Resistance paste and preparation method thereof
By using silver powder and other oxides to replace ruthenium powder to form a resistor paste, the problem of high cost of resistor paste is solved, achieving the effects of cost reduction and excellent electrical performance.
Patent Information
- Application Number
- CN202411321528.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-23
- Publication Date
- 2024-11-08
AI Technical Summary
The use of precious metal ruthenium powder in existing resistive pastes results in excessively high costs, limiting their application.
A lower-cost conductive phase, such as silver powder, is used to replace ruthenium powder, and appropriate amounts of precious metal oxides and other oxides are added. The resistive paste is formed by mixing them in a specific ratio, including a conductive phase, a glass phase, and an organic carrier.
This achieves a reduction in the cost of resistive pastes while maintaining good electrical performance and a low temperature coefficient, thus broadening the range of applications.
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of resistor paste, and in particular to a resistor paste and a preparation method thereof. Background Art
[0002] Resistor paste is an important foundation for the development of electronic technology towards miniaturization, high frequency, high integration and multi-dimensionality, and is used in military, aerospace, communication, computer, medical and other fields. Resistor paste is a complex multi-level dispersion system composed of a conductive phase, a glass phase and an organic carrier mixed in a certain proportion. Thick film resistors are formed by printing and sintering, in which the conductive phase plays a very critical role in the electrical properties of the paste. In current resistor pastes, the conductive phase mostly uses ruthenium-containing precious metal materials, such as the patent with announcement number CN107230540B, which leads to high costs and limits its application. Summary of the invention
[0003] In view of the shortcomings of the prior art, the present invention provides a resistor paste and a preparation method thereof, which uses other conductive phases with lower costs (such as silver powder) to replace the more expensive ruthenium powder to solve the problem of excessively high costs. The performance of the paste after the replacement is better.
[0004] To achieve the above object, the present invention provides the following technical solution: a resistor paste, comprising a conductive phase, a glass phase and an organic carrier, characterized in that: The weight percentage composition of the conductive phase, the glass phase and the organic carrier is: Conductive phase 20~80%, glass phase 10~50%, organic carrier 15~40%; The organic carrier is composed of the following components in terms of weight percentage: Resin 5~30%, organic solvent 20~90%, organic additive 1~5%; The conductive phase includes precious metal powder and precious metal oxide, such as: ruthenium-containing oxide precious metal material, silver powder, palladium powder, silver-palladium alloy powder, etc., wherein the weight of silver powder is 0.5 to 4 times that of ruthenate, preferably 1 to 3.5 times.
[0005] Furthermore, the glass phase includes glass powders of different types.
[0006] Furthermore, the resin includes one or more of ethyl cellulose, methyl cellulose, acrylic resin, hydroxyethyl cellulose, a phenolic resin mixture, a low-alcohol polyacrylic resin, and monobutylene glycol-acetate.
[0007] Furthermore, the organic solvent includes one or a mixture of terpineol, alcohol ester dodecanol, tributyl citrate, n-butanol, and other alcohol esters.
[0008] Furthermore, the organic additive includes one or more of tridecanol, castor oil, and phosphate anionic surfactants.
[0009] The present invention also provides another technical solution: a method for preparing a resistor paste, which is characterized by: 1) preparing an organic carrier: dissolving the resin in an organic solvent by heating and stirring according to the weight percentage composition, and obtaining the organic carrier after cooling; 2) Preparation of resistor paste: The conductive phase, glass phase, oxide, organic solvent, organic additive and organic carrier are uniformly mixed according to the weight percentage composition, and fully ground by rolling with a three-roll mill to a fineness of 5 μm or less to obtain a resistor paste.
[0010] Furthermore, the oxide includes one or more of manganese-containing oxides, copper oxide, titanium oxide, niobium pentoxide, zirconium boride, silicon dioxide, aluminum oxide, cobalt oxide, selenium dioxide, antimony trioxide, molybdenum trioxide, and lanthanum oxide.
[0011] Furthermore, an organic carrier is prepared: the weight ratio of resin to organic solvent is (1-1.5): (8-9.5), wherein pineol in the organic solvent accounts for 20-25% of the total weight of the organic carrier, tributyl citrate accounts for 20-25% of the total weight of the organic carrier, alcohol ester accounts for 20-25% of the total weight of the organic carrier, and other alcohol esters account for 20-25% of the total weight of the organic carrier. The resin is dissolved in the organic solvent under stirring and heating at 80-95°C, and the organic carrier is obtained after cooling.
[0012] Furthermore, a resistor paste is prepared: 12-30% of calcium ruthenate, 30-56% of silver powder, 30-35% of glass powder, 1-3% of oxide, 1-1.5% of dispersant, 0.5-0.8% of tridecanol, 10-15% of pine alcohol, 15-20% of alcohol ester dodecahydrate, and 20-25% of organic vehicle are uniformly mixed according to the weight percentage composition, and fully ground to a fineness of 5 μm or less using a three-roll mill to obtain a resistor paste; the obtained resistor paste has a resistance value of 6-9 Ω and a temperature coefficient of 10-35 ppm / ℃.
[0013] Compared with the prior art, the present invention has the following advantages and effects: the conductive phase of the present invention uses relatively cheap ruthenium acid and silver powder to replace the expensive metal ruthenium powder, and the reasonable addition of different oxides has different improvement effects on the temperature coefficient change, thereby reducing the cost of the resistor paste, and the resistor paste has good electrical properties and low temperature coefficient, so it has broad application prospects. DETAILED DESCRIPTION
[0014] The technical solutions in the embodiments of the present invention are clearly and completely described below. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present invention.
[0015] Example 1.
[0016] This embodiment provides a resistor paste and a preparation method thereof, which are specifically as follows: (1) Preparation of an organic carrier: Ethyl cellulose and an organic solvent are prepared in a weight percentage ratio of 1:9, wherein terpineol in the organic solvent accounts for 22% of the total weight of the organic carrier, tributyl citrate accounts for 22% of the total weight of the organic carrier, alcohol ester accounts for 22% of the total weight of the organic carrier, and other alcohol esters account for 22% of the total weight of the organic carrier. Ethyl cellulose is dissolved in the organic solvent under stirring and heating at 80° C., and the organic carrier is obtained after cooling.
[0017] (2) Preparation of resistor paste: 30% of calcium ruthenate, 40% of silver powder, 30% of glass powder, 3% of cobalt trioxide, 1% of dispersant, 0.5% of tridecanol, 15% of pine alcohol, 20% of alcohol ester dodecanol, and 22% of organic vehicle are uniformly mixed according to weight percentage, and the mixture is fully ground with a three-roll mill to a fineness of less than 5 μm to obtain a resistor paste.
[0018] (3) Test the resistance value and temperature coefficient TCR of the resistor paste.
[0019] Serial number Temperature / ℃ Resistance / Ω Temperature / ℃ Resistance / Ω TCR / ppm / ℃ 1 25.0 2.400 125.0 2.610 875.00 2 25.0 2.750 125.0 2.948 720.00 3 25.0 2.800 125.0 3.020 785.71 4 25.0 3.140 125.0 3.251 353.50 5 25.0 3.160 125.0 3.370 664.56 6 25.0 3.540 125.0 3.830 819.21 7 25.0 3.840 125.0 4.060 572.92 8 25.0 3.840 125.0 4.190 911.46 9 25.0 4.320 125.0 4.690 856.48 10 25.0 5.980 125.0 6.260 468.23 Example 2.
[0020] This embodiment provides a resistor paste and a preparation method thereof, which are specifically as follows: (1) Preparation of an organic carrier: Methyl cellulose and an organic solvent are prepared in a weight percentage ratio of 1:8, wherein the organic solvent comprises 22% of pineneol, 22% of tributyl citrate, 22% of alcohol ester dodecanedone, and 22% of other alcohol esters. Methyl cellulose is dissolved in the organic solvent under stirring and heating at 85° C., and the organic carrier is obtained after cooling.
[0021] (2) Preparation of resistor paste: 25% of calcium ruthenate, 45% of silver powder, 30% of glass powder, 2% of manganese dioxide, 1% of dispersant, 0.8% of tridecanol, 12% of pine alcohol, 20% of alcohol ester dodecanol, and 20% of organic vehicle are uniformly mixed according to weight percentage, and the mixture is fully ground with a three-roll mill to a fineness of less than 5 μm to obtain a resistor paste.
[0022] (3) Test the resistance value and temperature coefficient TCR of the resistor paste.
[0023] Serial number Temperature / ℃ Resistance / Ω Temperature / ℃ Resistance / Ω TCR / ppm / ℃ 1 25.0 3.133 125.0 3.298 526.65 2 25.0 3.158 125.0 3.400 766.31 3 25.0 3.263 125.0 3.399 416.79 4 25.0 3.585 125.0 3.720 376.57 5 25.0 3.867 125.0 3.974 276.70 6 25.0 4.030 125.0 4.171 349.88 7 25.0 4.067 125.0 4.192 307.35 8 25.0 4.216 125.0 4.374 374.76 9 25.0 4.336 125.0 4.490 355.17 10 25.0 4.504 125.0 4.666 359.68 Example 3.
[0024] This embodiment provides a resistor paste and a preparation method thereof, which are specifically as follows: (1) Preparation of an organic carrier: Ethyl cellulose and an organic solvent are prepared in a weight percentage ratio of 1:9, wherein pineol in the organic solvent accounts for 22% of the total weight of the organic carrier, tributyl citrate accounts for 22% of the total weight of the organic carrier, alcohol ester accounts for 22% of the total weight of the organic carrier, and other alcohol esters account for 22% of the total weight of the organic carrier. Ethyl cellulose is dissolved in the organic solvent under stirring and heating at 90° C., and the organic carrier is obtained after cooling.
[0025] (2) Preparation of resistor paste: 20% calcium ruthenate, 50% silver powder, 30% glass powder, 3% lanthanum oxide, 1.5% dispersant, 0.5% castor oil, 10% pine alcohol, 15% alcohol ester dodecahydrate, and 25% organic vehicle are uniformly mixed according to weight percentage, and fully ground by a three-roll mill to a fineness of less than 5 μm to obtain a resistor paste.
[0026] (3) Test the resistance value and temperature coefficient TCR of the resistor paste.
[0027] Serial number Temperature / ℃ Resistance / Ω Temperature / ℃ Resistance / Ω TCR / ppm / ℃ 1 25.0 4.758 125.0 4.863 220.68 2 25.0 4.763 125.0 4.914 317.03 3 25.0 5.017 125.0 5.191 346.82 4 25.0 5.262 125.0 5.424 307.87 5 25.0 5.669 125.0 5.865 345.74 6 25.0 5.784 125.0 5.904 207.47 7 25.0 5.902 125.0 6.051 252.46 8 25.0 6.764 125.0 6.925 238.02 9 25.0 7.689 125.0 7.820 170.37 10 25.0 8.177 125.0 8.356 218.91 Example 4.
[0028] This embodiment provides a resistor paste and a preparation method thereof, which are specifically as follows: (1) Preparation of an organic carrier: Ethyl cellulose and an organic solvent are prepared in a weight percentage ratio of 1:9, wherein terpineol in the organic solvent accounts for 22% of the total weight of the organic carrier, tributyl citrate accounts for 22% of the total weight of the organic carrier, alcohol ester accounts for 22% of the total weight of the organic carrier, and other alcohol esters account for 22% of the total weight of the organic carrier. Ethyl cellulose is dissolved in the organic solvent under stirring and heating at 80° C., and the organic carrier is obtained after cooling.
[0029] (2) Preparation of resistor paste: 18% ruthenium oxide, 52% silver powder, 30% glass powder, 3% manganese dioxide, 1% dispersant, 0.5% tridecanol, 15% pineol, 20% alcohol ester dodecanol, and 22% organic vehicle are uniformly mixed according to weight percentage, and the mixture is fully ground with a three-roll mill to a fineness of less than 5 μm to obtain a resistor paste.
[0030] (3) Test the resistance value and temperature coefficient TCR of the resistor paste.
[0031] Serial number Temperature / ℃ Resistance / Ω Temperature / ℃ Resistance / Ω TCR / ppm / ℃ 1 25.0 5.100 125.0 5.190 176.47 2 25.0 5.590 125.0 5.680 161.00 3 25.0 6.540 125.0 6.690 229.36 4 25.0 7.020 125.0 7.130 156.70 5 25.0 7.370 125.0 7.450 108.55 6 25.0 7.920 125.0 8.102 229.80 7 25.0 8.530 125.0 8.642 131.30 8 25.0 8.672 125.0 8.798 145.30 9 25.0 9.012 125.0 9.215 225.26 10 25.0 9.400 125.0 9.600 212.77 Example 5.
[0032] This embodiment provides a resistor paste and a preparation method thereof, which are specifically as follows: (1) Preparation of an organic carrier: Ethyl cellulose and an organic solvent are prepared in a weight percentage ratio of 1:9, wherein terpineol in the organic solvent accounts for 22% of the total weight of the organic carrier, tributyl citrate accounts for 22% of the total weight of the organic carrier, alcohol ester accounts for 22% of the total weight of the organic carrier, and other alcohol esters account for 22% of the total weight of the organic carrier. Ethyl cellulose is dissolved in the organic solvent under stirring and heating at 80° C., and the organic carrier is obtained after cooling.
[0033] (2) Preparation of resistor paste: 18% of calcium ruthenate, 50% of silver powder, 32% of glass powder, 3% of manganese dioxide, 1% of dispersant, 0.5% of tridecanol, 15% of pine alcohol, 20% of alcohol ester dodecanol, and 22% of organic vehicle are uniformly mixed according to weight percentage, and the mixture is fully ground with a three-roll mill to a fineness of less than 5 μm to obtain a resistor paste.
[0034] (3) Test the resistance value and temperature coefficient TCR of the resistor paste.
[0035] Serial number Temperature / ℃ Resistance / Ω Temperature / ℃ Resistance / Ω TCR / ppm / ℃ 1 25.0 5.289 125.0 5.441 287.39 2 25.0 5.834 125.0 5.994 274.25 3 25.0 6.098 125.0 6.264 272.22 4 25.0 6.542 125.0 6.682 214.00 5 25.0 6.804 125.0 7.002 291.01 6 25.0 7.104 125.0 7.299 274.49 7 25.0 7.133 125.0 7.303 238.33 8 25.0 7.262 125.0 7.462 275.41 9 25.0 8.697 125.0 8.899 232.26 10 25.0 9.495 125.0 9.694 209.58 Example 6.
[0036] This embodiment provides a resistor paste and a preparation method thereof, which are specifically as follows: (1) Preparation of an organic carrier: Ethyl cellulose and an organic solvent are prepared in a weight percentage ratio of 1:9, wherein terpineol in the organic solvent accounts for 22% of the total weight of the organic carrier, tributyl citrate accounts for 22% of the total weight of the organic carrier, alcohol ester accounts for 22% of the total weight of the organic carrier, and other alcohol esters account for 22% of the total weight of the organic carrier. Ethyl cellulose is dissolved in the organic solvent under stirring and heating at 80° C., and the organic carrier is obtained after cooling.
[0037] (2) Preparation of resistor paste: 15% calcium ruthenate, 55% silver powder, 30% glass powder, 3% molybdenum trioxide, 1% dispersant, 0.5% tridecanol, 15% pineol, 20% alcohol ester dodecanol, and 22% organic vehicle are uniformly mixed according to weight percentage, and the mixture is fully ground with a three-roll mill to a fineness of less than 5 μm to obtain a resistor paste.
[0038] (3) Test the resistance value and temperature coefficient TCR of the resistor paste.
[0039] Serial number Temperature / ℃ Resistance / Ω Temperature / ℃ Resistance / Ω TCR / ppm / ℃ 1 25.0 6.201 125.0 6.220 30.64 2 25.0 6.494 125.0 6.512 27.72 3 25.0 6.691 125.0 6.698 10.46 4 25.0 7.050 125.0 7.062 17.02 5 25.0 7.139 125.0 7.156 23.81 6 25.0 7.930 125.0 7.941 13.87 7 25.0 8.166 125.0 8.190 29.39 8 25.0 8.228 125.0 8.256 34.03 9 25.0 8.418 125.0 8.438 23.76 10 25.0 8.927 125.0 8.938 12.32 Example 7.
[0040] This embodiment provides a resistor paste and a preparation method thereof, which are specifically as follows: (1) Preparation of an organic carrier: Ethyl cellulose and an organic solvent are prepared in a weight percentage ratio of 1:9, wherein terpineol in the organic solvent accounts for 22% of the total weight of the organic carrier, tributyl citrate accounts for 22% of the total weight of the organic carrier, alcohol ester accounts for 22% of the total weight of the organic carrier, and other alcohol esters account for 22% of the total weight of the organic carrier. Ethyl cellulose is dissolved in the organic solvent under stirring and heating at 80° C., and the organic carrier is obtained after cooling.
[0041] (2) Preparation of resistor paste: 12% of calcium ruthenate, 56% of silver powder, 32% of glass powder, 3% of manganese dioxide, 1% of dispersant, 0.5% of tridecanol, 15% of pine alcohol, 20% of alcohol ester dodecanol, and 22% of organic vehicle are uniformly mixed according to weight percentage, and the mixture is fully ground with a three-roll mill to a fineness of less than 5 μm to obtain a resistor paste.
[0042] (3) Test the resistance value and temperature coefficient TCR of the resistor paste.
[0043] Serial number Temperature / ℃ Resistance / Ω Temperature / ℃ Resistance / Ω TCR / ppm / ℃ 1 25.0 10.760 125.0 10.994 217.47 2 25.0 11.789 125.0 11.888 83.98 3 25.0 12.241 125.0 12.410 138.06 4 25.0 12.367 125.0 12.654 232.07 5 25.0 12.453 125.0 12.563 88.33 6 25.0 12.728 125.0 12.844 91.14 7 25.0 12.766 125.0 12.875 85.38 8 25.0 12.846 125.0 13.036 147.91 9 25.0 12.895 125.0 12.921 20.16 10 25.0 14.279 125.0 14.590 217.80 The resistor paste prepared in Examples 1 to 7 was screen printed with a printing mesh of 320 meshes. After printing on the substrate, it was dried and sintered at 850° C., and then various properties of the product were tested under the same conditions.
[0044] From the test results in each table, the measured resistance values of Examples 1, 2 and 3 are too small, and the TCR is not within the test range (R≤10Ω: -100~300ppm / ℃); although the resistance value and TCR of Example 4 are within the range, compared with Examples 5 and 6, ruthenium powder is used for the conductive phase, which leads to increased costs; and in Example 7, the resistance value is too large. In Example 1, the addition of cobalt oxide makes the TCR too high; it can be seen from other examples that the addition of other oxides can reduce the TCR, except that the addition of molybdenum trioxide in Example 6 greatly reduces the TCR.
[0045] In summary, the resistor paste made of the combination with lower cost in Examples 5 and 6 has stable resistance, lower temperature coefficient, and better electrical properties, and can be used to replace the high-cost resistor paste, effectively reducing the cost of the resistor paste. At the same time, the addition of special oxides has different effects on reducing or increasing the TCR value, and can be selected according to experimental requirements in the future.
[0046] Although embodiments of the present invention have been shown and described, it will be apparent to those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and concepts of the present invention, and the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A resistor paste, comprising a conductive phase, a glass phase and an organic carrier, Its characteristics are: The weight percentage composition of the conductive phase, the glass phase and the organic carrier is: Conductive phase 20~80%, glass phase 10~50%, organic carrier 15~40%; The organic carrier is composed of the following components in terms of weight percentage: Resin 5~30%, organic solvent 20~90%, organic additive 1~5%; The conductive phase includes metal powder and metal oxide, wherein the weight of silver powder is 0.5 to 4 times that of ruthenate.
2. The resistor paste according to claim 1, Its characteristics are: The weight of the silver powder is 1 to 3.5 times that of the ruthenate.
3. The resistor paste according to claim 1, Its characteristics are: The glass phase includes glass powders of different types.
4. The resistor paste according to claim 1, Its characteristics are: The resin includes one or more of ethyl cellulose, methyl cellulose, acrylic resin, hydroxyethyl cellulose, a phenolic resin mixture, a low-alcohol polyacrylic resin, and monobutylene glycol-acetate.
5. The resistor paste according to claim 1, Its characteristics are: The organic solvent includes one or a mixture of multiple alcohol esters.
6. The resistor paste according to claim 1, Its characteristics are: The organic additive includes one or more of tridecanol, castor oil and phosphate anionic surfactant.
7. A method for preparing the resistor paste according to any one of claims 1 to 6, Its characteristics are: The details are as follows: 1) preparing an organic carrier: dissolving the resin in an organic solvent by heating and stirring according to the weight percentage composition, and obtaining the organic carrier after cooling; 2) Preparation of resistor paste: The conductive phase, glass phase, oxide, organic solvent, organic additive and organic carrier are uniformly mixed according to the weight percentage composition, and fully ground by rolling with a three-roll mill to a fineness of 5 μm or less to obtain a resistor paste.
8. The method for preparing the resistor paste according to claim 7, Its characteristics are: The oxide includes one or more of manganese-containing oxides, copper oxide, titanium oxide, niobium pentoxide, zirconium boride, silicon dioxide, aluminum oxide, cobalt oxide, selenium dioxide, antimony trioxide, molybdenum trioxide, and lanthanum oxide.
9. The method for preparing the resistor paste according to claim 7, Its characteristics are: Preparation of an organic carrier: prepare the organic carrier in a weight ratio of resin to organic solvent of (1-1.5):(8-9.5), wherein pineol in the organic solvent accounts for 20-25% of the total weight of the organic carrier, tributyl citrate accounts for 20-25% of the total weight of the organic carrier, alcohol ester accounts for 20-25% of the total weight of the organic carrier, and other alcohol esters account for 20-25% of the total weight of the organic carrier. Dissolve the resin in the organic solvent under stirring and heating at 80-95°C, and obtain the organic carrier after cooling.
10. The method for preparing the resistor paste according to claim 9, Its characteristics are: Preparation of resistor paste: 12-30% of calcium ruthenate, 30-56% of silver powder, 30-35% of glass powder, 1-3% of oxide, 1-1.5% of dispersant, 0.5-0.8% of tridecanol, 10-15% of pine alcohol, 15-20% of alcohol ester dodecahydrate, and 20-25% of organic vehicle are uniformly mixed according to the weight percentage composition, and fully ground to a fineness of 5 μm or less by rolling with a three-roll mill to obtain a resistor paste; the obtained resistor paste has a resistance value of 6-9 Ω and a temperature coefficient of 10-35 ppm / °C.
Citation Information
Cited By
Ruthenium oxide-based conductive paste, temperature sensor and preparation method thereof