, and carry out lifting method fatigue performance tests on standard parts and test pieces to obtain fatigue test data including fatigue limit and fatigue limit attenuation coefficient of pore defects of different levels; B3, evaluate the static strength and fatigue strength of pore defect sites of different levels on the main reducer casing through tensile test data and fatigue performance data.
[0040] like Figure 5-Figure 7 As shown, specifically, the test and evaluation method of the main reducer casing pore defect sample of the present invention manufactures standard parts and long strip ingot samples, and then fine-processes the long strip ingot samples into smooth round rod-shaped test pieces to truly simulate the real internal hole defects existing in the main reducer casing, and according to the requirements of the tensile performance test and the fatigue performance test, the tensile test pieces and the fatigue test pieces are respectively obtained during fine processing, and then the test pieces are inspected for pore defects to remove the test pieces whose pore defect levels and positions do not meet the requirements, so as to improve the reliability of the test results, and the yield strength, ultimate strength, yield strength and ultimate strength of the test pieces containing pore defects of different levels are obtained by carrying out tensile performance tests on standard parts and tensile test pieces and comparing the test data of the standard parts and the tensile test pieces. The tensile test data of strength attenuation coefficient and ultimate strength attenuation coefficient are obtained. At the same time, group fatigue performance tests of standard parts and fatigue test pieces are carried out to obtain test data for fitting fatigue performance curves, and lifting fatigue performance tests of standard parts and test pieces are carried out. By comparing the test data of standard parts and fatigue test pieces, fatigue test data of fatigue limit and fatigue limit attenuation coefficient containing different levels of pore defects are obtained. The static strength and fatigue strength of different levels of pore defects on the main reducer casing can be evaluated through the tensile test data and fatigue performance data, so as to quantitatively determine the tolerance of different levels of pore defects in the main reducer casing during factory acceptance, thereby improving the qualified rate of the casing, saving the manufacturing cost of the casing, and shortening the manufacturing cycle of the casing.
[0041] Optionally, when the long strip ingot sample is finely processed into a tensile test piece, the surface roughness of the tensile test piece is ensured to be Ra0.8 by turning, thereby ensuring the reliability of the test results in the subsequent tensile performance test. Optionally, when the long strip ingot sample is finely processed into a fatigue test piece, the surface roughness of the fatigue test piece is ensured to be Ra0.8 by turning, and then manual grinding or polishing with a polishing machine is used to ensure that the surface roughness of the fatigue test piece is Ra0.2, thereby ensuring the reliability of the test results in the subsequent fatigue performance test.
[0042] The specific calculation process of evaluating the static strength and fatigue strength attenuation coefficient of different levels of pore defects on the main reducer casing through tensile test data and fatigue performance data is as follows:
[0043] Static strength verification standard
[0044] The calculation formulas for yield strength reserve coefficient and ultimate strength reserve coefficient are as follows:
[0045]
[0046] Among them, K s is the yield strength reserve coefficient, K b is the ultimate strength reserve coefficient, σ lim is the maximum equivalent stress of the main reducer casing pore defect, σ b is the ultimate strength of magnesium alloy, σ s is the yield strength of magnesium alloy, S b is the ultimate strength attenuation coefficient of magnesium alloys with different levels of pore defects, S s is the yield strength attenuation coefficient of magnesium alloys with different levels of pore defects, σ bw is the median ultimate strength of the standard part, σ sw is the median yield strength of the standard part, σ bq is the median ultimate strength of the tensile test piece, σ sq is the median yield strength of the tensile test piece.
[0047] Fatigue strength verification standard
[0048] The fatigue equivalent stress is converted into stress cycle according to the Soderberg conversion formula. The calculation formula is as follows:
[0049] σ eq =σ a / (1-σ m / σ s )
[0050] Among them, σ eq is the dynamic value of the equivalent stress under symmetrical cycle in the main reducer casing pore defect area, σa is the dynamic value of the stress cycle in the elastic area of the main reducer casing pore, σ m It is the static value of stress cycle in the air hole defect area of the main reducer casing.
[0051] The calculation formula of low cycle fatigue strength reserve coefficient is as follows:
[0052]
[0053] Among them, K F低周 ≥0 is the low cycle fatigue strength reserve coefficient, σ eq低周 The low-cycle fatigue equivalent stress of the main reducer casing, S L is the fatigue limit of magnesium alloy, Fq is the low cycle fatigue limit attenuation coefficient of magnesium alloy with different levels of pore defects, σ -1w is the median fatigue casing of the standard part, σ -1q is the low cycle fatigue limit of the fatigue test piece.
[0054] If K F低周 ≥0, the low-cycle fatigue safety cycle number is 100,000 times. Otherwise, the low-cycle fatigue life is determined by the low-cycle safety fatigue SN curve. The basic equation of the low-cycle safety fatigue SN curve is:
[0055] S=F q ×S L [H+A×(10*N 低周 +C) -B ]
[0056] Among them, S is the dynamic stress of the main reducer casing pore defect area, N 低周 is the number of low cycle life cycles, and A, B, C, and H are fatigue performance constants.
[0057] The calculation formula of high cycle fatigue strength reserve coefficient is as follows:
[0058]
[0059] Among them, K F高周 is the high cycle fatigue strength reserve factor, σ eq高周 is the high cycle fatigue equivalent stress of the main reducer casing, k F is the fatigue strength reduction factor. If the part is not subjected to fatigue test, k F =3, if fatigue test is carried out, then k F =2,
[0060] If K F高周 ≥0, the high cycle fatigue life is infinite. Otherwise, the high cycle fatigue life is determined by the high cycle safety fatigue SN curve. The basic equation of the high cycle safety fatigue SN curve is:
[0061] S=F q ×S L [H+A×(N+C) -B ]
[0062] Where N is the number of high cycle life cycles.
[0063] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for manufacturing a main reducer casing air hole defect sample, characterized in that: The following steps are involved: A1, preparing chilled iron and heat-treating the chilled iron to be reused; A2, preparing the core sand into a sand core, and then preparing the molding sand into a sand mold, and then combining the sand core, the sand mold and the chill into a sand mold, wherein the sand mold includes a runner, a long strip-shaped ingot cavity and a riser connected to the ingot cavity, a plurality of ingot cavities are arranged in the sand mold at intervals and connected through the runner, and the riser and the ingot cavity are arranged one by one; A3, melting a magnesium alloy block into a magnesium alloy solution, and then pouring the magnesium alloy solution into a sand mold, and after the pouring is completed, evenly sprinkling a plurality of circular insolubles of different diameters from the upper end of the riser to form a magnesium alloy casting by casting, wherein the magnesium alloy casting has a plurality of long strips, and each of the long strips has pore defects of different levels; A4, taking out the magnesium alloy casting from the sand mold, removing the molding sand and core sand on the magnesium alloy casting, and then cutting the pouring riser on the magnesium alloy casting to obtain a plurality of long strip castings, and then marking, surface treating and heat treating the long strip castings in sequence; A5, inspect the long strip ingot for porosity defects, and mark the areas occupied by porosity defects of different grades, then process the long strip ingot according to the areas occupied by porosity defects of different grades, so as to process a single long strip ingot into multiple long strip ingot samples, and mark the multiple long strip ingot samples respectively, wherein each long strip ingot sample only has porosity defects of the same grade, and the porosity defects are located at the center of the long strip ingot sample.
2. The method for manufacturing a main reducer casing air hole defect sample according to claim 1, characterized in that: In step A1, the specific steps of heat treatment are as follows: Put the cold iron into the drying furnace for drying. After keeping it at 260℃-300℃ for 3h-4h, take out the cold iron from the drying furnace and let it cool naturally.
3. The method for manufacturing a main reducer casing air hole defect sample according to claim 1, characterized in that: In step A1, when the storage time of the heat-treated cold iron exceeds 2 days, the cold iron needs to be kept at 150°C-180°C for 30min-40min before use.
4. The method for manufacturing a main reducer casing air hole defect sample according to claim 1, characterized in that: The plurality of circular insoluble objects with different diameters include φ1 mm steel balls, φ2 mm steel balls and φ3 mm steel balls, and the surfaces of the steel balls are coated with a high temperature resistant coating.
5. The method for manufacturing a main reducer casing air hole defect sample according to any one of claims 1 to 4, characterized in that: In step A3, melting the magnesium alloy block into a magnesium alloy solution specifically includes the following steps: Preheat the crucible to 680°C-720°C, add the magnesium alloy block into the crucible, and cover the crucible with a gas protection cover to introduce protective gas into the crucible, wherein the ventilation rate is 15L / min-25L / min, and the heating temperature is 760°C-780°C; After the magnesium alloy block is completely melted, add a preset weight of Mg-Zr master alloy and stir for 8-12 minutes; The heating temperature is set to 765℃-775℃, and the ventilation rate of the protective gas is increased to 25L / min-35L / min. Then, a refiner is placed in the crucible and argon gas is introduced for refining. The ventilation rate of argon gas is 10L / min-20L / min, and the ventilation time is 12min-15min. After the refining is completed, the slag on the liquid surface of the crucible is removed to obtain a magnesium alloy solution.
6. The method for manufacturing a main reducer casing air hole defect sample according to claim 5, characterized in that: Mg-Zr master alloy needs to be preheated at 100℃-200℃ for at least 30 minutes before use.
7. The method for manufacturing a main reducer casing air hole defect sample according to any one of claims 1 to 4, characterized in that: In step A3, pouring the magnesium alloy solution into the sand mold specifically includes the following steps: The temperature of the magnesium alloy solution out of the crucible is controlled at 800°C-830°C, so that when the temperature of the magnesium alloy solution drops to 765°C-775°C, the magnesium alloy solution is poured into the sand mold, and the pouring time is controlled within 5s-15s.
8. The method for manufacturing a main reducer casing air hole defect sample according to any one of claims 1 to 4, characterized in that: In step A4, the specific steps of heat treatment are as follows: The long strip ingot is heated to 390℃-410℃ and kept warm for 1.5h-2.5h, then continued to heat to 515℃-525℃ and kept warm for 6h-8h, then quenched with a quenching medium of 60℃-80℃, and the quenching transfer time does not exceed 20s, and finally the long strip ingot is kept at 195℃-205℃ for 18h-24h.
9. The method for manufacturing a main reducer casing air hole defect sample according to any one of claims 1 to 4, characterized in that: In step A4, the specific steps of surface treatment are as follows: The flash and burrs on the surface of the long strip ingot are cleaned, and the sand on the surface and the gap of the long strip ingot is removed by using a gas medium, and then the excess on the surface of the long strip ingot is removed, and the long strip ingot is chromated.
10. A test and evaluation method for a main reducer casing air hole defect specimen, characterized in that: Testing and evaluating a long strip ingot sample manufactured by the method for manufacturing a main reducer casing porosity defect sample according to any one of claims 1 to 9 comprises the following steps: B1, using sand casting and machining to obtain multiple standard parts without metallurgical defects, and manufacturing multiple batches of long strip ingot specimens, each batch of long strip ingot specimens has different levels of porosity defects, and then fine-machining the multiple batches of long strip ingot specimens into smooth round rod-shaped test pieces, and then conducting porosity defect inspection on the test pieces to remove the test pieces whose porosity defect levels and positions do not meet the requirements, wherein the test pieces include tensile test pieces and fatigue test pieces; B2. Conduct tensile performance tests on standard parts and tensile test pieces to obtain tensile test data including yield strength, ultimate strength, yield strength attenuation coefficient and ultimate strength attenuation coefficient of pore defects of different levels. At the same time, conduct group fatigue performance tests on standard parts and fatigue test pieces to obtain test data for fitting fatigue performance curves. Conduct lifting fatigue performance tests on standard parts and test pieces to obtain fatigue test data including fatigue limit and fatigue limit attenuation coefficient of pore defects of different levels. B3, evaluate the static strength and fatigue strength of different levels of pore defects on the main reducer casing through tensile test data and fatigue performance data.
Citation Information
Patent Citations
Ultrahigh-cycle fatigue performance measuring method and measuring system
CN113720708A
Method for measuring zirconium content in magnesium alloy
CN117607129A
Topological optimization layout-based mounting leg type main reducer casing test piece optimization design method and mounting leg type main reducer casing test piece
CN118051986A
Magnesium-lithium alloy sand mold minimum casting wall thickness testing device
CN219511918U