Photosensitive resin composition of nitrogen-containing heterocyclic polysiloxane and application thereof
By introducing nitrogen-containing heterocyclic polysiloxane into the photosensitive resin composition, the dielectric constant and thermal expansion coefficient are reduced, and the problems of high dielectric constant and thermal stress of traditional polyimide materials are solved, thus achieving suitable application for semiconductors High performance insulation and protective film of the device.
Patent Information
- Application Number
- CN202410977367.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-19
AI Technical Summary
Traditional polyimide materials have a high dielectric constant, which is difficult to meet the needs of next-generation semiconductor packaging materials. At the same time, the thermal stress of their inorganic substrates causes layer warping, cracking or delamination, and the thermal expansion coefficient needs to be reduced to solve these problems. question.
Introduce a nitrogen-containing heterocycle polysiloxane into the photosensitive resin composition, and combines a precursor resin, a silane coupling agent, a photosensitive additive and a crosslinking agent to form a photosensitive resin with a low dielectric constant and a low thermal expansion coefficient. A composition is used to prepare a passivation film, a surface protective film and an interlayer insulating film of a semiconductor device.
The excellent dielectric properties and low thermal expansion coefficient of the photosensitive resin cured film are achieved, suitable for particle occlusion, surface protection or insulation of semiconductor components, and can be used to form interlayer insulation of multi-layer circuits and cover coating resistance of flexible copper clad plates. Solder film, etc.
Smart Images

Figure CN118915391A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a photosensitive resin composition and application thereof, in particular to a photosensitive resin composition of nitrogen-containing heterocyclic polysiloxane and application thereof, belonging to the technical field of polymer compounds. Background Art
[0002] Polyimide (PI) is a type of organic polymer material containing an imide ring. It has good thermal stability, chemical stability, electrical insulation and good mechanical properties. It is widely used in various components such as passivation films, surface protection films, and interlayer insulation films of semiconductor devices. Compared with non-photosensitive polyimide, photosensitive polyimide materials can be cured to form heat-resistant relief pattern coatings by coating, exposure, development and thermal imidization treatment of photosensitive polyimide, thereby greatly shortening the process.
[0003] The interlayer insulation film used for multi-layer metal interconnect circuits in semiconductor packaging requires the lowest possible dielectric constant and dielectric loss to minimize parasitic capacitance, thereby preventing signal transmission delays, crosstalk, and noise. Polyimide materials themselves have good temperature resistance, mechanical properties, and insulation properties, and are important materials for interlayer insulation films. However, the dielectric constant of traditional polyimide is relatively high (about 3.4), which is difficult to meet the needs of the next generation of semiconductor packaging materials, and low dielectric modification is required.
[0004] In addition, when PI materials are combined with inorganic materials such as metals and ceramics, the presence of thermal stress can cause the polymer layer and the inorganic substrate to warp, crack or delaminate. In order to avoid the thermal stress curling failure between PI and the substrate, how to reduce the thermal expansion coefficient of PI has become one of the most researched directions of PI. Summary of the invention
[0005] One of the purposes of the present invention is to provide a photosensitive resin composition, wherein a nitrogen-containing heterocyclic polysiloxane is introduced into the photosensitive resin composition to enhance the dielectric properties of a cured film and reduce the thermal expansion coefficient.
[0006] Another object of the present invention is to provide a photosensitive resin cured film obtained using the photosensitive resin composition of the present invention and a semiconductor device including a cured relief pattern formed using the photosensitive resin composition of the present invention.
[0007] According to one aspect of the present application, a photosensitive resin composition is provided, which has a very low dielectric constant and thermal expansion coefficient and can be used to form relief patterns such as passivation films, surface protection films and interlayer insulation films of semiconductor devices.
[0008] The photosensitive resin composition comprises a precursor resin, a nitrogen-containing heterocyclic polysiloxane, a silane coupling agent, a photosensitive auxiliary agent, a crosslinking agent and a solvent.
[0009] Furthermore, the viscosity of the photosensitive resin composition is 10 to 10000 cP, for example, 10 cP, 50 cP, 100 cP, 300 cP, 500 cP, 1000 cP, 1200 cP, 1500 cP, 2000 cP, 2500 cP, 3000 cP, 3500 cP, 4000 cP, 4500 cP, 5000 cP, 6000 cP, 7000 cP, 8000 cP, 9000 cP, or 10000 cP.
[0010] Optionally, the photosensitive resin composition has a viscosity of 500 to 5000 cP.
[0011] Optionally, the photosensitive resin composition has a viscosity of 1000 to 4000 cP.
[0012] Optionally, the photosensitive resin composition has a viscosity of 1500 to 3500 cP.
[0013] Furthermore, the precursor resin comprises at least one of a polymer having a structural unit represented by formula (1) and a polymer having a structural unit represented by formula (2);
[0014]
[0015] wherein i1 is selected from an integer between 2 and 200, such as 2, 5, 10, 30, 50, 80, 100, 130, 150, 180, and 200. i2 is selected from an integer between 2 and 50, such as 2, 5, 10, 20, 30, 40, and 50.
[0016] Preferably, the ratio of i1 to i2 is 100:2-20, for example, 100:2, 100:3, 100:4, 100:5, 100:6, 100:7, 100:8, 100:9, 100:10, 100:11, 100:12, 100:13, 100:14, 100:15, 100:16, 100:17, 100:18, 100:19, 100:20. More preferably, the ratio of i1 to i2 is 100:5-15.
[0017] In formula (1) and formula (2), X 1 A tetravalent organic group selected from a group having 4 to 40 carbon atoms;
[0018] Optionally, X 1 Selected from -COOR 7 Base-COOR 8The -CONH- group and the -CONH- group are ortho to each other and are aromatic groups or ester ring aliphatic groups.
[0019] Optionally, X 1 An organic group having 6 or more carbon atoms and containing an aromatic ring;
[0020] Optionally, X 1 At least one selected from the following structures (3), * represents the insertion site:
[0021]
[0022] In formula (1) and formula (2), X 2 It is selected from alicyclic tetravalent organic groups having 4 to 40 carbon atoms.
[0023] Optionally, X 2 At least one selected from the following structures (4), * represents an insertion site:
[0024]
[0025] In formula (1) and formula (2), Y 1 , Y 2 Each is independently selected from a divalent organic group having 2 to 40 carbon atoms.
[0026] Optionally, Y 1 , Y 2 Each independently selected from aromatic groups having 6 or more carbon atoms;
[0027] Optionally, Y 1 , Y 2 Each is independently selected from at least one of the following structures (5), * represents an insertion site:
[0028]
[0029] In formula (1), R 7 , R 8 Each is independently selected from a saturated aliphatic group having 1 to 4 carbon atoms, an organic group having a structure represented by the following formula (6), or a hydrogen atom.
[0030]
[0031] Optionally, R 7 , R 8 Each is independently selected from ethyl, methyl, hydroxyethyl methacrylate, and n-butyl.
[0032] In formula (6), R 9 , R 10 , R 11Each is independently selected from an organic group having 1 to 3 carbon atoms or a hydrogen atom.
[0033] Optionally, R 9 , R 10 From the viewpoint of photosensitivity, hydrogen atoms are preferred. 11 Preferably it is a hydrogen atom or a methyl group;
[0034] Optionally, m is an integer of 2 to 10, such as 2, 3, 4, 5, 6, 7, 8, 9, 10, preferably an integer of 2 to 4, from the perspective of photosensitivity.
[0035] Optionally, the precursor resin is selected from a precursor of a polyimide resin, a polyimide resin, or a precursor of a polyimide resin or a polyimide resin as main components.
[0036] Optionally, the precursor of the polyimide resin is selected from polyamide ester and / or polyamic acid.
[0037] Optionally, among all the structural units of the precursor resin, more than 50 mol% are structural units represented by formula (1) or formula (2), for example, 50 mol%, 60 mol%, 70 mol%, 80 mol%, 90 mol%, 95 mol%, preferably more than 70 mol%, more preferably more than 90 mol%.
[0038] Furthermore, other precursor resins may be contained as needed.
[0039] In order to improve the adhesion between the precursor resin layer formed by coating the photosensitive resin composition of the present invention onto the substrate and the substrate, when preparing the precursor resin, diaminosiloxanes such as 1,3-bis(3-aminopropyl)tetramethyldisiloxane and 1,4-bis(3-aminopropyldimethylsilyl)benzene can be used to copolymerize with the polyimide precursor.
[0040] After the amide polycondensation reaction is completed, the byproduct of the dehydration condensation agent in the reaction solution is filtered out as needed, and the reaction solution is put into a poor solvent such as water, aliphatic lower alcohol, or a mixture thereof to precipitate the polymer. The polymer is purified by repeating the operations of re-dissolving and re-precipitating as needed, and vacuum drying is performed to obtain a precursor resin. In order to improve the purity of the polymer, the polymer solution can also be passed through a column filled with an anion and / or cation exchange resin soaked in a suitable organic solvent to remove ionic impurities.
[0041] From the perspective of heat resistance and mechanical properties after heat treatment, the weight average molecular weight (Mw) of the above-mentioned precursor resin is preferably 1000 or more, and more preferably 5000 or more, based on the polystyrene conversion value of gel permeation chromatography (GPC). From the perspective of solubility of the photosensitive resin composition in the developer, the weight average molecular weight of the above-mentioned precursor resin is preferably 60000 or less, and more preferably 40000 or less. As a developing solvent for gel permeation chromatography, N-methyl-pyrrolidone or tetrahydrofuran is recommended. The molecular weight is obtained by a standard curve made using standard monodisperse polystyrene.
[0042] Optionally, the weight average molecular weight of the precursor resin is 10,000 to 40,000.
[0043] Optionally, the weight average molecular weight of the precursor resin is 15,000 to 30,000.
[0044] Optionally, the weight average molecular weight of the precursor resin is 15,000 to 25,000.
[0045] Optionally, the weight average molecular weight of the precursor resin is 18,000 to 25,000.
[0046] Furthermore, the nitrogen-containing heterocyclic polysiloxane is selected from at least one of the polymers represented by the following formula (7):
[0047]
[0048] In formula (7), Y is a nitrogen-containing heterocyclic organic group. Optionally, Y can be selected from one, two or more of the structures shown in formula (8) to formula (11) below, and * represents an insertion site:
[0049]
[0050] In formula (8) to formula (11), R 1 is selected from a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, or an alkoxy group having 1 to 20 carbon atoms. Specifically, the alkyl group or alkoxy group having 1 to 20 carbon atoms may be an alkyl group such as methyl, ethyl, propyl, isopropyl, butyl, tert-butyl, pentyl, hexyl, heptyl, octyl, nonyl, decyl, etc., and may be an alkoxy group such as hydroxyethyl methacrylate, hydroxyethyl acrylate, hydroxypropyl methacrylate, hydroxypropyl acrylate, etc. Preferably, R 1 Selected from hydrogen atom, methyl, ethyl, butyl, methacrylate hydroxyethyl.
[0051] In formula (8) to formula (11), the W group is selected from nitrogen-containing heterocyclic structures, such as structures containing triazole, tetrazolyl, triazine, imidazolyl, oxazolyl, etc.
[0052] Preferably, W is at least one of the structures ①, ②, and ③ in the following formula (12), and * represents an insertion site:
[0053]
[0054] In formula (12), R 2 , R 3 , R 4 , R 5 , R 6 Each independently selected from at least one of a hydrogen atom and a hydrocarbon group having 1 to 10 carbon atoms. The hydrocarbon group having 1 to 10 carbon atoms may be an alkyl group such as methyl, ethyl, propyl, isopropyl, butyl, tert-butyl, pentyl, hexyl, heptyl, octyl, nonyl, decyl, or a cycloalkyl group such as cyclopentyl or cyclohexyl, or an aromatic group such as phenyl or tolyl, or an aralkyl group such as benzyl, phenethyl, or phenylpropyl, or an unsaturated alkenyl group such as vinyl, allyl, butenyl, propenyl, isopropenyl, or phenylalkenyl.
[0055] Preferably, R 2 , R 3 , R 4 , R 5 , R 6 are independently selected from hydrogen atoms and saturated alkyl groups having 1 to 3 carbon atoms; more preferably, R 2 , R 3 , R 4 , R 5 , R 6 Each is independently selected from a hydrogen atom, a methyl group and an ethyl group.
[0056] The nitrogen-containing heterocyclic polysiloxane can be used alone or in combination of two or more. The nitrogen-containing heterocyclic polysiloxane has a significant promoting effect on the dielectric properties of precursor resins, especially polyimides, polyimide precursor heat-resistant resins and substrates.
[0057] Furthermore, the preparation method of the nitrogen-containing heterocyclic polysiloxane comprises the following steps:
[0058] Step 1, under gas protection, stirring and mixing the organic solvent, nitrogen-containing heterocyclic silane coupling agent monomer and catalyst;
[0059] Step 2, controlling the temperature of the mixture in step 1 at 0-40°C, adding water dropwise thereto, keeping the mixture warm for reaction after the addition is complete, and then raising the temperature to 50-100°C to continue the reaction;
[0060] Step 3: After the reaction, the organic layer is separated and the volatiles are removed by distillation to obtain a nitrogen-containing heterocyclic polysiloxane.
[0061] Furthermore, in step 1, the nitrogen-containing heterocyclic silane coupling agent monomer is selected from at least one of the structures represented by the following formula (13):
[0062]
[0063] In formula (13), R 1 The definition of W is consistent with the above definition.
[0064] In formula (13), R 12 is selected from a hydrocarbon group having 1 to 10 carbon atoms, which may be an alkyl group such as methyl, ethyl, propyl, isopropyl, butyl, tert-butyl, pentyl, hexyl, heptyl, octyl, nonyl, decyl, etc., a cycloalkyl group such as cyclopentyl, cyclohexyl, etc., an aromatic group such as phenyl, tolyl, an aralkyl group such as benzyl, phenethyl, phenylpropyl, etc., and an unsaturated alkenyl group such as vinyl, allyl, butenyl, propenyl, isopropenyl, phenylalkenyl, etc. Preferably, R 12 is a saturated alkyl group having 1 to 10 carbon atoms, more preferably, R 12 It is methyl or ethyl.
[0065] Furthermore, when the W group is When the nitrogen-containing heterocyclic silane coupling agent monomer represented by formula (13) is prepared by referring to the preparation method in patent ZL202111145299.6.
[0066] Furthermore, when the W group is
[0067] When, the preparation method of the nitrogen-containing heterocyclic silane coupling agent monomer represented by formula (13) is:
[0068] Category 1: Amide-based nitrogen-containing heterocyclic silane coupling agent monomers:
[0069] The oxazole diamine or imidazole diamine is mixed with a solvent, and then the silane coupling agent SANAH or 3-(trimethoxysilyl)propyl succinic anhydride is slowly added in an amount twice the molar amount of the diamine. After the addition is completed, the reaction is continued at 23-26° C. for 20-22 hours. After the reaction is completed, the nitrogen-containing heterocyclic silane coupling agent monomer of the amic acid type is obtained by distillation under reduced pressure and purification.
[0070] The second category: imide nitrogen-containing heterocyclic silane coupling agent monomer:
[0071] The oxazole diamine or imidazole diamine is mixed with a solvent, and then the silane coupling agent SANAH or 3-(trimethoxysilyl)propyl succinic anhydride is slowly added in a molar amount twice that of the diamine. After the addition is completed, the reaction is continued at 23-26° C. for 20-22 hours, and then a base and anhydride are added to the reaction system for imidization. After the reaction is completed, the solvent, unreacted raw materials and by-products in the system are removed by reduced pressure distillation to obtain an imide-type nitrogen-containing heterocyclic silane coupling agent monomer.
[0072] Category 3: Amide ester nitrogen-containing heterocyclic silane coupling agent monomers:
[0073] The oxazole diamine or imidazole diamine is mixed with a solvent, and then the silane coupling agent SANAH or 3-(trimethoxysilyl)propyl succinic anhydride is slowly added in a molar amount twice that of the diamine. After the addition is completed, the reaction is continued at 23-26° C. for 20-22 hours, and then an esterification agent (N,N-dimethylformamide dimethyl acetal, N,N-dimethylformamide diethyl acetal, etc.) is added to the system for esterification reaction. After the reaction is completed, it is distilled under reduced pressure to obtain an amide ester nitrogen-containing heterocyclic silane coupling agent monomer.
[0074] Optionally, in step 1, the organic solvent is selected from at least one of hydrocarbons, ketones, esters, ethers, and alcohols. The hydrocarbons include, for example, toluene and xylene; the ketones include, for example, methyl ethyl ketone, methyl isobutyl ketone, methyl n-amyl ketone, diethyl ketone, cyclohexanone, etc.; the esters include, for example, ethyl acetate, n-butyl acetate, isopentyl acetate, propylene glycol monomethyl ether acetate, 3-methoxybutyl acetate, ethyl lactate, etc.; the ethers include, for example, ethylene glycol dimethyl ether, ethylene glycol diethyl ether, tetrahydrofuran, dioxane, etc.; the alcohols include, for example, 1-hexanol, 4-methyl-2-pentanol, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol mono-n-propyl ether, ethylene glycol mono-n-butyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol mono-n-propyl ether, etc. The organic solvent is preferably one that is immiscible with water, and these organic solvents may be used alone or in combination of two or more.
[0075] Optionally, in step 1, the catalyst may be one of an acid, an alkali metal compound, an organic base, and the like. Examples of the acid include hydrochloric acid, p-toluenesulfonic acid, and the like; examples of the alkali metal compound include, for example, sodium hydroxide, potassium hydroxide, sodium methoxide, potassium methoxide, sodium ethoxide, potassium ethoxide, and the like; examples of the organic base include, for example, primary and secondary organic amines such as ethylamine, diethylamine, piperazine, piperidine, pyrrolidine, and pyrrole; tertiary organic amines such as triethylamine, tri-n-propylamine, tri-n-butylamine, pyridine, 4-dimethylaminopyridine, and diazacycloundecene; and quaternary organic amines such as tetramethylammonium hydroxide, and the like. Among these organic bases, triethylamine, tri-n-propylamine, tri-n-butylamine, pyridine, 4-dimethylaminopyridine, and tetramethylammonium hydroxide are preferred.
[0076] Optionally, in step 1, the mass ratio of the nitrogen-containing heterocyclic silane coupling agent monomer to the organic solvent is 1:0.5-20, for example, 1:0.5, 1:1, 1:2, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9, 1:10, 1:12, 1:14, 1:16, 1:18, 1:20, preferably 1:1-10.
[0077] Optionally, in step 1, the mass ratio of the nitrogen-containing heterocyclic silane coupling agent monomer to the catalyst is 1:0.01 to 0.3, for example, 1:0.01, 1:0.02, 1:0.03, 1:0.04, 1:0.05, 1:0.06, 1:0.07, 1:0.08, 1:0.09, 1:0.1, 1:0.15, 1:0.2, 1:0.25, 1:0.3, preferably 1:0.01 to 0.1.
[0078] Optionally, in step 2, the mass ratio of the nitrogen-containing heterocyclic silane coupling agent monomer to water is 1:1-50, for example, 1:1, 1:2, 1:5, 1:10, 1:15, 1:20, 1:25, 1:30, 1:35, 1:40, 1:45, 1:50, preferably 1:2-20.
[0079] Optionally, in step 2, the water is added dropwise for 0.5 to 5 h, for example, 0.5 h, 1 h, 2 h, 3 h, 4 h, or 5 h.
[0080] Optionally, in step 2, water is added dropwise at 0-40°C, and the temperature can be 0°C, 5°C, 10°C, 15°C, 20°C, 25°C, 30°C, 35°C, 40°C. After the water is added dropwise, the reaction is kept warm for 3-6 hours, such as 3 hours, 4 hours, 5 hours, 6 hours. After the reaction, the temperature is continued to rise to 50-100°C, such as 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C, 95°C, 100°C, and the reaction is continued at this temperature for 6-12 hours, such as 6 hours, 7 hours, 8 hours, 9 hours, 10 hours, 11 hours, 12 hours.
[0081] Furthermore, the silane coupling agent includes at least one of a nitrogen-containing heterocyclic silane coupling agent, a urea-based silane coupling agent, a mercapto silane coupling agent, a vinyl-based silane coupling agent, and an epoxy-based silane coupling agent.
[0082] The nitrogen-containing heterocyclic silane coupling agent can be selected from at least one of the following structural formulas (14-1) and (14-2):
[0083]
[0084]
[0085] The preparation method of the nitrogen-containing heterocyclic silane coupling agent in formula (14-1) and formula (14-2) can refer to the preparation method of the nitrogen-containing heterocyclic silane coupling agent monomer of the present application.
[0086] The nitrogen-containing heterocyclic silane coupling agent can also be selected from at least one of the following structural formulas (14-3):
[0087]
[0088] The preparation method of the nitrogen-containing heterocyclic silane coupling agent of formula (14-3) is as follows:
[0089] Category 1: Amide-based nitrogen-containing heterocyclic silane coupling agent monomers:
[0090] The nitrogen-containing heterocyclic monoamine is mixed with a solvent, and then a silane coupling agent SANAH or 3-(trimethoxysilyl)propyl succinic anhydride is slowly added in a molar amount of one times the nitrogen-containing heterocyclic monoamine. After the addition is completed, the reaction is continued at 23-26° C. for 20-22 hours. After the reaction is completed, the nitrogen-containing heterocyclic silane coupling agent monomer of the amide acid type is obtained by distillation under reduced pressure and purification.
[0091] The second category: imide nitrogen-containing heterocyclic silane coupling agent monomer:
[0092] The nitrogen-containing heterocyclic monoamine is mixed with a solvent, and then a silane coupling agent SANAH or 3-(trimethoxysilyl)propyl succinic anhydride in a molar amount of one times the nitrogen-containing heterocyclic monoamine is slowly added, and after the addition is completed, the reaction is continued at 23-26° C. for 20-22 hours, and then a base and anhydride are added to the reaction system for imidization. After the reaction is completed, the solvent, unreacted raw materials and by-products in the system are removed by reduced pressure distillation to obtain an imide-type nitrogen-containing heterocyclic silane coupling agent monomer.
[0093] Category 3: Amide ester nitrogen-containing heterocyclic silane coupling agent monomers:
[0094] The nitrogen-containing heterocyclic monoamine is mixed with a solvent, and then a silane coupling agent SANAH or 3-(trimethoxysilyl)propyl succinic anhydride in a molar amount of one times the nitrogen-containing heterocyclic monoamine is slowly added. After the addition is completed, the reaction is continued at 23-26° C. for 20-22 hours, and then an esterification agent (N,N-dimethylformamide dimethyl acetal, N,N-dimethylformamide diethyl acetal, etc.) is added to the system for esterification reaction. After the reaction is completed, reduced pressure distillation is performed to obtain an amide ester nitrogen-containing heterocyclic silane coupling agent monomer.
[0095] The urea-based silane coupling agent can be selected from 3-urea-based propyltriethoxysilane (Nanjing Xuanhao New Material Technology, XH-1160), 3-urea-based propyltrimethoxysilane (Nanjing Dimonte, DMT-116), 1-propyl-1-(triethoxysilyl)methylurea (Nanjing Xuanhao New Material Technology, XH-712), etc., or the structure of the following formula (15):
[0096]
[0097] The urea-based silane coupling agent of formula (15) was prepared by referring to patent CN111825884B.
[0098] Examples of epoxy-based silane coupling agents include (3-glycidoxypropyl)trimethoxysilane (KH-560), (8-glycidoxyoctyl)trimethoxysilane (Japan Shin-Etsu Chemical, KBM-4803), and (3-glycidoxypropyl)trimethoxysilane (Japan Shin-Etsu Chemical, KBM-403).
[0099] Examples of mercapto-based silane coupling agents include 3-(triethoxysilylthio)propyltrimethoxysilane (Shin-Etsu Chemical, X-12-1056ES), 3-(trimethoxysilyl)-1-propanethiol (Maitu High-Tech Materials, A-189), γ-thiopropyltriethoxysilane (Nanjing Xuanhao New Materials Technology, KH-580), and the like.
[0100] Examples of vinyl silane coupling agents include vinyl triethoxysilane (Nanjing Demonte, KH-151), p-vinyl phenyl trimethoxy silane (Japan Shin-Etsu Chemical, KBM-1403), etc., but are not limited thereto.
[0101] It has been verified by experiments that the silane coupling agent is preferably one or two of a nitrogen-containing heterocyclic silane coupling agent and an epoxy silane coupling agent, and more preferably a nitrogen-containing heterocyclic silane coupling agent and an epoxy silane coupling agent are used in combination.
[0102] Furthermore, the photosensitive auxiliary agent includes a photopolymerization initiator and / or a photoacid generator. The photosensitive auxiliary agent varies according to the components of the photosensitive resin composition.
[0103] First, the case of negative type is described. In this case, a photopolymerization initiator is used as a photosensitizing agent, preferably a photo radical polymerization initiator, such as acetophenone compounds, biimidazole compounds, triazine compounds, oxime compounds or a mixture of two or more thereof. Preferred examples of the photopolymerization initiator include 1-(4-phenylthio-phenyl)-octane-1,2-dione-2-oxime-0-benzoate, 2-hydroxy-2-methyl-1-phenylpropane-1-one, 1-hydroxycyclohexyl phenyl ketone, dibenzyl ketone, 4-benzoyl-4'-methyldiphenyl ketone, fluorenone, 2,2'-diethoxyacetophenone, 2-hydroxy-2-methylpropiophenone, 3-{4-[2,4-bis(trichloromethyl)-s-triazin-6-yl]phenylthio}propionic acid, 1,1,1,3,3,3-hexafluoroisopropyl-3-{4-[2,4-bis(trichloromethyl)-s-triazin-6-yl]phenylthio}propionic acid, and 2-oxiranyl-2-{4-[2,4-bis(trichloromethyl)-s-triazin-6-yl]phenylthio}acetate, but the present invention is not limited thereto. Among the above-mentioned photopolymerization initiators, oxime compounds are more preferred from the viewpoint of photosensitivity.
[0104] Next, the case where the positive type is desired is described. In this case, a photoacid generator is used as a photosensitizer, and specifically, a quinone diazide compound, an onium salt, a halogen-containing compound, etc. can be used, but from the viewpoint of solvent solubility and storage stability, an ester compound obtained by ester-bonding a sulfonic acid of a quinone diazide to a polyhydroxy compound is preferred, and examples of the polyhydroxy compound include: 2,6-dimethoxymethyl-4-tert-butylphenol, 2,6-dimethoxy-p-cresol, 2,6-diacetoxymethyl-p-cresol, tetrahydroxybenzophenone, etc., but are not limited thereto. Commercially available quinonediazide compounds are preferred, for example, NT-300 (esterification reaction product of 2,3,4-tetrahydroxybenzophenone and 6-diazo-5,6-dihydroxy-5-oxy-1-naphthalenesulfonic acid), 4NT-350, 4NT-300 (esterification reaction product of 2,3,4,4-tetrahydroxybenzophenone and 6-diazo-5,6-dihydroxy-5-oxy-1-naphthalenesulfonic acid), esterification reaction product of tris(4-hydroxyphenyl)ethane (HP-190) and 6-diazo-5,6-dihydroxy-5-oxy-1-naphthalenesulfonic acid (manufactured by Toyo Gosei Kogyo Co., Ltd., Japan), etc.
[0105] Furthermore, the crosslinking agent can promote the polymerization reaction or the polymerization reaction of the addition polymerizable compound itself to form a crosslinked network structure. The crosslinking agent includes an addition polymerizable compound and / or a thermal crosslinking agent. The addition polymerizable compound can further improve the heat resistance and chemical resistance of the cured film formed by the photosensitive resin composition.
[0106] As the negative photosensitive composition, the crosslinking agent may be an addition polymerizable compound, and examples thereof include tetraethylene glycol dimethacrylate, diethylene glycol diacrylate, triethylene glycol diacrylate, diethylene glycol dimethacrylate, triethylene glycol dimethacrylate, tetraethylene glycol dimethacrylate, trimethylolpropane diacrylate, trimethylolpropane triacrylate, trimethylolpropane dimethacrylate, etc., but are not limited thereto. The above-mentioned addition polymerizable compounds may be used alone or in combination of two or more thereof.
[0107] As the positive photosensitive composition, the crosslinking agent may be a thermal crosslinking agent, and examples thereof include, but are not limited to, DMOM-PTBP-MF, TMOM-BP, HMOM-TPHAP, DML-PC, DMOM-MBPC, HMOM-TPHAP (the above are trade names, manufactured by Honshu Chemical Industry Co., Ltd.), MX-100LM (the above are trade names, manufactured by Sanwa Chemical Co., Ltd.), etc. The above thermal crosslinking agents may be used alone or in combination of two or more.
[0108] Furthermore, the solvent is selected from at least one of N-methylpyrrolidone, methyl ethyl ketone, acetone, γ-butyrolactone, ethyl acetate, ethyl lactate, toluene, xylene, diethylene glycol monobutyl ether, propylene glycol methyl ether, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, tetrahydrofuran, dioxane, N,N-dimethylformamide, N,N-dimethylacetamide, and dimethyl sulfoxide.
[0109] Further, the mass ratio of the precursor resin to the nitrogen-containing heterocyclic polysiloxane is 100:0.01-20, for example, any value in 1:0.01, 1:0.03, 1:0.05, 1:0.08, 1:0.1, 1:0.3, 1:0.5, 1:0.8, 1:1, 1:2, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9, 1:10, 1:11, 1:12, 1:13, 1:14, 1:15, 1:16, 1:17, 1:18, 1:19, 1:20, or a range between any two of them.
[0110] Preferably, the mass ratio of the precursor resin to the nitrogen-containing heterocyclic polysiloxane is 100:0.1-10.
[0111] More preferably, the mass ratio of the precursor resin to the nitrogen-containing heterocyclic polysiloxane is 100:1-10.
[0112] Furthermore, the mass ratio of the precursor resin to the silane coupling agent is 100:0.1-5, for example, any value among 1:0.1, 1:0.3, 1:0.5, 1:0.8, 1:1, 1:2, 1:3, 1:4, 1:5 or any range value between two of them.
[0113] Preferably, the mass ratio of the precursor resin to the silane coupling agent is 100:1-5.
[0114] Furthermore, the mass ratio of the precursor resin to the photosensitive auxiliary agent is 100:0.1-30, for example, any value among 1:0.1, 1:0.3, 1:0.5, 1:0.8, 1:1, 1:3, 1:5, 1:8, 1:10, 1:13, 1:15, 1:18, 1:20, 1:23, 1:25, 1:28, 1:30, or any range value between two of them.
[0115] Preferably, the mass ratio of the precursor resin to the photosensitizing agent is 100:0.5-25.
[0116] More preferably, the mass ratio of the precursor resin to the photosensitizing agent is 100:0.5-20.
[0117] Furthermore, the mass ratio of the precursor resin to the cross-linking agent is 100:0.5-30, for example, any value of 1:0.5, 1:0.8, 1:1, 1:3, 1:5, 1:8, 1:10, 1:13, 1:15, 1:18, 1:20, 1:23, 1:25, 1:28, 1:30 or any range between two values.
[0118] Preferably, the mass ratio of the precursor resin to the cross-linking agent is 100:1-20.
[0119] Further, the mass ratio of the precursor resin to the solvent is 100:80-5000, for example, 100:80, 100:100, 100:130, 100:150, 100:180, 100:200, 100:230, 100:250, 100:280, 100:300, 100:330, 100:350, 100:380, 100: Any value among 400, 100:500, 100:600, 100:700, 100:800, 100:900, 100:1000, 100:1500, 100:2000, 100:2500, 100:3000, 100:3500, 100:4000, 100:4500, 100:5000, or any range between them.
[0120] Preferably, the mass ratio of the precursor resin to the solvent is 100:100-1000.
[0121] More preferably, the mass ratio of the precursor resin to the solvent is 100:150-400.
[0122] Furthermore, in order to improve the stability of the viscosity and sensitivity of the photosensitive resin composition solution containing a solvent during storage, the negative photosensitive resin composition may further include a polymerization inhibitor.
[0123] Optionally, the inhibitor includes at least one of hydroquinone, p-hydroxyanisole, N-nitrosodiphenylamine, phenothiazine, p-tert-butylcatechol, N-phenylnaphthylamine, ethylenediaminetetraacetic acid, 1,2-cyclohexanediaminetetraacetic acid, 2,6-di-tert-butyl-p-methylphenol, 5-nitroso-8-hydroxyquinoline, and N-nitroso-N(1-naphthyl)hydroxylamine ammonium salt.
[0124] Optionally, the mass ratio of the precursor resin to the inhibitor is 100:0.01-15, for example, any value among 1:0.01, 1:0.03, 1:0.05, 1:0.08, 1:0.1, 1:0.3, 1:0.5, 1:0.8, 1:1, 1:2, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9, 1:10, 1:11, 1:12, 1:13, 1:14, 1:15, or any range value between any two of them.
[0125] Preferably, the mass ratio of the precursor resin to the polymerization inhibitor is 100:0.1-10.
[0126] More preferably, the mass ratio of the precursor resin to the polymerization inhibitor is 100:0.5-5.
[0127] According to another aspect of the present application, a method for preparing the above-mentioned photosensitive resin composition is provided, comprising at least the following steps:
[0128] The precursor resin, the nitrogen-containing heterocyclic polysiloxane, the silane coupling agent, the photosensitive auxiliary agent, the crosslinking agent and the solvent are mixed to obtain the photosensitive resin composition.
[0129] Optionally, it specifically includes:
[0130] In a three-necked flask equipped with a stirrer, the precursor resin and the inhibitor are dissolved in a solvent (if the inhibitor is present), the nitrogen-containing heterocyclic polysiloxane and the silane coupling agent are added, and stirring is continued until completely dissolved, and then the photosensitive auxiliary agent and the cross-linking agent are added in sequence, and after stirring and dissolving, filter pressing (using a filter with a pore size of 0.1 μm to 5 μm) to obtain the photosensitive resin composition.
[0131] According to another aspect of the present application, a photosensitive resin cured film is provided, which is obtained by curing the above-mentioned photosensitive resin composition. The photosensitive resin cured film can be used for particle shielding, surface protection or insulation of semiconductor elements, and insulating layers and interlayer insulating layers of OLED elements.
[0132] According to another aspect of the present application, a method for preparing the above-mentioned photosensitive resin cured film is provided, comprising at least the following steps:
[0133] The photosensitive resin composition is applied to a surface of a substrate and heat-treated in an inert gas atmosphere to obtain the photosensitive resin cured film.
[0134] The substrate includes, but is not limited to, a copper sheet, a copper alloy sheet, a silicon sheet, a ceramic sheet, a titanium sheet, a glass sheet, an ITO glass, etc. As the coating method, there can be cited: a spray coating method, a spin coating method, a doctor blade method and the like. The coating film thickness will also be different due to the different coating methods, rotation speeds, viscosities, composition components, etc. In the present invention, a 4-inch copper sheet is preferably used as the substrate of the coating film, and the coating is preferably carried out by spin coating, and the thickness of the cured film on the copper sheet is controlled to be 10 to 20 μm.
[0135] Subsequently, the substrate coated with the photosensitive resin composition is subjected to heat treatment to obtain a photosensitive resin cured film. Specifically, the method comprises the following steps:
[0136] The photosensitive resin composition is coated on a 4-inch substrate by a coating machine, and then soft-baked at 120°C for 3 minutes using a heating table, and then the prepared resin cured film is placed in a vacuum oxygen-free oven to maintain nitrogen circulation for heat treatment. Specifically, after ensuring that the oxygen content in the oven cavity is reduced to below 50ppm, the temperature is first raised to 170°C and kept constant for 30 minutes, and then the temperature is raised to 350°C after 1 hour, and treated at 350°C for 1 hour to obtain a photosensitive resin cured film.
[0137] According to another aspect of the present application, a semiconductor device is provided, comprising a cured relief pattern formed from the above-mentioned photosensitive resin composition.
[0138] According to another aspect of the present application, a method for preparing the semiconductor device is provided, comprising at least the following steps:
[0139] The photosensitive resin composition is coated on the surface of a substrate, exposed, developed, and heat-treated to obtain the semiconductor device.
[0140] Specifically, the steps include:
[0141] (1) coating a photosensitive resin composition on a substrate to form a photosensitive resin layer on the substrate;
[0142] (2) exposing the photosensitive resin layer;
[0143] (3) developing the exposed photosensitive resin layer to form a relief pattern;
[0144] (4) The relief pattern is subjected to a heat treatment to form a solidified relief pattern, thereby obtaining the semiconductor device.
[0145] Wherein, the substrate includes silicon, copper, copper alloy, titanium, titanium alloy, and aluminum.
[0146] Wherein, step (1) is the same as the above-mentioned method for preparing the resin cured film.
[0147] The exposure treatment in step (2) is to expose the above-mentioned resin cured film to ultraviolet rays, X-rays, electron beams, etc. through a photomask or mask with a pattern or directly to a mask having a desired pattern on the above-mentioned resin film. Common active light rays include ultraviolet rays, X-rays, electron beams, etc. In the present invention, a mercury lamp is preferably used, which includes i-line (365nm), h-line (405nm), and g-line (436nm).
[0148] In order to improve the sensitivity, etc., a post-exposure bake and / or a pre-development bake based on any combination of temperature and time may be performed as required. The baking conditions are a temperature of 40 to 120° C. and a time of 10 to 240 seconds, and are not limited to this range as long as the properties of the photosensitive resin composition of the present invention are not affected.
[0149] After exposure, a pattern is formed by removing the unexposed portion using a developer. Common developers include: N-methyl-2-pyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, methanol, ethanol, isopropanol, ethyl lactate, butyl acetate, propylene glycol monomethyl ether acetate, cyclopentanone, cyclohexanone, isobutyl ketone, tetramethylammonium hydroxide aqueous solution, etc. After development, it is preferably rinsed with deionized water, ethanol, isopropanol, ethyl lactate, propylene glycol monomethyl ether acetate, etc. For example, a developer and a rinse solution are poured into two glass culture dishes respectively. The developer temperature is controlled to be 25±1°C, the exposed resin film is immersed in the developer, and the timing is started immediately. After the unexposed part is completely exposed to the substrate, the development is completed, the timing is stopped, and the time required for the whole process is recorded.
[0150] Finally, the resin pattern obtained after development is thermally imidized at 200-500°C to convert it into a cured film. This heat treatment usually selects staged temperature increase and maintains a certain time at different temperatures or selects a certain temperature range for continuous temperature increase. For example, a heat treatment method is performed at 180°C, 240°C, and 350°C for 30 minutes respectively, or a method of linearly increasing the temperature from 25°C to 400°C over 2 hours.
[0151] The cured relief pattern can be used as a surface protection film, an interlayer insulating film, an insulating film for redistribution, a protective film for a flip chip device, or a protective film for a semiconductor device having a bump structure.
[0152] The present invention introduces a nitrogen-containing heterocyclic polysiloxane into a photosensitive resin composition having a specific resin structure, and a photosensitive resin cured film prepared by the photosensitive resin composition can exhibit excellent dielectric properties and a low thermal expansion coefficient. The cured film formed by the photosensitive resin composition can be used for particle shielding, surface protection or insulation of semiconductor elements, insulating layers of OLED elements, etc., and can also be used to form cured relief patterns such as passivation films, surface protection films and interlayer insulating films of semiconductor devices, and can also be used for interlayer insulation of multilayer circuits, cover coating solder resist films of flexible copper-clad boards, and liquid crystal orientation films, etc., and has broad application prospects in semiconductor-related fields. BRIEF DESCRIPTION OF THE DRAWINGS
[0153] Figure 1 The infrared spectra of nitrogen-containing heterocyclic polysiloxanes PS-11, PS-15, PS-14, and PS-18. DETAILED DESCRIPTION
[0154] The technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0155] Several specific synthesis examples and embodiments are given below to illustrate the present invention, which will help those skilled in the art to more fully understand the present invention, but the present invention is not limited to these examples. It should be noted that the evaluation of the products prepared in the following synthesis examples and embodiments is carried out according to the following method.
[0156] (1) Infrared spectrum test
[0157] The synthesized polysiloxane sample was tested using an infrared spectrometer (Shimadzu, IRAffinity-1S) by a KBr pellet method to detect whether the polysiloxane of the present invention was successfully prepared.
[0158] (2) Molecular weight test
[0159] The weight average molecular weight (Mw) of the resin was determined by gel permeation chromatography (standard polystyrene conversion). The gel permeation chromatograph used in the determination was LC-20AD of Shimadzu Corporation of Japan, the chromatographic column was KF-804 of Showa Denko, the detector was differential RID-20A of Shimadzu Corporation of Japan, and the mobile phase was N-methylpyrrolidone (NMP).
[0160] (3) Viscosity test
[0161] 0.5 mL of the photosensitive resin composition sample was taken and placed in the sample cell of a rotational viscometer (BROOKFIELD DV2T RV), and a viscosity test was performed with a suitable measuring range and the temperature controlled at 25±0.1°C.
[0162] (4) Thermal expansion coefficient
[0163] With reference to the national standard GB / T 36800.2-2018 Plastics Thermomechanical Analysis (TMA) Part 2: Determination of Linear Thermal Expansion Coefficient and Glass Transition Temperature, the thermal expansion coefficient was tested using the thermomechanical analyzer TMA 450 (USA) TA.
[0164] (5) Dielectric constant
[0165] Referring to the national standard GB / T 31838.6-2021 dielectric and resistance properties of solid insulating materials, the dielectric constant was measured at 25°C using a DMS2000 high and low temperature dielectric resistance thermometer, and the value at a frequency of 1 MHz was recorded.
[0166] The abbreviations of ingredients used in this application are as follows:
[0167] MIBK: Methyl isobutyl ketone
[0168] NMP: N-methylpyrrolidone
[0169] GBL: gamma-butyrolactone
[0170] ODPA: 4,4-oxydiphthalic anhydride
[0171]
[0172] BPDA: 3,3',4,4'-biphenyltetracarboxylic dianhydride
[0173] ODA: 4,4'-diaminodiphenyl ether
[0174] m-TD: 2,2'-dimethyl-4,4'-diaminobiphenyl
[0175] CpODA:
[0176]
[0177] BZDA:
[0178]
[0179] SiDA: 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane silane coupling agent SCA:
[0180] SCA-1:
[0181]
[0182] SCA-2:
[0183]
[0184] SCA-3:
[0185]
[0186] SCA-4:
[0187]
[0188] SCA-5:
[0189]
[0190] SCA-6:
[0191]
[0192] SCA-7:
[0193]
[0194] SCA-8:
[0195]
[0196] SCA-9:
[0197]
[0198] SCA-10:
[0199]
[0200] SCA-11:
[0201]
[0202] SCA-12:
[0203]
[0204] SCA-13:
[0205]
[0206] SCA-14:
[0207]
[0208] SCA-15:
[0209]
[0210] SCA-16:
[0211]
[0212] Among them, the silane coupling agent monomer SCA-1 is prepared according to the method of Example 1 in Patent ZL202111145299.6, SCA-3 is prepared according to the method of Example 2 in Patent ZL202111145299.6, SCA-4 is prepared according to the method of Example 3 in Patent ZL202111145299.6, and SCA-5 is prepared according to the method of Example 4 in Patent ZL202111145299.6.
[0213] Preparation method of SCA-2: In a 500mL three-necked flask equipped with a stirrer and a thermometer, add 250.00g of solvent N-methylpyrrolidone and 0.1mol of 3,5-diamino-1,2,4-triazole in sequence, start stirring, and after 3,5-diamino-1,2,4-triazole is fully dissolved, slowly add 0.2mol of silane coupling agent 3-(trimethoxysilyl)propyl succinic anhydride, and after the addition is completed, continue to react at 25°C for 20 hours, then add 0.4mol of N,N-dimethylformamide dimethyl acetal to the system, continue to react at 25°C for 4 hours, and after the reaction is completed, distill under reduced pressure to obtain SCA-2.
[0214] Preparation method of SCA-6:
[0215] Into a 500 mL three-necked flask equipped with a stirrer and a thermometer, 250.00 g of solvent N-methylpyrrolidone and 0.1 mol of 2-(4-aminophenyl)-5-aminobenzimidazole were added in sequence, and stirring was started. After 2-(4-aminophenyl)-5-aminobenzimidazole was fully dissolved, 0.2 mol of silane coupling agent 3-(trimethoxysilyl)propyl succinic anhydride was slowly added. After the addition was completed, the reaction was continued at 25° C. for 20 hours. After the reaction was completed, the mixture was purified by vacuum distillation to obtain SCA-6.
[0216] Preparation method of SCA-7:
[0217] To a 500 mL three-necked flask equipped with a stirrer and a thermometer, 250.00 g of solvent N-methylpyrrolidone and 0.1 mol of 2-(4-aminophenyl)-5-aminobenzimidazole were added in sequence, and stirring was started. After 0.1 mol of 2-(4-aminophenyl)-5-aminobenzimidazole was fully dissolved, 0.2 mol of silane coupling agent 3-(trimethoxysilyl)propyl succinic anhydride was slowly added. After the addition was completed, the reaction was continued at 25° C. for 20 hours, and then 0.4 mol of pyridine was added to the reaction system. After stirring evenly, 0.4 mol of acetic anhydride was slowly added, and the reaction was carried out at 25° C. for 20 hours. After the reaction was completed, the solvent, acetic anhydride, and the generated acetic acid and pyridine in the system were removed by reduced pressure distillation to obtain SCA-7.
[0218] Preparation method of SCA-8: The same as SCA-6 except that 0.2 mol of 3-(trimethoxysilyl)propyl succinic anhydride was replaced by 0.2 mol of silane coupling agent SANAH (Shin-Etsu Chemical Co., Ltd.).
[0219] Preparation method of SCA-9: except replacing 0.2 mol of 3-(trimethoxysilyl)propyl succinic anhydride with 0.2 mol of silane coupling agent SANAH, the rest is the same as SCA-7.
[0220] The preparation method of SCA-10 is the same as that of SCA-6 except that 0.1 mol of 2-(4-aminophenyl)-5-aminobenzimidazole is replaced by 0.1 mol of 2-(4-aminophenyl)-5-aminobenzoxazole.
[0221] Preparation method of SCA-11: except that 0.1 mol of 2-(4-aminophenyl)-5-aminobenzimidazole is replaced by 0.1 mol of 2-(4-aminophenyl)-5-aminobenzoxazole, the rest is the same as SCA-7.
[0222] Preparation method of SCA-12: except that 0.1 mol of 2-(4-aminophenyl)-5-aminobenzimidazole is replaced by 0.1 mol of 2-(4-aminophenyl)-5-aminobenzoxazole, the rest is the same as SCA-8.
[0223] Preparation method of SCA-13: except replacing 0.1 mol of 2-(4-aminophenyl)-5-aminobenzimidazole with 0.1 mol of 2-(4-aminophenyl)-5-aminobenzoxazole, the rest is the same as SCA-9.
[0224] Preparation method of SCA-14: To a 500mL three-necked flask equipped with a stirrer and a thermometer, add 250.00g of solvent N-methylpyrrolidone and 0.1mol of 2-(4-aminophenyl)-5-aminobenzoxazole in sequence, start stirring, and after 2-(4-aminophenyl)-5-aminobenzoxazole is fully dissolved, slowly add 0.2mol of silane coupling agent SANAH, and after the addition is completed, continue to react at 25°C for 20 hours, then add 0.4mol of N,N-dimethylformamide diethyl acetal to the system, continue to react at 25°C for 4 hours, and after the reaction is completed, distill under reduced pressure to obtain SCA-14.
[0225] Preparation method of SCA-15: To a 500mL three-necked flask equipped with a stirrer and a thermometer, add 250.00g of solvent N-methylpyrrolidone and 0.1mol of 4,4'-diaminodiphenyl ether in sequence, start stirring, and after 4,4'-diaminodiphenyl ether is fully dissolved, slowly add 0.2mol of silane coupling agent 3-(trimethoxysilyl)propyl succinic anhydride, and after the addition is completed, continue to react at 25°C for 20 hours. After the reaction is completed, distill under reduced pressure to obtain SCA-15.
[0226] Preparation method of SCA-16: Add 250.00 g of solvent N-methylpyrrolidone and 0.1 mol of 4,4'-diaminobenzanilide in sequence to a 500 mL three-necked flask equipped with a stirrer and a thermometer, start stirring, and after 4,4'-diaminobenzanilide is fully dissolved, slowly add 0.2 mol of silane coupling agent 3-(trimethoxysilyl)propyl succinic anhydride, and continue to react at 25° C. for 20 hours after the addition is completed. After the reaction is completed, distill under reduced pressure to obtain SCA-16.
[0227] The silane coupling agent was characterized by hydrogen nuclear magnetic resonance spectroscopy. Some hydrogen spectrum information is as follows:
[0228]
[0229] Synthesis example 1
[0230] Under nitrogen protection, 100 g of methyl isobutyl ketone (MIBK), 30 g of nitrogen-containing heterocyclic silane coupling agent monomer SCA-1, and 1.5 g of p-toluenesulfonic acid were added to a 250 ml three-necked flask, and the mixture was stirred and mixed evenly, and the system temperature was maintained at 10° C. (reaction temperature 1) to obtain a mixed solution; 150 g of deionized water was dropped into the mixed solution within 4 hours. After the addition was completed, the mixture was kept at 10° C. for 4 hours, and then the temperature was raised to 70° C. (reaction temperature 2) and the reaction was continued for 10 hours; after the reaction was completed, the organic layer was taken out, and the volatiles were evaporated off using a rotary evaporator to obtain nitrogen-containing heterocyclic polysiloxane PS-1.
[0231] Synthesis example 2-20
[0232] The nitrogen-containing heterocyclic polysiloxanes PS-2 to PS-20 were prepared by referring to the method of Synthesis Example 1. The reaction conditions used were selected according to Table 1 below.
[0233] Table 1
[0234]
[0235] Characterization of nitrogen-containing heterocyclic polysiloxanes: The synthesized polysiloxanes were characterized by infrared spectroscopy. From the infrared characterization results, it can be seen that each polysiloxane has a -1 The Si-O-Si stretching vibration peak appears, indicating that the alkoxy group has been successfully converted into a Si-O-Si structure by hydrolysis. Among them, the infrared spectra of PS-11, PS-15, PS-14, and PS-18 are as follows: Figure 1 shown.
[0236] Synthesis Example 21
[0237] Polysiloxane PS-21 was prepared according to the method of Synthesis Example 1, except that 30 g of nitrogen-containing heterocyclic silane coupling agent monomer SCA-1 was replaced with 30 g of silane coupling agent monomer SCA-15.
[0238] Synthesis example 22
[0239] Polysiloxane PS-22 was prepared according to the method of Synthesis Example 1, except that 30 g of nitrogen-containing heterocyclic silane coupling agent monomer SCA-1 was replaced with 30 g of silane coupling agent monomer SCA-16.
[0240] Synthesis example 23
[0241] Synthesis of polyimide precursor C-1:
[0242] The whole reaction was carried out under nitrogen protection.
[0243] ① Place 31.02 g (0.1 mol) of 4,4'-oxydiphthalic anhydride (ODPA) in a 500 mL three-necked flask, add 26.03 g (0.2 mol) of hydroxyethyl methacrylate (HEMA) and 100.00 g of γ-butyrolactone (GBL), and dropwise add (0.2 mol) of 15.82 g of pyridine at a temperature below 10°C while stirring to obtain reaction mixture I. After naturally rising to 25°C, stir for 12 hours.
[0244] ② Next, 41.25 g (0.2 mol) of dicyclohexylcarbodiimide (DCC) was dissolved in 50.00 g of GBL solution to form a DCC mixed solution. The DCC mixed solution was added dropwise to the reaction mixture I with stirring using a feeding pump over an ice bath for 40 min. The temperature was raised to 10°C and the reaction was kept warm for 30 min to obtain a reaction mixture II.
[0245] ③ Add 18.05g (0.085mol) of 2,2'-dimethyl-4,4'-diaminobiphenyl (m-TD) and 3.84g (0.01mol) of CpODA to 70.00g of GBL solution and stir to dissolve to obtain a diamine solution. Use a feed pump to gradually drop the diamine solution into the reaction mixture II at 10°C for 60min. After the addition is completed, naturally rise to 25°C, add 80.00g of GBL, continue stirring for 12hr, then add 6.00g of ethanol and stir for 1hr, filter to remove the precipitate produced in the reaction mixture, and obtain reaction solution III.
[0246] ④ The obtained reaction solution III was added to 1L of ethanol to precipitate the polymer, and then 300mL of tetrahydrofuran was used to dissolve the precipitated polymer, and the obtained polymer solution was dropped into 5L of ultrapure water to precipitate the polymer, and the obtained precipitate was filtered out and vacuum dried at 50°C for 72 hours to obtain a polymer powder, i.e., a polyimide precursor C-1. The molecular weight of the polymer powder was measured by gel permeation chromatography (standard polystyrene conversion), and the weight average molecular weight (Mw) was 18,000 to 22,000.
[0247] Synthesis Examples 24-29, Synthesis Example 32
[0248] The polyimide precursors C-2 to C-7 and C-10 were synthesized by referring to the synthesis method of Synthesis Example 23, except that the dianhydride and diamine used were as shown in Table 2.
[0249] Synthesis example 30
[0250] Synthesis of polyimide C-8:
[0251] 31.02 g (0.1 mol) of 4,4'-oxydiphthalic dianhydride (ODPA) was placed in a 500 mL three-necked flask, and 100.00 g of NMP was added. At room temperature, 70.00 g of NMP solution containing 18.05 g (0.085 mol) of 4,4'-bis-(4-nitrophenoxy)biphenyl (m-TD) and 3.84 g (0.01 mol) of CpODA was added over 60 min. The mixture was reacted at 30°C for 4 h. Then, 22.46 g (0.22 mol) of acetic anhydride and 17.40 g (0.22 mol) of pyridine were added, and the mixture was reacted at 30°C for 2 h.
[0252] The obtained reaction solution was added into 5L of deionized water to precipitate a polymer precipitate. The obtained precipitate was filtered out, washed three times with deionized water, and vacuum dried at 50°C for 72 hours to obtain a polymer powder, i.e., polyimide C-8. The molecular weight of the polymer powder was measured by gel permeation chromatography (standard polystyrene conversion), and the weight average molecular weight (Mw) was 18,000 to 22,000.
[0253] Synthesis Examples 31, 33
[0254] Polyimide C-9 and C-11 were synthesized by referring to the synthesis method of Synthesis Example 30, except that the dianhydride and diamine used were as shown in Table 2.
[0255] Table 2
[0256]
[0257] Examples and Comparative Examples
[0258] In a three-necked flask equipped with a stirrer, 25.00 g of the synthesized polyimide precursor or polyimide was dissolved in 50.00 g of N-methylpyrrolidone (NMP). After the polymer was completely dissolved, polysiloxane was added according to Table 3, and then 0.25 g of SCA-2 and 0.25 g of KH560 (Nanjing Dimonte) were added. Stirring was continued until completely dissolved, and then 1.00 g of photoinitiator 1-(4-phenylthio-phenyl)-octane-1,2-diketo-2-oxime-0-benzoate (OXE-1, BASF), 4.00 g of thermal crosslinking agent triethylene glycol dimethacrylate (TEGDMA), and 0.25 g of thermal polymerization inhibitor p-hydroxyanisole (MEHQ) were added in sequence. After fully dissolved, the photosensitive resin composition was obtained by filter pressing using a 1.0 μm filter membrane, and the viscosity was measured at 25° C. to be 2500-3000 cP.
[0259] Table 3
[0260]
[0261]
[0262]
[0263] The photosensitive resin composition prepared above was evaluated according to the dielectric constant and thermal expansion coefficient test methods described above. The results are shown in Table 4.
[0264] Table 4
[0265]
[0266]
[0267] From the above table we can see that:
[0268] From the comparison of Example 1, Examples 4-22, Example 31, Comparative Example 1, Comparative Example 2, and Comparative Examples 5-8, it can be seen that the photosensitive resin composition obtained in the examples of the present application has a lower dielectric constant and thermal expansion coefficient, among which the photosensitive resin composition with the addition of PS-11 to PS-20 has better performance than the photosensitive resin composition with the addition of PS-1 to PS-10.
[0269] From the comparison between Example 13, Examples 23-30, and Comparative Examples 3-4, it can be seen that the dielectric constant and thermal expansion coefficient of the photosensitive resin composition are further reduced by optimizing the structure of the precursor resin of the present invention.
[0270] The above are only a few embodiments of the present application and do not constitute any form of limitation to the present application. Although the present application is disclosed as above with preferred embodiments, it is not intended to limit the present application. Any technician familiar with the profession, without departing from the scope of the technical solution of the present application, using the technical content disclosed above to make slight changes or modifications are equivalent to equivalent implementation cases and fall within the scope of the technical solution.
Claims
1. A photosensitive resin composition, characterized in that It includes precursor resin, nitrogen-containing heterocyclic polysiloxane, silane coupling agent, photosensitive auxiliary agent, crosslinking agent and solvent; The precursor resin comprises at least one of a polymer having a structural unit represented by formula (1) and a polymer having a structural unit represented by formula (2); Wherein, i1 is selected from an integer between 2 and 200, and i2 is selected from an integer between 2 and 50; X1 is selected from a tetravalent organic group having 4 to 40 carbon atoms; X2 is selected from alicyclic tetravalent organic groups having 4 to 40 carbon atoms; Y1 and Y2 are each independently selected from a divalent organic group having 2 to 40 carbon atoms; R7 and R8 are each independently selected from a saturated aliphatic group having 1 to 4 carbon atoms, an organic group having a structure represented by the following formula (6), or a hydrogen atom; In formula (6), R9, R 10 , R 11 Each is independently selected from an organic group having 1 to 3 carbon atoms or a hydrogen atom; m is selected from an integer between 2 and 10; The nitrogen-containing heterocyclic polysiloxane is selected from at least one of the polymers represented by the following formula (7): In formula (7), Y is an organic group containing a nitrogen heterocyclic ring.
2. The photosensitive resin composition according to claim 1, characterized in that In formula (1) and formula (2), X1 is selected from at least one of the structures shown in the following formula (3), and * represents an insertion site: X2 is selected from at least one of the structures shown in the following formula (4), and * represents an insertion site: Y1 and Y2 are each independently selected from at least one of the structures represented by the following formula (5): R7 and R8 are each independently selected from methyl, ethyl, methacrylate hydroxyethyl, and n-butyl.
3. The photosensitive resin composition according to claim 1 or 2, characterized in that: In formula (1) and formula (2), the quantitative ratio of i1 to i2 is 100:2-20, preferably, the quantitative ratio of i1 to i2 is 100:5-15; preferably, among all the structural units of the precursor resin, more than 50 mol% of the structure is a structural unit represented by formula (1) or formula (2); preferably, the precursor resin is selected from a precursor of a polyimide resin, a polyimide resin, or has a precursor of a polyimide resin or a polyimide resin as the main component.
4. The photosensitive resin composition according to claim 1, characterized in that In formula (7), Y is selected from at least one of the structures shown in formula (8) to formula (11), and * represents an insertion site: Wherein, R1 is selected from a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, or an alkoxy group having 1 to 20 carbon atoms; Wherein, W is at least one of the structures ①, ②, and ③ in the following formula (12), and * represents an accession site: Here, R2, R3, R4, R5, and R6 each independently represent a hydrogen atom or a hydrocarbon group having 1 to 10 carbon atoms.
5. The photosensitive resin composition according to claim 4, characterized in that: R1 is selected from hydrogen atom, methyl group, ethyl group, butyl group, hydroxyethyl group of methacrylate; R2, R3, R4, R5, R6 are each independently selected from hydrogen atom, methyl group, ethyl group.
6. The photosensitive resin composition according to claim 1, characterized in that: The silane coupling agent includes at least one of a nitrogen-containing heterocyclic silane coupling agent, a urea-based silane coupling agent, a mercapto-based silane coupling agent, a vinyl-based silane coupling agent, and an epoxy-based silane coupling agent; The photosensitizer comprises at least one of a photo-radical polymerization initiator, a diazoquinone compound, an onium salt and a halogen-containing compound; The crosslinking agent includes at least one of tetraethylene glycol dimethacrylate, diethylene glycol diacrylate, triethylene glycol diacrylate, diethylene glycol dimethacrylate, triethylene glycol dimethacrylate, tetraethylene glycol dimethacrylate, trimethylolpropane diacrylate, trimethylolpropane triacrylate, trimethylolpropane dimethacrylate, DMOM-PTBP-MF, TMOM-BP, HMOM-TPHAP, DML-PC, DMOM-MBPC, HMOM-TPHAP and MX-100LM; The solvent is selected from at least one of N-methylpyrrolidone, methyl ethyl ketone, acetone, γ-butyrolactone, ethyl acetate, ethyl lactate, toluene, xylene, diethylene glycol monobutyl ether, propylene glycol methyl ether, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, tetrahydrofuran, dioxane, N,N-dimethylformamide, N,N-dimethylacetamide, and dimethyl sulfoxide.
7. The photosensitive resin composition according to claim 1, characterized in that: The mass ratio of the precursor resin to the nitrogen-containing heterocyclic polysiloxane is 100:0.01-20; The mass ratio of the precursor resin to the silane coupling agent is 100:0.1-5; The mass ratio of the precursor resin to the photosensitive auxiliary agent is 100:0.1-30; The mass ratio of the precursor resin to the cross-linking agent is 100:0.5-30; The mass ratio of the resin to the solvent is 100:80-5000.
8. The photosensitive resin composition according to claim 1, characterized in that: Also included are polymerization inhibitors; Preferably, the polymerization inhibitor comprises at least one of hydroquinone, p-hydroxyanisole, N-nitrosodiphenylamine, phenothiazine, p-tert-butylcatechol, N-phenylnaphthylamine, ethylenediaminetetraacetic acid, 1,2-cyclohexanediaminetetraacetic acid, 2,6-di-tert-butyl-p-methylphenol, 5-nitroso-8-hydroxyquinoline, and N-nitroso-N (1-naphthyl) hydroxylamine ammonium salt; Preferably, the mass ratio of the precursor resin to the polymerization inhibitor is 100:0.01-15; Preferably, the viscosity of the photosensitive resin composition is 10 to 10000 cP.
9. A photosensitive resin cured film, characterized in that: The method is obtained by curing the photosensitive resin composition according to any one of claims 1 to 8.
10. A semiconductor device, characterized in that: A cured relief pattern formed from the photosensitive resin composition according to any one of claims 1 to 8 is contained.
Citation Information
Patent Citations
A class of silane coupling agents with urea and imide structures, their preparation methods and applications
CN111825884B
Triazolyl silane coupling agent as well as preparation method and application thereof
CN114456205A
Photosensitive resin composition, cured film, electronic component, antenna element, semiconductor package, and compound
CN116802559A
Polybenzoxazole photosensitive resin composition as well as preparation method and application thereof
CN116880123A
Photosensitive resin composition, dry film, and processed component using the same
JP2004361883A