Preparation method of high-temperature alloy with both infrared radiation performance and body performance
By constructing a database of the corresponding relationship between high-temperature oxidation parameters and performance, and optimizing the high-temperature oxidation process, the problem of high-temperature alloys taking into account infrared radiation and body performance is solved, performance improvement and process simplification are achieved, and costs are reduced.
Patent Information
- Application Number
- CN202410971278.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-08
AI Technical Summary
In the high-temperature oxidation treatment, existing high-temperature alloys are difficult to take into account both infrared radiation and body properties, and the preparation process is complex and costly, which makes it difficult to meet performance requirements.
Design high-temperature oxidation orthogonal tests to construct a database of high-temperature oxidation parameters, infrared radiation performance, body performance correspondence and regularity. Select appropriate high-temperature oxidation parameters through the database, and use high-temperature oxidation technology to generate an oxide film on the surface of the high-temperature alloy matrix to form an infrared High-temperature alloy parts with radiation and body properties.
It realizes the improvement of infrared radiation performance and body performance of high-temperature alloy parts, simplifies the process flow, reduces costs, ensures controllability of performance and meets performance requirements.
Smart Images

Figure CN118917076A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of thermal surface treatment of high-temperature alloys, and in particular relates to a method for preparing a high-temperature alloy that takes both infrared radiation performance and bulk performance into consideration. Background Art
[0002] High-temperature alloy is a metal alloy. It has become the preferred material for aerospace due to its stable structure, excellent thermal strength, hot and cold processing and welding performance. It plays a very important role in the development of modern aviation industry. At present, aircraft are constantly developing towards the goal of high Mach number and long flight time. When the aircraft encounters serious aerodynamic heating problems during high-speed reentry, in order to ensure the safety of personnel and the normal operation of equipment, it is necessary to lay lightweight, high-temperature resistant anti-insulation materials with different temperature resistance levels on the surface of the aircraft to meet the anti-insulation requirements of different parts of the aircraft. The reusable thermal protection system consists of a surface high infrared radiation performance coating and an internal low thermal conductivity insulation material. The internal low thermal conductivity insulation material can prevent heat from being transferred to the interior of the aircraft, while the surface high infrared radiation performance coating can dissipate heat to the external environment through radiation. Aircraft parts made of high-temperature alloys are often used in relatively high ambient temperatures. Therefore, the infrared radiation performance of their surface has a crucial influence on the high-temperature service of high-temperature alloy parts.
[0003] At present, composite coatings with high infrared radiation performance made of metal oxides or minerals are widely used as new heat-resistant materials on metal alloy surfaces to improve infrared radiation performance. The complex preparation process, high price and complicated spraying process of high infrared radiation performance coatings have become the shortcomings that restrict their widespread application. Summary of the invention
[0004] In view of the above analysis, the present invention is based on the fact that the oxide film generated on the surface of the high-temperature alloy by a high-temperature oxidation process can improve the infrared radiation performance, and provides a method for preparing a high-temperature alloy that takes into account both infrared radiation performance and bulk performance. It is used to solve the problems in the prior art that the high-temperature oxidation parameters are uncontrollable, the high-temperature alloy prepared is difficult to take into account both infrared radiation performance and bulk performance, the alloy products fail to meet the performance requirements, and the preparation process is difficult.
[0005] On the one hand, the present invention provides a method for preparing a high-temperature alloy that takes into account both infrared radiation performance and bulk performance, comprising the following steps:
[0006] S1. Design high-temperature oxidation orthogonal test, build the database of correspondence and regularity between high-temperature oxidation parameters, infrared radiation performance and bulk performance, and select the corresponding high-temperature oxidation parameters according to the bulk performance and infrared radiation performance requirements of high-temperature alloy parts based on the database;
[0007] S2. A high-temperature oxidation process is used to generate an oxide or mineralized oxide film on the surface of a high-temperature alloy substrate to obtain a high-temperature alloy part having both infrared radiation performance and bulk performance, wherein the parameters of the high-temperature oxidation process are determined from the database obtained in S1 according to the bulk performance and infrared radiation performance requirements of the high-temperature alloy part.
[0008] Furthermore, the preparation method of the high temperature alloy substrate includes:
[0009] S21, Additive Manufacturing: Perform additive manufacturing to prepare high-temperature alloy matrix parts;
[0010] S22, stress relief annealing: vacuum stress relief annealing heat treatment is used to eliminate the residual stress generated by the high-temperature alloy matrix parts during the additive manufacturing process;
[0011] S23, wire cutting: separate the substrate from the high-temperature alloy matrix parts;
[0012] S24, solution heat treatment: vacuum solution heat treatment of high temperature alloy base parts;
[0013] S25, machining: machining high temperature alloy base parts into welded parts of certain size according to product requirements;
[0014] S26. Welding: Weld the welded parts together to form an assembly.
[0015] Furthermore, in S1, the high-temperature oxidation parameters include heating temperature and holding time; the infrared radiation performance includes infrared emissivity, oxide layer thickness, oxide layer morphology, oxidation phase analysis, and weight gain after oxidation; the bulk properties include bulk mechanical properties, weld mechanical properties, and weld quality; the bulk mechanical properties include tensile strength, yield strength, elongation after fracture, and hardness.
[0016] Furthermore, the high temperature alloy substrate is GH4099 or GH3128 alloy.
[0017] Furthermore, the GH4099 alloy was subjected to high temperature oxidation treatment in an air environment, with a heating temperature of 850°C and a holding time of 8h.
[0018] Furthermore, the GH3128 alloy was subjected to high temperature oxidation treatment in an air environment, with a heating temperature of 900°C and a holding time of 20 h.
[0019] Further, the S1 includes:
[0020] S11. Design a high-temperature oxidation orthogonal test, design and process performance characterization parts, use the performance characterization parts to complete the high-temperature oxidation experiment and perform performance tests;
[0021] S12, sorting out the performance results, obtaining the corresponding relationship between high temperature oxidation parameters, infrared radiation performance, and bulk performance, and completing the construction of a regularity database;
[0022] S13, using intermediate parameters or repeated experiments to calibrate and compensate the database;
[0023] S14. Use the database to combine the high-temperature alloy product's intrinsic properties and infrared radiation performance requirements to select high-temperature oxidation parameters.
[0024] On the other hand, the present invention also proposes a high-temperature alloy that takes into account both infrared radiation performance and bulk performance, which is prepared by the above method.
[0025] Furthermore, the high-temperature alloy meets the requirements of infrared radiation performance and bulk performance at the same time; the oxide film is formed by the high-temperature alloy itself and is a metal mineralize or oxide; the infrared radiation performance of the GH3128 alloy: infrared emissivity ≥0.75, bulk performance: room temperature tensile strength ≥800MPa, elongation ≥25%, 900℃ tensile strength ≥210MPa, elongation ≥50%; the infrared radiation performance of the GH4099 alloy: infrared emissivity ≥0.75, bulk performance: room temperature tensile strength ≥1000MPa, elongation ≥10%, 900℃ tensile strength ≥380MPa, elongation ≥10%.
[0026] Furthermore, the oxide film has a thickness of 5 μm to 50 μm.
[0027] Compared with the prior art, the present invention can achieve at least one of the following beneficial effects:
[0028] 1) The present invention provides a method for preparing a high-temperature alloy that takes into account both infrared radiation performance and bulk performance. After the high-temperature alloy is subjected to high-temperature oxidation processing in a certain high-temperature oxygen-containing environment, the oxide film composed of the oxide on its surface is itself an excellent interface for improving its own infrared radiation performance. However, the study found that after a certain high-temperature oxidation, there must be a difference between the bulk performance and the infrared radiation performance of the high-temperature alloy compared to before oxidation. If the alloy meets the bulk performance requirements before high-temperature oxidation, a high-temperature oxidation experiment is carried out to improve the infrared radiation performance. Although the infrared radiation performance of the alloy is improved after the experiment, its bulk performance has also changed after high-temperature oxidation. At this time, the alloy cannot meet the bulk performance requirements, which is undesirable. The present invention constructs a database of correspondence and rules between high-temperature oxidation parameters, bulk performance and infrared radiation performance. The database can select high-temperature oxidation parameters that can simultaneously meet the two performances, and use the parameters for high-temperature oxidation treatment to prepare alloy products that can meet both infrared radiation performance and bulk performance requirements.
[0029] 2) Rely on its own high-temperature oxide film to improve the emissivity. The oxide film is formed by itself, eliminating the need for spraying process and expensive spraying materials. The preparation process is simple, the price is low and the parameters are controllable. It can reduce or replace the use of existing high-emissivity coatings on the surface of high-temperature alloys and reduce the processing cost of parts. For existing high-emissivity coatings on the surface of high-temperature alloys, the coating materials need to match the chemical composition, crystal structure and thermal expansion coefficient of the substrate alloy to reduce the stress at the interface and avoid stratification. The operation process is complicated and the cost is high; the high-temperature oxide film itself avoids the above defects and has good alloy bonding strength. When the emissivity requirements of the parts are not very high, the high-temperature oxide film itself can replace the high-emissivity coating. At this time, the high-temperature oxide film can be made in one piece during the heat treatment process of the high-temperature alloy itself, simplifying the process and reducing the processing cost of the parts; when the parts have high emissivity requirements, the high-temperature oxide film itself can partially replace the high-emissivity coating, thereby reducing the thickness of the high-emissivity coating and reducing the cost of the high-emissivity coating.
[0030] 3) The present invention provides a new idea for the performance evaluation of high-temperature alloys. The existing performance evaluation of high-temperature alloys, such as infrared surface emissivity testing, is expensive, the testing process is complicated, and there are many types of performance evaluation, such as bulk mechanical properties, weld mechanical properties, weld quality, oxide layer thickness, etc. At present, the requirements for the performance of high-temperature alloys in applications are mostly within a range, such as room temperature hardness HV ≥ 400, room temperature bulk mechanical properties: tensile strength ≥ 1000MPa, yield strength ≥ 700MPa, elongation after fracture ≥ 10%, etc., and the performance requirements are not precise. The present invention constructs a database of the correspondence and regularity of high-temperature oxidation parameters, bulk properties and infrared radiation properties. After that, for parts prepared under the same process conditions, their performance can be predicted with reference to the database, for example, based on fixed high-temperature oxidation parameters, the bulk and infrared radiation performance of the parts are estimated; based on the infrared radiation performance test results, the bulk performance of the parts is estimated; based on the bulk performance test results, the infrared radiation performance of the parts is estimated. The database is used to achieve accurate and low-cost prediction and detection of infrared radiation performance under specific high-temperature oxidation process parameters.
[0031] 4) It provides a new idea for performance regulation. After oxidation at a certain high temperature regime, the high-temperature alloy's own performance and surface infrared radiation performance are bound to be different from those before oxidation. Therefore, how to achieve regulation between the two properties is the key to the application of high-temperature alloy oxide films. The present invention utilizes a set of infrared radiation properties to achieve regulation between the bulk performance and the infrared radiation performance, providing a possibility for the preparation of high-temperature alloys that take into account both infrared radiation performance and bulk performance, and for the use of the high-temperature alloy's own oxide film to improve its own emissivity.
[0032] Other features and advantages of the present invention will be described in the following description, and part of them will become obvious from the description, or will be understood by practicing the present invention. The purpose and other advantages of the present invention can be realized and obtained through the written description. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] The drawings are only for the purpose of illustrating particular embodiments and are not to be construed as limiting the invention.
[0034] Figure 1 It is a schematic diagram of the process of regulating the properties of high-temperature alloys based on high-temperature oxidation;
[0035] Figure 2 This is a schematic diagram of the infrared radiation performance characterization of GH4099 high-temperature alloy parts;
[0036] Figure 3 This is a schematic diagram of the performance representation of the GH4099 high-temperature alloy part.
[0037] Figure 4 It is a schematic diagram of GH3128 high temperature alloy shaft parts and specific surfaces;
[0038] Figure 5 The actual pictures of the high temperature alloy of the present invention before (left) and after (right) high temperature oxidation;
[0039] Figure 6 A high-temperature alloy (left) and a representative part (right) that failed to be prepared according to the method of the present invention;
[0040] Figure 7 This is a SEM image of the high-temperature alloy prepared by the present invention;
[0041] Figure 8 This is a SEM image of the longitudinal section of the high-temperature alloy prepared by the present invention;
[0042] Fig. 9 This is the XRD diagram of the high-temperature alloy prepared in the present invention.
[0043] Reference numerals
[0044] 1-Infrared emissivity test piece; 2-Oxide layer thickness test piece; 3-Welding test piece; 4-Mechanical tensile test bar; 5-Hardness characterization test block; 6-Specific surface. DETAILED DESCRIPTION
[0045] The preferred embodiments of the present invention are described in detail below. The embodiments are only used to illustrate the principles of the present invention and are not used to limit the scope of the present invention.
[0046] The present invention intends to use a high-temperature oxidation process to generate an oxide film on the surface of a high-temperature alloy to prepare a metal oxide coating with high infrared radiation performance. After the high-temperature alloy is subjected to high-temperature oxidation under certain high-temperature oxidation parameters, a layer of oxide film is formed on the surface of the high-temperature alloy. The oxide film formed by itself is equivalent to a metal oxide coating, which is an excellent interface with high infrared radiation performance. The oxide film of this method is formed by itself, eliminating the spraying process and the need for expensive spraying materials. The preparation process is simple and the price is low. However, because the high-temperature oxidation parameters are uncontrollable, the prepared high-temperature alloy is likely to fail to meet the performance requirements, and the preparation process is difficult. There is an urgent need to find a controllable method for high-temperature oxidation parameters.
[0047] The properties of high-temperature alloys include bulk properties and infrared radiation properties. Bulk properties are generally determined by chemical composition and microstructure. When the bulk properties are changed, the infrared radiation properties will also change. Similarly, when the infrared radiation properties are changed, the bulk properties of the alloy may be adversely affected, such as reducing its tensile strength and elongation. High-temperature oxidation requires precise control of temperature, time and oxygen environment, and it is also necessary to regulate bulk properties and infrared radiation properties, which is difficult in actual operation.
[0048] In view of the above analysis, the present invention provides a method for preparing a high-temperature alloy that takes into account both infrared radiation performance and bulk performance, so as to solve the problem that the high-temperature oxidation parameters of the existing high-temperature alloys based on high-temperature oxidation are uncontrollable during preparation, the prepared high-temperature alloy may not be able to take into account both properties, the alloy product cannot meet the performance requirements, and the preparation process is difficult.
[0049] On the one hand, the present invention proposes a method for preparing a high-temperature alloy that takes into account both infrared radiation performance and bulk performance. The main process and process principle are as follows: Figure 1 As shown, it mainly includes the following steps:
[0050] S1. Design high-temperature oxidation orthogonal test, build the database of correspondence and regularity between high-temperature oxidation parameters, infrared radiation performance and bulk performance, and select the corresponding high-temperature oxidation parameters according to the bulk performance and infrared radiation performance requirements of high-temperature alloy parts based on the database;
[0051] S2. A high-temperature oxidation process is used to generate an oxide or mineralized oxide film on the surface of a high-temperature alloy substrate to obtain a high-temperature alloy part having both infrared radiation performance and bulk performance, wherein the parameters of the high-temperature oxidation process are determined from the database obtained in S1 according to the bulk performance and infrared radiation performance requirements of the high-temperature alloy part.
[0052] Specifically, S1 includes:
[0053] S11. Design a high-temperature oxidation orthogonal test, design and process performance characterization parts, use the performance characterization parts to complete the high-temperature oxidation experiment and perform performance tests;
[0054] When designing the orthogonal test of high-temperature oxidation, only the performance characterization parts are designed. According to the technical conditions of the parts and the performance of concern, the performance characterization parts are designed and processed, and the high-temperature oxidation orthogonal test is completed using the performance characterization parts. Select the high-temperature oxidation parameters: any one of the heating temperature and the holding time is a variable and the other is quantitative to conduct the high-temperature oxidation test. For example, select the heating temperature as a quantitative value (750℃), the holding time as a variable (2h, 4h, 6h, 8h, 10h, 12h), and conduct a high-temperature oxidation test to obtain the infrared radiation and bulk performance results at different holding times at 750℃. Or select the holding time as a quantitative value (2h), the heating temperature as a variable (700℃, 750℃, 800℃, 850℃, 900℃), conduct a high-temperature oxidation test, characterize the results of the performance characterization parts, and obtain the infrared radiation and bulk performance results of holding for 2h at different heating temperatures.
[0055] S12. Arrange the performance results, obtain the corresponding relationship between high temperature oxidation parameters, infrared radiation performance, and bulk performance, and complete the construction of a regularity database, wherein the database is composed of test result data points.
[0056] S13, using intermediate parameters or repeated experiments to calibrate and compensate the database;
[0057] Repeat the experiment to correct the abnormal result data points that may exist, and use the intermediate parameters in the database to compensate the performance results. Use intermediate parameters or repeated experiments to check and compensate the database, and continuously improve the database and improve its accuracy. For example, according to the results in the regular database, the performance obtained under 850℃8h insulation can meet the performance requirements of the parts, while the performance obtained under 850℃6h insulation cannot meet the performance requirements of the parts. In order to explore the best process window, the database was corrected at 850℃7h. The specific performance results are shown in Table 5. Table 5 is the test results of infrared emissivity performance, bulk mechanical properties (yield strength, tensile strength, elongation after fracture, hardness), and weld mechanical properties obtained from the test with a heating temperature of 850℃ and a holding time of 7h. In addition, in this step, the abnormal points in the database can also be tested repeatedly.
[0058] S14. Use the database to combine the intrinsic properties of high-temperature alloy products with the infrared radiation performance requirements, and select high-temperature oxidation parameters in the database that can take into account both the intrinsic properties and infrared radiation performance, in preparation for the subsequent S2 high-temperature oxidation process.
[0059] In one possible way, in order to ensure the mechanical properties when constructing the database, the GH4099 performance characterization parts were subjected to orthogonal tests with heating temperatures of 700℃, 750℃, 800℃, 850℃, and 900℃, and holding times of 2h, 4h, 6h, 8h, 10h, and 12h, and the infrared emissivity performance, oxide layer thickness, bulk mechanical properties (tensile strength, yield strength, elongation), hardness, weld mechanical properties (tensile strength, yield strength, elongation) and other performance results were obtained. Some results are shown in Tables 3 and 4. Table 3 shows the orthogonal test results with heating temperature of 750℃ and holding time of 2h, 4h, 6h, 8h, 10h, and 12h; Table 4 shows the orthogonal test results with heating temperature of 850℃ and holding time of 2h, 4h, 6h, 8h, 10h, and 12h. By using the obtained database of correspondence and rules between high-temperature oxidation parameters, infrared radiation performance, and bulk performance, the corresponding high-temperature oxidation parameters in the set are selected according to the design requirements of different GH4099 parts and infrared radiation performance, and the parameters can be used to solidify the high-temperature alloy preparation process.
[0060] It should be noted that infrared radiation and bulk performance testing usually require the use of performance characterization parts. Therefore, when designing a high-temperature oxidation orthogonal test, only the performance characterization parts are designed and processed, and the high-temperature oxidation orthogonal test is completed using the performance characterization parts. The main function of these characterization parts is to provide a benchmark or reference for testing and analysis to ensure the accuracy and reliability of the measurement results. When performing performance testing, these characterization parts can simulate the material behavior in actual applications under controlled laboratory conditions, thereby more accurately evaluating the performance of the material, predicting its performance in actual use, and ensuring the quality and reliability of the product.
[0061] Specifically, in order to ensure the consistency and comparability of the database results, the shape of the performance characterization part needs to be designed, because different test types and test methods have different requirements for the shape of the performance characterization part, and the shape design of the performance characterization part is not universal. The shape of the specific performance characterization part is designed according to the test requirements of the database results.
[0062] When conducting infrared emissivity tests, the shape of the characterizing piece is a disc, and the diameter of the disc is manufactured according to the requirements of the infrared testing instrument, generally ranging from 10mm to 50mm. The disc shape helps ensure the consistency and comparability of the test results. It is also highly symmetrical, with small directional errors, and the surface can provide uniform infrared radiation and reception, helping to reduce the impact of local hot spots or cold spots on the test results. The diameter is easy to measure and standardize, which helps to accurately control the test parameters and improve the accuracy, repeatability and comparability of infrared emissivity tests. For example, Figure 2 The shape of the mid-infrared emissivity test piece.
[0063] When testing the oxide layer thickness and oxide layer morphology, both can be tested using SEM to characterize the shape of the part. Figure 2 The shape of the medium oxide thickness test piece is a square test piece. The side length is made according to the standard sample and processing allowance, generally about 10mm, and the thickness is 1 to 3mm. The square test piece meets many standards and specifications for oxide thickness testing, which helps to ensure the consistency and comparability of test results. The surface is relatively uniform, which helps to obtain more consistent results in oxide thickness testing. The processing processes such as cutting and grinding are simple and easy to implement. The size of the test piece is easy to measure and can be precisely controlled to ensure the accuracy of the test results. It helps to improve the accuracy, repeatability and comparability of oxide thickness testing. It is a standard shape widely used in oxide thickness evaluation.
[0064] When conducting oxidation phase analysis, XRD phase analysis can be used, and the shape of the characterization part can be as follows Figure 2 The shape of the mid-infrared emissivity test piece is a disc, or it can be Figure 2 The shape of the medium oxide layer thickness test piece is a square test piece.
[0065] When conducting the post-oxidation weight gain test, an analytical balance is used to measure the post-oxidation weight gain, and the shape of the characterization part is as follows: Figure 2 The shape of the mid-infrared emissivity test piece is a disk.
[0066] When testing the weld quality, use SEM to observe the weld after welding and oxidation to see if there are cracks. If there are no cracks, it means the quality is qualified. Figure 3 Welding of representative parts of the welding test piece shape ( Figure 3 The welding test piece is a rectangular test piece, and the side length is made according to the standard sample and processing allowance, generally 100×200mm; the rectangular test piece conforms to a variety of welding standards and specifications, such as AWS and ISO, which helps to ensure the consistency and comparability of test results; it can more accurately represent the actual shape and size of the weld, because the weld is usually long in the actual welding process; it is relatively easy to cut out from the welded part, especially when destructive testing is required; the shape of the rectangular test piece helps to improve the accuracy, repeatability and comparability of welding joint quality testing, and is a standard shape widely used in welding quality assessment). Figure 3 The representative parts in the shape of the welding test piece are welded to form a square weld quality test piece generally with a size of 200×200 mm, and then the weld of the weld quality test piece is observed by SEM.
[0067] When conducting weld mechanical properties test, in order to evaluate the mechanical properties of the weld joint, a portion of the 200×200mm square weld quality test specimen can be cut to form a long strip including the weld as a representative piece for the weld mechanical properties test.
[0068] When testing the mechanical properties of the body, the shape of the representative part is cylindrical, and the specific size is made according to the standard sample and processing allowance, which is generally During the test, the bulk mechanical properties such as tensile strength, yield strength, and elongation after fracture can be obtained at the same time. The cylindrical shape has been adopted by multiple international standards. Since stress concentration usually occurs at sharp corners or irregular shapes of the specimen, the stress distribution of the cylindrical geometry is relatively uniform, which can reduce stress concentration and help to more accurately evaluate the mechanical properties of the material; during the stretching process, the cylinder is easier to be fixed by the clamp, the diameter and length are easy to measure, and the deformation of the specimen is easier to predict and control, which helps to accurately control the size of the specimen, thereby ensuring the accuracy of the test results. For example, the characterization parts of the bulk mechanical properties test are such as Figure 3 The shape of the medium mechanical tensile test bar.
[0069] When conducting a hardness characterization block test, the characterization piece is in the shape of a cube, and the side length is made according to the standard specimen and processing allowance, generally 5mm to 20mm. The cube shape meets the standards of most hardness tests, such as Rockwell hardness and Brinell hardness tests, which helps to ensure the consistency and comparability of test results. The cube shape helps to reduce stress concentration, and its six faces are flat, which can reduce measurement errors caused by irregular shapes and help stabilize the specimen during the test. In addition, this shape is easy to process, and it is also easy to position and align the test instrument during the test, which can reduce operational errors. For example, the characterization piece of the hardness characterization block test is such as Figure 3 Medium hardness characterizes the shape of the test piece.
[0070] Furthermore, in S11, the types of performance characterization parts, such as test bars for body mechanical properties (yield strength, tensile strength, elongation after fracture), test blocks for body mechanical properties (hardness), and discs for infrared emissivity performance characterization, should be as complete as possible so as to pass a high-temperature oxidation process test once and test more performance results to improve the applicability of building a database.
[0071] In a possible implementation, in order to establish a database, an additively manufactured GH4099 furnace test bar is used to characterize the mechanical tensile properties of parts at room temperature and 900°C; an additively manufactured GH4099 furnace test block is used to characterize the room temperature hardness; additively manufactured GH4099 furnace test pieces of different sizes are used to characterize the room temperature hardness; infrared emissivity test pieces and oxide layer thickness test pieces of corresponding sizes and shapes are used to characterize the infrared radiation performance of high-temperature alloys; the number of the above characterization parts can be determined according to design requirements, and the design schematic diagrams of different performance characterization parts are shown in the figure. Figure 2 , Figure 3 shown.
[0072] Furthermore, in S2, the method for preparing the high temperature alloy substrate comprises:
[0073] S21, Additive Manufacturing: Perform additive manufacturing to prepare high-temperature alloy matrix parts;
[0074] S22, stress relief annealing: vacuum stress relief annealing heat treatment is used to eliminate the residual stress generated by the high-temperature alloy matrix parts during the additive manufacturing process;
[0075] S23, wire cutting: separate the substrate from the high-temperature alloy matrix parts;
[0076] S24, solution heat treatment: vacuum solution heat treatment of high temperature alloy base parts;
[0077] S25, machining: machining high temperature alloy base parts into welded parts of certain size according to product requirements;
[0078] S26. Welding: Weld the welded parts together to form an assembly.
[0079] Furthermore, after the high-temperature alloy is prepared, in combination with the database, the body and infrared radiation performance of the high-temperature alloy parts prepared under the fixed high-temperature oxidation parameters can be estimated in advance. If the product needs to be characterized, a performance characterization part is required to detect its body and infrared radiation performance. At this time, the performance characterization part is obtained after performing steps S21 to S26 together with the part. The body performance of the part can also be estimated based on the infrared radiation performance test results. For example, in order to solve the problem that the infrared radiation performance test of the surface of the high-temperature alloy after high-temperature oxidation is expensive and difficult to evaluate, the weight gain before and after oxidation is used as a means of evaluating infrared radiation performance. The test only needs to use an analytical balance to test the weight gain of the infrared emissivity test piece after high-temperature oxidation to obtain the result, making the test simpler and more convenient. Or estimate the infrared radiation performance of the part based on the body performance test results.
[0080] Specifically, additive manufacturing in S21 refers to the additive manufacturing of parts, using the same materials as high-temperature alloy products for additive manufacturing, and the integral parts that require high-temperature oxidation are welded assemblies made of high-temperature alloy additive manufacturing. When the final high-temperature alloy product requires performance testing, it also includes additive manufacturing of furnace performance characterization parts. At this time, the raw materials for performance characterization parts and parts additive manufacturing must be consistent.
[0081] In one possible implementation, GH4099 powder is used to perform additive manufacturing on the parts and their performance characterization parts. The forming method is laser selective additive manufacturing, the laser power is 275W, the spot size is 0.07mm, the scanning speed is 960mm / s, the oxygen content in the forming chamber is 0-0.02%, the argon pressure is 4-10bar, the powder thickness is 0.04mm, the powder speed is 20-100mm / s, the wind speed is 20-60%, and the powder feeding ratio is 30-100%.
[0082] Specifically, in S22, the parts after additive manufacturing are subjected to vacuum stress relief annealing to eliminate the residual stress in the laser additive manufacturing process. The stress relief annealing parameters of the present invention are heating at 5°C / min, heating to 600-650°C, keeping the temperature for 4 hours, and then cooling to room temperature in the furnace.
[0083] Specifically, after the substrate and the parts are separated by wire cutting in S23, the parts after wire cutting may be degreased.
[0084] Specifically, the purpose of the solution heat treatment in S24 is to improve the microstructure and macroscopic properties of the material, improve the performance of the additively manufactured parts, and make them meet the application requirements of the product. The solution treatment can refer to the solution heat treatment system of the specific material. For example, the solution heat treatment system of GH4099 material is a heating temperature of 1150°C, a holding time of 1.5-2h, and 2Bar-4Bar argon gas cooling.
[0085] Specifically, machining in S25 refers to machining allowance. Factors such as material deposition and heat effects during additive manufacturing lead to insufficient dimensional accuracy of parts and high surface roughness of additive manufacturing. Machining can improve surface quality, reduce surface defects, and ensure that parts meet design requirements. In addition, after high-temperature oxidation treatment, performance characterization parts will also be processed for subsequent performance testing, which generally refers to mechanical processing, such as processing test rods into a certain test size, cutting welding test pieces into the size required for testing, etc.
[0086] Specifically, welding in S26: If parts need to be welded, weld the parts according to the welding process parameters of the parts, and weld the welded parts together to form an assembly. For example, GH4099 alloy uses vacuum electron beam welding, with a welding speed of 1mm / min, an acceleration voltage of 120KV, and an electron beam current of 32 / mA. If high-temperature oxidation aging is placed before welding, the parts also need to be polished, sandblasted, or cleaned with a solution before welding to make the surface easy to weld.
[0087] Specifically, in S2, the high temperature oxidation process can be performed after welding or before welding, and can be set according to product requirements. If the entire surface of the product requires an oxide film, the high temperature oxidation process can be placed after welding; if part of the surface of the product requires an oxide film, the high temperature oxidation process can be placed before welding.
[0088] Furthermore, when the product quality requirements are high, aging heat treatment is also required, the purpose of which is to improve the performance of the alloy, stabilize the microstructure and geometric dimensions. The high-temperature oxidation process can be combined with the aging heat treatment. During the aging heat treatment, the alloy is exposed to the air. Due to the high temperature, the alloy surface reacts with oxygen to form oxides, completing the high-temperature oxidation and simplifying the process.
[0089] In one possible implementation, the aging heat treatment system of the GH4099 high-temperature alloy is used to perform high-temperature oxidation treatment on the parts and all performance-characteristic parts in an air environment, with a heating temperature of 850°C and a holding time of 8 hours, and the aging heat treatment is performed by extending the holding time. The aging heat treatment system of the GH3128 high-temperature alloy is used to perform high-temperature oxidation treatment on the parts and all performance-characteristic parts in an air environment, with a heating temperature of 900°C and a holding time of 20 hours.
[0090] Specifically, the alloy needs to be surface treated before the high temperature oxidation process, and the surface treatment includes: grinding and polishing, sandblasting, cleaning and wiping, and tooling treatment.
[0091] Grinding and polishing is rough grinding with a grinding wheel or a grinding head to remove surface unevenness and roughness to make the surface smoother. Mechanical polishing equipment or manual operation is used to grind and polish parts and other performance characterization parts, especially infrared radiation performance characterization parts. The main purpose is to remove the surface oxide layer, rust and other pollutants of parts and performance characterization parts to ensure that the metal surface is brighter and increase its appearance texture. After grinding and polishing, quality inspection is carried out. The surface of the parts must be smooth, without bumps and other pollution. There should be no obvious uneven grinding and polishing on the surface of the parts and infrared performance characterization parts, and the overall surface should be consistent.
[0092] Sandblasting is to spray dry, oil-free, and non-large-particle quartz sand onto the metal surface of parts and other performance-characterizing parts through compressed air to remove surface stains and impurities, and at the same time increase the roughness of the metal surface for subsequent high-temperature treatment. The diameter of the quartz sand and the air pressure of the sandblasting machine can be reasonably selected according to the material and thickness of the parts. The workpiece after sandblasting should evenly and completely reveal the original color of the metal. The parts after sandblasting are strictly prohibited from being touched with bare hands. If sweat stains appear, uneven color is likely to appear on the surface of the oxide layer. The diameter of the quartz sand of the present invention is 2 mm, the air pressure is 0.3-0.4 MPa, and the spray angle is 60°.
[0093] Cleaning and wiping is to use a dust-free cloth dipped in anhydrous ethanol solution or acetone solution to clean the surface of the parts after sandblasting. Ensure that the surfaces of the cleaned parts and other performance-characterizing parts are prohibited from being touched with bare hands.
[0094] Tooling treatment: If the parts need tooling during the high-temperature oxidation process, and the surface of the parts in contact with the tooling needs to form a dense and uniform oxide film, the contact position between the tooling and the parts needs to be cleaned. The tooling cleaning method can be sandblasting after grinding.
[0095] Furthermore, the high temperature oxidation parameters include heating temperature and holding time; the heating temperature and holding time can be set according to design requirements and processing requirements. The oxygen environment mainly includes a conventional air environment and an oxygen-rich environment. Generally, to obtain the same oxide layer thickness and infrared radiation performance, the processing time of the high temperature alloy in a conventional air environment is longer than that in an oxygen-rich environment. Therefore, the oxygen environment can also be reasonably selected according to the setting of the holding time.
[0096] In a possible implementation, the high-temperature oxidation parameters selected by S1 are: temperature 850°C and holding time 8h. Before loading the furnace, the surface of the parts and tooling should be clean and dry. After loading the furnace, an air heating furnace with substitute fan circulation is used for high-temperature oxidation treatment. The high-temperature oxidation treatment temperature is 850°C and the time is controlled at 8h. Finally, the parts or performance characterization parts after being taken out of the furnace are inspected for appearance to confirm whether the color of the surface oxide film is uniform and consistent.
[0097] The infrared radiation performance includes infrared emissivity, oxide layer thickness, oxide layer morphology, oxidation phase analysis, and weight gain after oxidation. The high-temperature oxidation process will affect the infrared radiation performance of the alloy. In order to obtain the infrared radiation performance under high-temperature oxidation parameters, an infrared radiation performance test is required. The infrared emissivity test can test the ability of the material to emit infrared radiation under thermal radiation conditions, which helps to evaluate the heat dissipation, corrosion resistance and wear resistance of the material; the oxide layer thickness test is to determine whether the protective layer on the surface of the material meets the requirements to judge the corrosion resistance and wear resistance of the material; the oxide layer morphology observation is to observe the surface morphology of the oxide layer to evaluate its quality and performance; the oxide layer phase analysis is to determine the phase composition of the oxide layer to understand its stability and reactivity under different conditions; the weight gain test before and after oxidation is to evaluate the protection ability of the coating or material to the substrate at high temperature by the change in mass of the sample before and after oxidation.
[0098] Furthermore, infrared radiation performance testing is closely related to performance characterization parts. Objects of different shapes and sizes may have different infrared radiation energy distribution and intensity emitted from their surfaces. Infrared testing has high requirements for the test environment. If the shape and size of the performance characterization part are significantly different from the actual product, the test results cannot truly reflect the performance of the product. Therefore, choosing the right performance characterization part is an important prerequisite for ensuring the accuracy of the test results.
[0099] The bulk properties include bulk mechanical properties, weld mechanical properties, and weld quality; the bulk mechanical properties include tensile strength, yield strength, elongation after fracture, and hardness. The high-temperature oxidation process will affect the bulk properties of the alloy. In order to obtain the bulk properties under high-temperature oxidation parameters, bulk performance testing is required.
[0100] Bulk mechanical property testing can determine the basic mechanical properties of materials, such as tensile strength, yield strength, elastic modulus, hardness, etc.; it can evaluate the response of materials under different load conditions, ensure that the materials can withstand the expected stress and strain in actual applications, and provide data support for material selection and design.
[0101] Weld mechanical property evaluation can evaluate the mechanical properties of welded joints, including their response under tension, compression, bending and impact loads; ensure that the mechanical properties of welds meet the design requirements and avoid structural failure due to welding quality problems; detect defects that may occur during welding, such as cracks, pores, lack of fusion, etc., and guide the improvement of welding technology through test results.
[0102] The quality of weld joints can evaluate the macro and micro structures of welds, including the shape, size and internal organization of welds, and check whether welds have defects such as cracks, inclusions, holes, etc., which may affect the load-bearing capacity and durability of welds.
[0103] Furthermore, the main performance test is closely related to the performance characterization part. The shape and size of the performance characterization part directly affect the stress distribution and deformation mode during the test, which is crucial to the accuracy, representativeness and reliability of the test results. The performance characterization part with the appropriate shape and size can be selected according to the specific test requirements.
[0104] On the other hand, the present invention also proposes a high-temperature alloy that takes into account both infrared radiation performance and bulk performance, which is prepared by the above method. The alloy meets the requirements of infrared radiation performance and bulk performance at the same time; the high-temperature alloy substrate is GH4099 or GH3128 alloy, and its surface has a dense oxide film.
[0105] like Figure 5The following are the actual pictures of the high-temperature alloy of the present invention before (left) and after (right) high-temperature oxidation. It can be seen from the picture that the color of the alloy changes after high-temperature oxidation. The color distribution of the alloy surface in the right picture is uniform, indicating that there is an additional oxide film with uniform material distribution on the surface. Figure 7 As shown in FIG. 1 , it is a SEM image of the high temperature alloy prepared by the present invention. As can be seen from the image, the thickness of the oxide film is evenly distributed on the entire surface, there is no obvious thickness difference, and no major defect changes occur, indicating that the prepared high temperature alloy is very successful.
[0106] The oxide film is formed by the high-temperature alloy itself and is a metal mineralization or oxide. For example, the oxide film formed by oxidizing the GH4099 high-temperature alloy is mainly made of Cr2Ni3, Cr2O3, and CoCr2O4. Fig. 9 As shown, it is the XRD diagram of the high-temperature alloy prepared by the present invention. After phase retrieval analysis and comparison of the phase and the powder standard diffraction file of the corresponding phase, the main phase of the surface phase composition of GH4099 is Cr2Ni3 (65-6291) type face-centered cubic phase; a small amount of phase is Cr2O3: (38-1479) with a trigonal structure and CoCr2O4 (78-0711) with a face-centered cubic structure.
[0107] The thickness of the oxide film is 5 μm to 50 μm. Figure 8 , which is a SEM image of a longitudinal section of a high-temperature alloy prepared in the present invention, from which it can be seen that the thickness of the oxide layer on the surface of the high-temperature alloy is 15.3 μm.
[0108] The infrared radiation performance of the high-temperature alloy is: infrared emissivity ≥ 0.75, and the bulk performance is: room temperature tensile strength ≥ 800MPa, elongation ≥ 10%, 900°C tensile strength ≥ 210MPa, elongation ≥ 10%.
[0109] The following is a further explanation of a method for preparing a high-temperature alloy having both infrared radiation performance and bulk performance according to the present invention through specific examples.
[0110] Example 1
[0111] A preparation method of GH4099 high-temperature alloy taking both infrared radiation performance and bulk performance into consideration.
[0112] GH4099 high temperature alloy is one of the most widely used high temperature alloy materials in aerospace applications. It is a highly alloyed nickel-based aging alloy. The Cr, Co, W, and Mo elements added to the alloy are solid solution strengthened, Al and Ti elements are added to form aging strengthened phases, and the added B, Ce, and Mg elements play a role in strengthening grain boundaries. The alloy can be used for a long time at temperatures below 900°C, and the short-term maximum operating temperature can reach 1000°C. The main heat treatment methods for GH4099 high temperature alloy are solid solution treatment and aging treatment, which can be carried out in a vacuum environment and air atmosphere.
[0113] In this embodiment, the integral part that needs high temperature oxidation is a welded assembly manufactured by additive manufacturing of GH4099 high temperature alloy. The performance of the overall part that needs to be paid attention to is mainly divided into two parts: bulk performance and infrared radiation performance. The bulk performance and requirements include: room temperature hardness (HV ≥ 400), room temperature weld mechanical properties, room temperature and 900 ° C high temperature mechanical tensile properties of parts (yield strength, tensile strength, elongation), and the specific design requirements are shown in Table 1.
[0114] Table 1 GH4099 alloy body properties and requirements
[0115]
[0116] The surface radiation performance includes: infrared emissivity after high temperature oxidation (room temperature ≥ 0.75, 1000℃ ≥ 0.8) and oxide layer thickness ≥ 15μm. According to the technical solution provided by the present invention, the specific steps in this embodiment are as follows:
[0117] (1) Design high-temperature oxidation orthogonal experiments to obtain high-temperature oxidation parameters, infrared radiation performance, and bulk performance, and complete the construction of a regularity database;
[0118] Design high-temperature oxidation orthogonal test, design and process performance characterization parts, use performance characterization parts to complete high-temperature oxidation experiment and conduct corresponding performance tests.
[0119] In this implementation, the material state of the parts before high-temperature oxidation is in a solid solution state. According to the properties of the material and general rules, it is difficult to meet the precipitation of the strengthening phase in the GH4099 material at a lower temperature, which does not achieve the purpose of strengthening the material. At the same time, it is also very difficult to produce an oxide film on the surface of the material at a lower temperature. The solid solution temperature of GH4099 is around 1100°C, and the temperature of high-temperature oxidation should be lower than the solid solution temperature. Therefore, in order to meet the mechanical properties of the parts, the high-temperature oxidation temperature parameter of the orthogonal test can be set at 750°C-950°C.
[0120] For the GH4099 parts in this embodiment, in order to ensure the mechanical properties, orthogonal tests were carried out with heating temperatures of 700°C, 750°C, 800°C, 850°C, and 900°C and holding times of 2h, 4h, 6h, 8h, 10h, and 12h, and the performance results of bulk mechanical properties test, weld joint quality, weld joint performance, oxide layer thickness, infrared emissivity, weight gain before and after oxidation, oxide layer morphology and phase analysis were obtained. The designed orthogonal test is shown in Table 2.
[0121] Table 2 High temperature oxidation orthogonal test
[0122]
[0123] In this embodiment, because the parts are formed by additive manufacturing, the GH4099 furnace test bars manufactured by additive manufacturing are used to characterize the mechanical tensile properties of the parts at room temperature and 900°C high temperature; the GH4099 furnace test blocks manufactured by additive manufacturing are used to characterize the room temperature hardness; the GH4099 furnace test pieces of different sizes manufactured by additive manufacturing are used to characterize the room temperature hardness; infrared emissivity test pieces and oxide layer thickness test pieces of corresponding sizes and shapes manufactured by additive manufacturing are used to characterize the infrared radiation performance of high-temperature alloys; the test plates manufactured by additive manufacturing are welded by a specific welding method, and the strength of the welded joints is tested; the number of the above characterization parts can be determined according to design requirements. The design schematic diagram of different performance characterization parts is shown in the figure. Figure 2 , Figure 3 As shown, the test pieces, test rods and test blocks are just different in shape and all are performance characterization parts.
[0124] The performance results were sorted out to obtain the corresponding relationships among high-temperature oxidation parameters, infrared radiation performance, and bulk mechanical properties, and the construction of a regularity database was completed.
[0125] According to the overall test results, the corresponding relationship between high-temperature oxidation parameters, infrared radiation performance, and bulk mechanical properties is obtained and the construction of the regularity database is completed. For the convenience of explanation, only some results are shown in Tables 3 and 4. Table 3 shows the test results of emissivity performance, mechanical properties, hardness, and room temperature mechanical properties of welds obtained by orthogonal tests with heating temperature of 750℃ and holding time of 2h, 4h, 6h, 8h, 10h, and 12h. Table 4 shows the test results of emissivity performance, mechanical properties, hardness, and room temperature mechanical properties of welds obtained by orthogonal tests with heating temperature of 850℃ and holding time of 2h, 4h, 6h, 8h, 10h, and 12h.
[0126] Table 3 Orthogonal test results with heating temperature of 750℃ and holding time of 2h, 4h, 6h, 8h, 10h and 12h
[0127]
[0128]
[0129] Table 4 Orthogonal test results with heating temperature of 850℃ and holding time of 2h, 4h, 6h, 8h, 10h, and 12h
[0130]
[0131] According to the infrared radiation performance and bulk performance requirements of the alloy product, find out the high-temperature oxidation parameters that can meet the two performance indicators from the database;
[0132] By using the obtained set of experimental parameters and performance results, the corresponding high-temperature oxidation parameters in the set can be selected according to the design requirements of the body performance and infrared radiation performance of different GH4099 parts.
[0133] According to the infrared radiation performance requirements: infrared emissivity after high-temperature oxidation (room temperature ≥ 0.75), the data in Table 3 were screened, and it was found that the room temperature emissivity results in Table 3 did not meet the requirement of ≥ 0.75, so Table 3 was excluded; then the data in Table 4 were screened, and it was found that only the test group numbers 3-3, 4-3, 5-3, and 6-3 in Table 4 met the requirements, so 1-3 and 2-3 were excluded.
[0134] According to the infrared radiation performance requirements: infrared emissivity after high temperature oxidation (1000°C ≥ 0.8), data were screened in the test groups 3-3, 4-3, 5-3, and 6-3 in Table 4, and it was found that these test groups all met the requirements.
[0135] According to the infrared radiation performance requirements: oxide layer thickness ≥ 15μm, the data in the test group numbers 3-3, 4-3, 5-3, and 6-3 in Table 4 were screened and it was found that only the test group numbers 4-3, 5-3, and 6-3 met the requirements, so 3-3 was excluded.
[0136] In turn, according to the main performance requirements: room temperature hardness (HV ≥ 400), room temperature weld mechanical properties, room temperature and 900 ° C high temperature mechanical tensile properties (yield strength, tensile strength, elongation after fracture) specific design requirements, screening was carried out in test groups numbered 4-3, 5-3, and 6-3, and it was found that all met the requirements.
[0137] Test group numbers 4-3, 5-3, and 6-3 all meet the experimental requirements, that is, 850℃8h, 850℃10h, and 850℃12h all meet the requirements, and the most energy-saving 850℃8h is selected as the optimal condition, that is, the performance obtained under 850℃8h insulation can meet the part performance requirements.
[0138] Use intermediate parameters or repeated experiments to calibrate and compensate the database, continuously improve the database and enhance its accuracy.
[0139] In order to explore the best process window, although experiment 3-3 (850℃6h) was excluded before, it is not yet determined whether 850℃7h is better than 850℃8h, so the database was corrected using 850℃7h. The specific performance results are shown in Table 5, which is the test results of emissivity performance, mechanical properties, hardness, and mechanical properties of welds at room temperature obtained from the test with a heating temperature of 850℃ and a holding time of 7h. In addition, in this step, the abnormal points in the database can also be tested repeatedly.
[0140] Table 5 Test results of heating temperature of 850℃ and holding time of 7h
[0141]
[0142] According to the infrared radiation performance requirements: infrared emissivity after high-temperature oxidation (room temperature ≥ 0.75, 1000°C ≥ 0.8), oxide layer thickness ≥ 15 μm, the data in Table 5 were screened and it was found that Table 5 met the requirements.
[0143] According to the requirements of the main performance: room temperature hardness (HV ≥ 400), and the mechanical properties of the room temperature weld in Table 1, and the specific design requirements of the mechanical tensile properties at room temperature and 900 ° C (yield strength, tensile strength, elongation after fracture), the data in Table 5 were screened and it was found that the mechanical properties of the room temperature weld (yield strength / MPa) were required to be ≥ 650, while the value in Table 5 was 620, which did not meet the requirements. Therefore, the condition of 850 ° C 7h was excluded, and the condition of 850 ° C 8h was the optimal condition.
[0144] In summary, it is found from the database results and the compensation group experimental results that the process parameters of 850℃8h meet the design requirements of the parts.
[0145] (2) Additive manufacturing: Additive manufacturing is performed to produce parts;
[0146] (3) Stress relief annealing: vacuum stress relief annealing heat treatment is used to eliminate the residual stress generated by the parts during the additive manufacturing process;
[0147] (4) Wire cutting: After the part is processed, it needs to be separated from the additive manufacturing substrate. Wire cutting is used to separate the substrate from the part.
[0148] (5) Solution heat treatment: vacuum solution heat treatment of parts;
[0149] (6) Machining: Machining parts into welded parts of a certain size according to product requirements;
[0150] (7) Welding: Weld the welded parts together to form an assembly.
[0151] (8) High temperature oxidation aging: After surface treatment, furnace loading, high temperature oxidation treatment and appearance inspection, the high temperature alloy product is obtained.
[0152] Surface treatment of parts includes grinding and polishing, sandblasting, solution cleaning and wiping.
[0153] 1. Grinding and polishing: use a grinding wheel or a grinding head for rough grinding to remove surface unevenness and roughness to make the surface smoother. Use a polishing machine or manual fine polishing to ensure that the metal surface is brighter and increase its appearance texture;
[0154] 2. Sand blasting: using compressed air to spray quartz sand onto the metal surface to remove stains and impurities on the surface, while increasing the roughness of the metal surface for subsequent high-temperature treatment. After sand blasting, the surface color of parts and infrared radiation-related performance characterization parts should be uniform;
[0155] 3. Solution cleaning and wiping: Use a dust-free cloth dipped in alcohol solution to wipe the surface of the parts after sandblasting to ensure cleaning.
[0156] After the parts are loaded into the furnace, they are subjected to high-temperature oxidation treatment. The aging heat treatment system of GH4099 is used to carry out high-temperature oxidation treatment on the parts and all performance-characterizing parts in an air environment. The heating temperature is 850°C, the holding time is 8h, and the oxygen environment is a conventional air environment.
[0157] Conduct performance tests on alloy products. Use performance characterization parts to conduct corresponding performance tests on alloy products to obtain performance reference data.
[0158] like Figure 5 The actual pictures of the high-temperature alloy in this embodiment before (left) and after (right) high-temperature oxidation are shown. It can be seen from the figure that after high-temperature oxidation, the color of the alloy changes. The color distribution of the alloy surface in the right picture is uniform, indicating that the material distribution of the surface oxide film is uniform.
[0159] like Figure 7 As shown in FIG. 1 , it is a SEM image of the high temperature alloy prepared by the present invention. As can be seen from the image, the thickness of the oxide film is evenly distributed on the entire surface, there is no obvious thickness difference, and no major defect changes occur, indicating that the prepared high temperature alloy is very successful.
[0160] like Figure 8 , which is a SEM image of a longitudinal section of a high-temperature alloy prepared in the present invention, from which it can be seen that the thickness of the oxide layer on the surface of the high-temperature alloy is 15.3 μm.
[0161] like Fig. 9As shown, it is the XRD diagram of the high-temperature alloy prepared by the present invention. After phase retrieval analysis and comparison of the phase and the powder standard diffraction file of the corresponding phase, the main phase of the surface phase composition of GH4099 is Cr2Ni3 (65-6291) type face-centered cubic phase; a small amount of phase is Cr2O3: (38-1479) with a trigonal structure and CoCr2O4 (78-0711) with a face-centered cubic structure.
[0162] In summary, all the properties obtained when the heating temperature is 850°C, the holding time is 8h, and the oxygen environment is an ordinary air environment meet the design requirements of the parts in this embodiment, and the curing process is possible. In order to reduce the testing cost and ensure the product quality, in the subsequent production process, the thickness before and after oxidation is selected as a means of evaluating the infrared radiation performance of the parts. This test only requires the use of an analytical balance to test the weight gain of the infrared emissivity test piece after high-temperature oxidation to obtain the result.
[0163] Example 2
[0164] A preparation method of GH3128 high-temperature alloy taking both infrared radiation performance and bulk performance into consideration.
[0165] GH3128 is a high-performance nickel-based alloy with excellent plasticity, long-term creep strength, oxidation resistance, and good stamping and welding properties. Through solid solution strengthening of tungsten and molybdenum elements and grain boundary strengthening of boron and zirconium elements, the overall performance of GH3128 is in a leading position among similar nickel-based solid solution alloys. This alloy is particularly suitable for manufacturing high-temperature parts such as combustion chamber flame tubes, afterburner housings, and regulating plates. It can withstand high temperatures of 950°C and work for a long time, so it is widely used in the field of aircraft engines.
[0166] In this embodiment, the integral part that needs high-temperature oxidation is a GH3128 high-temperature alloy shaft-shaped part. There are requirements for the mechanical properties of the part body, and at the same time, the performance that needs to be paid attention to on a specific surface of the part is the infrared radiation performance. The body performance includes: the mechanical tensile properties of the part at room temperature and 900°C high temperature (tensile strength, elongation). The specific requirements are: after the part is oxidized at high temperature, the infrared emissivity should be ≥0.75, and the room temperature tensile strength of the part should be ≥800MPa, and the elongation should be ≥25%, the tensile strength at 900°C should be ≥210MPa, and the elongation should be ≥50%. The infrared radiation performance includes: infrared emissivity after high-temperature oxidation. The general shape of the part and the specific surfaces that need to pay attention to the infrared radiation performance are as follows Figure 4 As shown in , according to the technical solution provided by the present invention, the specific steps in this embodiment are as follows:
[0167] (1) Design high-temperature oxidation orthogonal experiments to obtain high-temperature oxidation parameters, infrared radiation performance, and bulk performance, and complete the construction of a regularity database;
[0168] According to the technical conditions and performance of the parts, the process design and process preparation of the parts and performance characterization parts are carried out. In this embodiment, the GH3128 furnace test rod is used to characterize the mechanical tensile properties of the parts at room temperature and 900℃ high temperature; infrared emissivity test pieces and oxide layer thickness test pieces of corresponding size and shape are used to characterize the infrared radiation performance of the high-temperature alloy; at the same time, before the parts are officially put into production and processing, the process method provided by the present invention is used to complete the relationship set between different holding times and the infrared emissivity of the GH3128 high-temperature alloy surface under 900℃ heating conditions. The brief list of the set is as follows:
[0169] Table 6 Relationship between holding time at 900℃ and infrared emissivity of GH3128 superalloy surface
[0170] Heating temperature / ℃ Insulation time / h Oxygen environment Surface infrared emissivity <![CDATA[Oxidation weight gain / mg·cm -2 > 900 10h Conventional air 0.55 0.25 900 20h Conventional air 0.75 0.31 900 30h Conventional air 0.79 0.34 900 40h Conventional air 0.81 0.39
[0171] Table 7 Relationship between holding time at 900℃ and bulk properties of GH3128 superalloy
[0172]
[0173] According to the infrared radiation performance and bulk performance requirements of the alloy product, find out the high-temperature oxidation parameters that can meet the two performance indicators from the database;
[0174] According to the infrared radiation performance requirements: infrared emissivity after high-temperature oxidation (room temperature ≥ 0.75), screening was performed in Table 6, and the conditions of infrared emissivity of 0.55 and 900°C for 10h were excluded.
[0175] According to the requirements of the main body performance: the room temperature tensile strength of the parts ≥ 800MPa, elongation ≥ 25%, the 900℃ tensile strength ≥ 210MPa, elongation ≥ 50%, the data in Table 7 are screened and found to meet the requirements, that is, the heating temperature of 900℃ and the insulation time of 20h to 40h meet the requirements. At this time, the most energy-saving 900℃20h is selected as the best condition, that is, the performance obtained under the insulation of 900℃20h can meet the performance requirements of the parts. At this time, combined with Table 6, it can be seen that the oxidation weight gain / mg·cm -2 Should be ≥ 0.31 mg cm -2 .
[0176] In summary, the process parameters of 900℃20h meet the design requirements of the parts.
[0177] (2) Additive manufacturing: Additive manufacturing is performed to produce parts;
[0178] (3) Stress relief annealing: vacuum stress relief annealing heat treatment is used to eliminate the residual stress generated by the parts during the additive manufacturing process;
[0179] (4) Wire cutting: After the part is processed, it needs to be separated from the additive manufacturing substrate. Wire cutting is used to separate the substrate from the part.
[0180] (5) Solution heat treatment: vacuum solution heat treatment of parts;
[0181] (6) Machining: Machining parts into welded parts of a certain size according to product requirements;
[0182] (7) Welding: Weld the welded parts together to form an assembly.
[0183] (8) High temperature oxidation aging: After surface treatment, furnace loading, high temperature oxidation treatment and appearance inspection, the high temperature alloy product is obtained.
[0184] Surface treatment of parts includes grinding and polishing, sandblasting, solution cleaning and wiping.
[0185] 1. Grinding and polishing: use a grinding wheel or a grinding head for rough grinding to remove surface unevenness and roughness to make the surface smoother. Use a polishing machine or manual fine polishing to ensure that the metal surface is brighter and increase its appearance texture;
[0186] 2. Sand blasting: using compressed air to spray quartz sand onto the metal surface to remove stains and impurities on the surface, while increasing the roughness of the metal surface for subsequent high-temperature treatment. After sand blasting, the surface color of parts and infrared radiation-related performance characterization parts should be uniform;
[0187] 3. Solution cleaning and wiping: Use a dust-free cloth dipped in alcohol solution to wipe the surface of the parts after sandblasting to ensure cleaning.
[0188] After the parts are loaded into the furnace, they are subjected to high-temperature oxidation treatment. The aging heat treatment system of GH3128 is used to carry out high-temperature oxidation treatment on the parts and all performance-characterizing parts in an air environment. The heating temperature is 900°C, the holding time is 20h, and the oxygen environment is a conventional air environment.
[0189] In this embodiment, only one surface of the shaft-shaped part needs to be subjected to high temperature oxidation treatment, so the high temperature oxidation surface needs to be processed in the preliminary machining process. After the oxidation treatment, other areas except the surface where the heat preservation oxide film needs to be retained need to be subjected to final machining treatment to remove the oxide layer in other areas of the high temperature alloy part.
[0190] Conduct performance tests on alloy products.
[0191] For the GH3128 part, the high temperature oxidation process is used to cure it. Since the infrared emissivity test cost is 1,500 yuan per time, in order to reduce the test cost and ensure product quality, in the subsequent production process, the weight gain before and after oxidation is used as a means of evaluating the infrared radiation performance of the part. That is, the weight gain of the infrared emissivity test piece after high temperature oxidation is tested using an analytical balance to calculate the oxidation weight gain, and according to the design requirements, the oxidation weight gain should be ≥0.31mg·cm -2 .
[0192] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by any technician familiar with the technical field within the technical scope disclosed by the present invention should be covered within the protection scope of the present invention.
Claims
1. A method for preparing a high-temperature alloy having both infrared radiation performance and bulk performance, characterized in that: The following steps are involved: S1. Design high-temperature oxidation orthogonal test, build the database of correspondence and regularity between high-temperature oxidation parameters, infrared radiation performance and bulk performance, and select the corresponding high-temperature oxidation parameters according to the bulk performance and infrared radiation performance requirements of high-temperature alloy parts based on the database; S2. A high-temperature oxidation process is used to generate an oxide or mineralized oxide film on the surface of a high-temperature alloy substrate to obtain a high-temperature alloy part having both infrared radiation performance and bulk performance, wherein the parameters of the high-temperature oxidation process are determined from the database obtained in S1 according to the bulk performance and infrared radiation performance requirements of the high-temperature alloy part.
2. The preparation method according to claim 1, characterized in that: In S2, the method for preparing the high temperature alloy substrate comprises: S21, Additive Manufacturing: Perform additive manufacturing to prepare high-temperature alloy matrix parts; S22, stress relief annealing: vacuum stress relief annealing heat treatment is used to eliminate the residual stress generated by the high-temperature alloy matrix parts during the additive manufacturing process; S23, wire cutting: separate the substrate from the high-temperature alloy matrix parts; S24, solution heat treatment: vacuum solution heat treatment of high temperature alloy base parts; S25, machining: machining high temperature alloy base parts into welded parts of certain size according to product requirements; S26. Welding: Weld the welded parts together to form an assembly.
3. The preparation method according to claim 1, characterized in that: In S1, The high temperature oxidation parameters include heating temperature and holding time; The infrared radiation performance includes infrared emissivity, oxide layer thickness, oxide layer morphology, oxidation phase analysis, and weight gain after oxidation; The body properties include body mechanical properties, weld mechanical properties, and weld quality; The mechanical properties of the main body include tensile strength, yield strength, elongation after fracture and hardness.
4. The preparation method according to claim 1 or 2, characterized in that: The high temperature alloy substrate is GH4099 or GH3128 alloy.
5. The preparation method according to claim 4, characterized in that: GH4099 alloy was subjected to high temperature oxidation treatment in air environment with heating temperature of 850℃ and holding time of 8h.
6. The preparation method according to claim 4, characterized in that: GH3128 alloy was subjected to high temperature oxidation treatment in air environment with heating temperature of 900℃ and holding time of 20h.
7. The preparation method according to any one of claims 1 to 6, characterized in that: The S1 includes: S11. Design a high-temperature oxidation orthogonal test, design and process performance characterization parts, use the performance characterization parts to complete the high-temperature oxidation experiment and conduct performance tests; S12, sorting out the performance results, obtaining the corresponding relationship between high temperature oxidation parameters, infrared radiation performance, and bulk performance, and completing the construction of a regularity database; S13, using intermediate parameters or repeated experiments to calibrate and compensate the database; S14. Use the database to combine the high-temperature alloy product's intrinsic properties and infrared radiation performance requirements to select high-temperature oxidation parameters.
8. A high temperature alloy having both infrared radiation performance and bulk performance, characterized in that: The invention is prepared by the preparation method according to any one of claims 1 to 7.
9. The high temperature alloy according to claim 8, characterized in that: The high-temperature alloy satisfies the requirements of infrared radiation performance and bulk performance at the same time, and has an oxide film on its surface; the oxide film is formed by the high-temperature alloy itself, and is a metal mineralize or oxide; the infrared radiation performance of the high-temperature alloy: infrared emissivity ≥0.75, bulk performance: room temperature tensile strength ≥800MPa, elongation ≥10%, 900℃ tensile strength ≥210MPa, elongation ≥10%.
10. The high temperature alloy according to claim 8 or 9, characterized in that: The oxide film has a thickness of 5 μm to 50 μm.
Citation Information
Cited By
Temperature-resistant resin-based radar wave-absorbing coating and design method and application thereof
CN119490791A
Heat treatment method for improving mechanical property of GH4099 high-temperature alloy
CN119634752A