Homogeneous chemical coating modified nickel powder Ni-coated NiO as well as preparation method and application thereof
By generating homogeneous chemically coated modified nickel powder Ni@NiO of the nano nickel oxide shell on the surface of the nickel powder, the internal electrode discontinuity and oxidation ease of Ni powder in MLCC are solved, and the anti-oxidation and sintering performance are improved. Suitable for efficient and economical preparation of base metal nickel electrode paste.
Patent Information
- Application Number
- CN202410913451.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-11-08
AI Technical Summary
The application of Ni powder in MLCC has problems with internal electrode discontinuity and oxidation, which leads to the impact of stability and reliability, and existing improvement methods such as the use of additives or core-shell structures with high preparation costs or affects material performance.
Homochemically coated modified nickel powder Ni@NiO, and a basic nickel carbonate coating is formed on the surface of the nickel powder by co-precipitation method, and calcined in an inert atmosphere to form a nano nickel oxide shell to form a core-shell structure to improve resistance Oxidation and sintering properties.
The antioxidant performance and sintering characteristics of nickel powder are improved. The MLCC base metal nickel electrode slurry using this modified nickel powder has excellent antioxidant and co-fired matching properties, reducing the preparation cost and avoiding the introduction of impurities.
Smart Images

Figure CN118919294A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of electronic paste preparation, and specifically relates to a homogeneous chemically coated modified nickel powder Ni@NiO and a preparation method and application thereof. Background Art
[0002] As MLCC develops towards high capacity, small size and high reliability, its production cost continues to increase, making the development of base metal internal electrodes such as Ni the focus of MLCC research. However, there are two major problems in the application of Ni powder in MLCC: First, in the preparation process of MLCC, the electrode slurry containing Ni powder is printed on the dielectric BaTiO 3 The raw porcelain belt is sintered simultaneously, and the Ni powder and the medium BaTiO 3 The different sintering behaviors will lead to the discontinuity of Ni internal electrode, and if the size of Ni powder becomes smaller, this discontinuity will be further aggravated; secondly, Ni powder is easily oxidized during application. Therefore, the maximum temperature of MLCC debinding process usually needs to be strictly controlled below 300℃, and it needs to be carried out in a non-oxidizing atmosphere or sintered in a reducing atmosphere. It is usually contradictory to further reduce the residual carbon in the final MLCC product while maintaining the excellent metal properties of Ni powder. It can be seen that the two problems of internal electrode discontinuity and easy oxidation in Ni powder co-firing will significantly affect the stability and reliability of the electrode.
[0003] The co-firing and oxidation problems of Ni powder can be improved to a certain extent by using additives, such as introducing 5-20wt% boron (B) into thick film electronic paste. Boron sintered in air to form a dense B 2 O 3 The protective layer is formed, thereby avoiding the oxidation of the Ni inner layer. Although the additive can effectively inhibit the premature sintering of pure Ni powder, the uniform dispersion of the nanoparticle mixture is another challenge. Further, the related problems can be improved by preparing nickel-based composite powders in a core-shell structure, such as synthesizing Ni@CrO with a core-shell structure using DC arc plasma in a pure nitrogen atmosphere. x Nanopowders, the prepared materials show excellent oxidation resistance and sintering properties. However, the high preparation cost of the DC arc plasma method violates the original intention of base metalization, and CrO x It belongs to the doping phase and will affect the application of MLCC. Summary of the invention
[0004] In view of the above technical problems, the purpose of the present invention is to provide a homogeneous chemically coated modified nickel powder Ni@NiO and a preparation method thereof and application in MLCC base metal nickel electrode slurry. The MLCC base metal nickel electrode slurry prepared by the modified nickel powder provided by the present invention has excellent anti-oxidation and co-firing matching properties.
[0005] In a first aspect, the present invention provides a homogeneous chemically coated modified nickel powder Ni@NiO, wherein the homogeneous chemically coated modified nickel powder Ni@NiO has a core-shell structure with nickel powder as a core and a nano nickel oxide layer as an outer shell; The particle size of the nickel powder core is 0.1-2 μm.
[0006] Preferably, based on the total mass of the homogeneous chemically coated modified nickel powder Ni@NiO being 100%, the mass of the nickel powder core accounts for 60-90%, and the mass of the nickel oxide layer shell accounts for 10-40%.
[0007] In a second aspect, the present invention provides a method for preparing the above-mentioned homogeneous chemically coated modified nickel powder Ni@NiO, the preparation method comprising the following steps: (1) dispersing nickel powder in an ammonium bicarbonate solution formed by mixing ammonium bicarbonate and an inert medium, then adding a nickel sulfate solution thereto, reacting on the surface of the nickel powder by a coprecipitation method to form a basic nickel carbonate coating layer, and after the reaction is completed, centrifuging, washing, vacuum drying, grinding and screening to obtain a nickel powder coated with basic nickel carbonate; (2) calcining the nickel powder coated with basic nickel carbonate, during which the basic nickel carbonate is decomposed into nano nickel oxide, and the homogeneous chemically coated modified nickel powder Ni@NiO is obtained through screening.
[0008] Preferably, in step (1), the inert medium is deionized water, ethanol, ethylene glycol, or glycerol; The concentration of the nickel sulfate solution is 0.1-2.0 mol / L, preferably 0.1-0.9 mol / L.
[0009] Preferably, the usage ratio of the nickel powder, the inert medium, the ammonium bicarbonate and the nickel sulfate solution is 1-6 g: 100-600 mL: 0.005-100 mol: 5-50 mL, preferably 1-6 g: 100-600 mL: 1-100 mol: 5-50 mL.
[0010] Preferably, in step (1), the nickel sulfate solution is added dropwise at a rate of 0.3-1.8 mL / min.
[0011] Preferably, in step (1), the pH value of the coprecipitation reaction system is controlled at 7-8, the coprecipitation reaction temperature is 20-40°C, and the reaction time is 1-3h.
[0012] Preferably, in step (2), the calcination is carried out under an inert atmosphere, preferably argon, nitrogen or helium; the calcination temperature is 350-600° C., and the calcination time is 10-60 min.
[0013] Preferably, in step (2), the calcined powder is sieved using a 500-mesh sieve.
[0014] In a third aspect, the present invention provides an application of the above-mentioned homogeneous chemically coated modified nickel powder Ni@NiO in the preparation of MLCC base metal nickel electrode slurry and MLCC.
[0015] Beneficial Effects The present invention provides a simple and easy-to-operate method for homogeneous chemical coating modification of nickel powder. After coating, a dense and uniform nano-nickel oxide layer is formed on the surface of the nickel powder, and the thickness of the coating layer is controllable. After coating, the anti-oxidation performance and sintering characteristics of the nickel powder are improved. The base metal nickel electrode slurry for MLCC using the nickel powder has excellent anti-oxidation and co-firing matching performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 XRD diagrams of Ni@NiO-1 prepared in Example 1 and Ni in Comparative Example 1; Figure 2-6 SEM images of Ni@NiO-1, Ni@NiO-2, Ni@NiO-3, Ni@NiO-4, and Ni@NiO-5 prepared in Examples 1-5, respectively; Figure 7 This is the SEM image of Ni@NiO-6 prepared in Comparative Example 4; Figure 8 This is the SEM image of Ni@NiO-7 prepared in Comparative Example 5; Figure 9-11 SEM images of the printed surfaces of Ni@NiO-2, Ni@NiO-3 and Ni@NiO-8 prepared in Examples 2-3 and Comparative Example 7, respectively; Fig.12 TGA graphs of Ni@NiO-1 prepared in Example 1 and Ni in Comparative Example 1; Fig.13 The modified nickel powder and BaTiO in Examples 1-3, Comparative Examples 1-3 and Comparative Examples 6-7 are 3 Comparison of thermal shrinkage curves; Fig.14 This is a photo of the nickel electrode slurry prepared in Example 1 after co-firing with the MLCC dielectric; Fig.15 This is a photo of the nickel electrode slurry prepared in Comparative Example 2 after co-firing with the MLCC dielectric; Fig.16 , 17 They are respectively the SEM image and the SEM magnified image of the nickel electrode slurry prepared in Example 1 after co-firing with the MLCC dielectric; Fig.18 , 19They are the SEM image and SEM magnified image of the nickel electrode slurry prepared in Comparative Example 2 after co-firing with the MLCC medium. DETAILED DESCRIPTION
[0017] The present invention is further described below by the following embodiments. It should be understood that the following embodiments are only used to illustrate the present invention, but not to limit the present invention.
[0018] First, the present invention provides a homogeneous chemically coated modified nickel powder Ni@NiO, wherein the homogeneous chemically coated modified nickel powder Ni@NiO has a core-shell structure with nickel powder as a core and a nano nickel oxide layer as a shell; wherein the particle size of the nickel powder core can be controlled to be 0.1-2 μm.
[0019] The core particle size of the modified nickel powder provided by the present invention is mainly formulated according to the application requirements of MLCC, which has basically no effect on the oxidation performance, but has a certain effect on the co-firing performance of the material. To a certain extent, the larger the particle size, the more conducive to co-firing, but it is not enough to improve the huge sintering characteristic temperature gap between the nickel electrode and the dielectric layer. In addition, the thickness of the outer layer increases with the increase in the amount of nickel sulfate solution added. To a certain extent, the thicker the thickness, the better the co-firing matching, and the oxidation resistance will also be improved to a certain extent.
[0020] In some embodiments, based on the total mass of the homogeneous chemically coated modified nickel powder Ni@NiO being 100%, the mass of the nickel powder core may account for 60-90%, and the mass of the nano nickel oxide layer shell may account for 10-40%.
[0021] The homogeneous chemically coated modified nickel powder Ni@NiO provided by the present invention greatly improves the oxidation resistance and sintering characteristics of Ni powder by NiO coating, and the base metal nickel electrode slurry for MLCC using the modified nickel powder has excellent oxidation resistance and co-firing matching performance. NiO coating of Ni will not bring other additional impurity elements, nor will there be the influence of element diffusion causing the change of element ratio in MLCC medium. However, such as Ni@SiO 2 and Ni@TiO 2 Such materials have relatively poor co-firing performance with the MLCC dielectric layer, making it difficult to achieve the effect of the present invention.
[0022] The following is an exemplary description of the preparation method of the homogeneous chemically coated modified nickel powder Ni@NiO provided by the present invention. The preparation method may include the following steps: (1) dispersing nickel powder in an ammonium bicarbonate solution formed by mixing ammonium bicarbonate and an inert medium, then adding a nickel sulfate solution dropwise thereto, reacting on the surface of the nickel powder to form a basic nickel carbonate coating layer by a coprecipitation method, adjusting the thickness of the coating layer by controlling the amount of nickel sulfate added, and after the reaction is completed, centrifuging, washing, vacuum drying, grinding and screening to obtain nickel powder coated with basic nickel carbonate; (2) calcining the nickel powder coated with basic nickel carbonate, during which the basic nickel carbonate is decomposed into nano nickel oxide, and the homogeneous chemically coated modified nickel powder Ni@NiO is obtained through screening.
[0023] It should be noted that if the nickel powder is mixed with the nickel sulfate solution and then the ammonium bicarbonate solution is added, a large amount of CO will be released. 2 Gas, and the addition of ammonium bicarbonate will affect the uniformity of the reaction, which is not conducive to the formation of a uniform core-shell structure. The relevant reaction principle is as follows: 3NiSO 4 +6NH 4 HCO 3 +H 2 O=NiCO 3 ·2Ni(OH) 2 ·2H 2 O↓+3(NH 4 ) 2 SO 4 +5CO 2 ↑ (1)
[0024] In addition, the reaction principle of the sintering process in the above step (2) is as follows: NiCO 3 ·2Ni(OH) 2 ·2H 2 O=3NiO+4H 2 O↑+CO 2 ↑ (2)
[0025] In some embodiments, in step (1), the particle size of the nickel powder can be 0.1-2 μm. The nickel powder particle size is controlled within this range based on the application in MLCC. If it is too large, the development of MLCC miniaturization will be restricted, and if it is too small, it will be difficult to solve its dispersion and other problems.
[0026] In some embodiments, in step (1), the inert medium may be deionized water, ethanol, ethylene glycol, or glycerol.
[0027] In some embodiments, in step (1), the concentration of the nickel sulfate solution may be 0.1-2.0 mol / L, preferably 0.1-0.9 mol / L.
[0028] In some embodiments, in step (1), the amount ratio of the nickel powder, inert medium, ammonium bicarbonate and nickel sulfate solution can be 1-6g: 100-600mL: 0.005-100mol: 5-50mL, preferably 1-6g: 100-600mL: 1-100mol: 5-50mL. The ratio of each raw material is determined according to the ratio and coating amount in the relevant reaction equation. Among them, too low a nickel powder dosage will result in too much coating, and the coated powder is easy to form hard agglomerates and difficult to disperse. Too high a nickel powder dosage will result in too little coating, and it is difficult to generate a uniform coating layer. Too low an inert medium dosage will result in too high a concentration of the reaction system and too violent a reaction. Too high an amount will result in too low a concentration of the reaction system and too slow a reaction speed. In addition, ammonium bicarbonate and nickel sulfate solution also control the appropriate amount of the reaction. Too low an amount will result in too little coating, and too high an amount will result in too much coating.
[0029] It should also be noted that the use of nickel sulfate and ammonium bicarbonate as reaction raw materials in the present invention is different from the use of nickel nitrate or nickel acetate and urea. Although the latter can achieve nickel powder coating, the coated powder has poor dispersibility and is easy to aggregate into clumps after printing rather than obtaining a flat electrode layer; in addition, its co-firing properties with MLCC dielectric materials are poor and cannot meet the requirements of the present technical invention.
[0030] In some embodiments, in step (1), the dropping speed of the nickel sulfate solution can be 0.3-1.8 mL / min.
[0031] In some embodiments, in step (1), the pH value of the coprecipitation reaction system is controlled at 7 to 8. If the pH value is too high, the equilibrium constant of the chemical reaction will be destroyed, which is not conducive to the reaction.
[0032] In some embodiments, in step (1), the coprecipitation reaction temperature may be 20-40° C. and the reaction time may be 1-3 h.
[0033] In some embodiments, in step (1), the mesh size of the ground sieve can be 200-500.
[0034] In some embodiments, in step (2), the calcination is performed under an inert atmosphere, preferably argon, nitrogen, or helium.
[0035] In some embodiments, in step (2), the calcination temperature may be 350-600° C., and the calcination time may be 10-60 min. Too low a temperature or too short a calcination time may result in the inability to completely thermally decompose the basic nickel carbonate, while too high a temperature or too long a calcination time may result in the grain growth of the nickel powder due to the heat, causing agglomeration.
[0036] In some embodiments, in step (2), the calcined powder is sieved using a 500-mesh sieve.
[0037] The present invention realizes homogeneous chemical coating of nickel powder through a simple co-precipitation method, which not only improves the anti-oxidation performance of nickel powder, but also improves the co-firing matching characteristics of base metal nickel electrode slurry and MLCC medium, which is of great significance for the base metalization of MLCC technology.
[0038] The homogeneous chemically coated modified nickel powder Ni@NiO provided by the present invention can be used to prepare MLCC base metal nickel electrode slurry and MLCC.
[0039] The following further examples are given to illustrate the present invention in detail. It should also be understood that the following examples are only used to further illustrate the present invention and cannot be construed as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the above content of the present invention all belong to the scope of protection of the present invention. The specific process parameters of the following examples are also only examples within a suitable range, that is, those skilled in the art can make selections within a suitable range through the description of this article, and are not limited to the specific values exemplified below. If not specifically stated, the technical means used in the embodiments are conventional means well known to those skilled in the art.
[0040] Example 1
[0041] The preparation method of the homogeneous chemically coated modified nickel powder Ni@NiO provided in this embodiment comprises the following steps: Take 3 g of nickel powder with a particle size of 150 nm and place it in 300 mL of deionized water and 0.005 mol NH 4 HCO 3 Configured NH 4 HCO 3 The solution was stirred for 20 min and ultrasonicated for 10 min. After the ultrasonication, the beaker was placed on a stirrer and stirred continuously. At the same time, 12.5 mL (0.2 mol / L) NiSO was slowly added dropwise using a rubber-tipped dropper. 4 The solution was stirred continuously for 2 hours, the mixed solution was centrifuged and washed, and placed in a vacuum oven at 80°C for 12 hours. After drying, the sample was ground and sieved, calcined at 400°C for 30 minutes under a nitrogen atmosphere, and sieved with a 500-mesh sieve to obtain the homogeneous chemically coated modified nickel powder Ni@NiO-1. The homogeneous chemically coated modified nickel powder Ni@NiO-1 is used to prepare base metal nickel electrode slurry for MLCC.
[0042] Example 2
[0043] The preparation method of the homogeneous chemically coated modified nickel powder Ni@NiO provided in this embodiment comprises the following steps: Take 2 g of nickel powder with a particle size of 1 μm and place it in 300 mL of deionized water and 0.005 mol NH 4 HCO 3 Configured NH 4 HCO 3 The solution was stirred for 20 min and ultrasonicated for 10 min. After the ultrasonication, the beaker was placed on a stirrer and stirred continuously. At the same time, 25 mL (0.2 mol / L) NiSO was slowly added using a rubber dropper. 4 The solution was stirred continuously for 3 hours, the mixed solution was centrifuged and washed, and placed in a vacuum oven at 80°C for 12 hours. After drying, the sample was ground and sieved, calcined at 500°C for 20 minutes under a nitrogen atmosphere, and sieved with a 500-mesh sieve to obtain the homogeneous chemically coated modified nickel powder Ni@NiO-2. Use the homogeneous chemically coated modified nickel powder Ni@NiO-2 to prepare base metal nickel electrode slurry for MLCC
[0044] Example 3
[0045] The preparation method of the homogeneous chemically coated modified nickel powder Ni@NiO provided in this embodiment comprises the following steps: Take 1g of nickel powder with a particle size of 100nm and place it in 300mL of ethanol and 0.005mol NH 4 HCO 3 Configured NH 4 HCO 3 The solution was stirred for 20 min and ultrasonicated for 10 min. After the ultrasonication, the beaker was placed on a stirrer and stirred continuously. At the same time, 37.5 mL (0.2 mol / L) NiSO was slowly added using a rubber-tipped dropper. 4 The solution was stirred continuously for 2 hours, the mixed solution was centrifuged and washed, and placed in a vacuum oven at 80°C for 12 hours. After drying, the sample was ground and sieved, calcined at 350°C for 60 minutes under a helium atmosphere, and sieved with a 500-mesh sieve to obtain the homogeneous chemically coated modified nickel powder Ni@NiO-3. Use the homogeneous chemically coated modified nickel powder Ni@NiO-3 to prepare base metal nickel electrode slurry for MLCC
[0046] Example 4
[0047] The preparation method of the homogeneous chemically coated modified nickel powder Ni@NiO provided in this embodiment comprises the following steps: Take 5g of nickel powder with a particle size of 2μm and place it in 300mL of ethylene glycol and 0.005mol NH 4 HCO 3 Configured NH 4 HCO 3The solution was stirred for 20 min and ultrasonicated for 10 min. After the ultrasonication, the beaker was placed on a stirrer and stirred continuously. At the same time, 50 mL (0.2 mol / L) NiSO was slowly added using a rubber dropper. 4 The solution was stirred continuously for 2 hours, the mixed solution was centrifuged and washed, and placed in a vacuum oven at 80°C for 12 hours. After drying, the sample was ground and sieved, calcined at 600°C for 10 minutes under an argon atmosphere, and sieved with a 500-mesh sieve to obtain the homogeneous chemically coated modified nickel powder Ni@NiO-4. Use the homogeneous chemically coated modified nickel powder Ni@NiO-4 to prepare base metal nickel electrode slurry for MLCC
[0048] Example 5
[0049] The preparation method of the homogeneous chemically coated modified nickel powder Ni@NiO provided in this embodiment comprises the following steps: Take 3 g of nickel powder with a particle size of 150 nm and place it in 300 mL of deionized water and 0.005 mol NH 4 HCO 3 Configured NH 4 HCO 3 The solution was stirred for 20 min and ultrasonicated for 10 min. After the ultrasonication, the beaker was placed on a stirrer and stirred continuously. At the same time, 10 mL (2 mol / L) NiSO was slowly added using a rubber dropper. 4 The solution was stirred continuously for 2 hours, the mixed solution was centrifuged and washed, and placed in a vacuum oven at 80°C for 12 hours. After drying, the sample was ground and sieved, calcined at 400°C for 60 minutes under a nitrogen atmosphere, and sieved with a 500-mesh sieve to obtain the homogeneous chemically coated modified nickel powder Ni@NiO-5. Use the homogeneous chemically coated modified nickel powder Ni@NiO-5 to prepare base metal nickel electrode slurry for MLCC
[0050] Comparative Example 1
[0051] In this comparative example 1, uncoated nickel powder Ni with a particle size of 150 nm was used to prepare base metal nickel electrode slurry for MLCC.
[0052] Comparative Example 2
[0053] The base metal nickel electrode slurry for MLCC in this comparative example refers to Example 1, with the main difference being that silicon oxide-coated nickel powder is used, specifically: 3 g of nickel powder with a particle size of 150 nm was placed in 300 mL of anhydrous ethanol, stirred for 20 min, and ultrasonicated for 10 min. After the ultrasonication, the beaker was placed on a stirrer for continuous stirring, and 3.6 mL of LTEOS was slowly added dropwise using a pipette, and the stirring was continued for 6 h. The mixed solution was centrifuged and washed, and placed in a vacuum oven at 80 ° C for 12 h. After drying, it was ground and sieved with a 500-mesh sieve to obtain silicon oxide-coated nickel powder Ni@SiO 2 -1. The silicon oxide-coated nickel powder Ni@SiO 2 -1 Preparation of base metal nickel electrode slurry for MLCC.
[0054] Comparative Example 3
[0055] The base metal nickel electrode slurry for MLCC in this comparative example refers to Example 1, with the main difference being that silicon oxide-coated nickel powder is used, specifically: 3 g of nickel powder with a particle size of 150 nm was placed in 300 mL of anhydrous ethanol, stirred for 20 min, and ultrasonicated for 10 min. After the ultrasonication, the beaker was placed on a stirrer for continuous stirring, and 1.8 mL of TEOS was slowly added dropwise using a pipette, and the stirring was continued for 6 h. The mixed solution was centrifuged and washed, and placed in a vacuum oven at 80 ° C for 12 h. After drying, it was ground and sieved with a 500-mesh sieve to obtain silicon oxide-coated nickel powder Ni@SiO 2 -2. The silicon oxide-coated nickel powder Ni@SiO 2 -2 Preparation of base metal nickel electrode slurry for MLCC.
[0056] Comparative Example 4
[0057] The base metal nickel electrode slurry for MLCC in this comparative example refers to Example 1, the main difference is that: alkaline NH 4 HCO 3 The order of adding the solution and nickel sulfate is opposite, specifically: Take 3g of nickel powder with a particle size of 150nm and place it in 300mL of deionized water and 0.0025mol NiSO 4 Configured into NiSO 4 The solution was stirred for 20 min and ultrasonicated for 10 min. After the ultrasonication, the beaker was placed on a stirrer and stirred continuously. At the same time, 0.3 mL (16.67 mol / L) NH 4 HCO 3 The solution was stirred continuously for 2 hours, the mixed solution was centrifuged and washed, and placed in a vacuum oven at 80°C for 12 hours. After drying, the sample was ground and sieved, calcined at 400°C for 30 minutes under a nitrogen atmosphere, and sieved with a 500-mesh sieve to obtain the modified nickel powder Ni@NiO-6. The homogeneous chemically coated modified nickel powder Ni@NiO-6 is used to prepare base metal nickel electrode slurry for MLCC.
[0058] Comparative Example 5
[0059] The base metal nickel electrode slurry for MLCC in this comparative example refers to Example 1, with the main difference being that the usage ratios of nickel powder and inert medium, ammonium bicarbonate and nickel sulfate solution are not appropriate, specifically: Take 0.5 g of nickel powder with a particle size of 150 nm and place it in 300 mL of deionized water and 0.005 mol NH 4 HCO 3 Configured NH 4 HCO 3 The solution was stirred for 20 min and ultrasonicated for 10 min. After the ultrasonication, the beaker was placed on a stirrer and stirred continuously. At the same time, 12.5 mL (0.2 mol / L) NiSO was slowly added dropwise using a rubber-tipped dropper. 4 The solution was stirred continuously for 2 hours, the mixed solution was centrifuged and washed, and placed in a vacuum oven at 80°C for 12 hours. After drying, the sample was ground and sieved, calcined at 400°C for 30 minutes under a nitrogen atmosphere, and sieved with a 500-mesh sieve to obtain the homogeneous chemically coated modified nickel powder Ni@NiO-7. The homogeneous chemically coated modified nickel powder Ni@NiO-7 is used to prepare base metal nickel electrode slurry for MLCC.
[0060] Comparative Example 6
[0061] The base metal nickel electrode slurry for MLCC in this comparative example refers to Example 1, with the main difference being that nickel powder coated with titanium oxide is used, specifically: 3 g of nickel powder with a particle size of 150 nm was placed in 300 mL of anhydrous ethanol, stirred for 20 min, and ultrasonicated for 10 min. After the ultrasonication, the beaker was placed on a stirrer for continuous stirring, and 1.2 mL of tetrabutyl titanate TBOT was slowly added dropwise using a pipette, and the stirring was continued for 6 h. The mixed solution was centrifuged and washed, and placed in a vacuum oven at 80 ° C for 12 h. After drying, it was ground and sieved with a 500-mesh sieve to obtain titanium oxide-coated nickel powder Ni@TiO 2 . The titanium oxide-coated nickel powder Ni@TiO 2 Preparation of base metal nickel electrode slurry for MLCC.
[0062] Comparative Example 7
[0063] The base metal nickel electrode slurry for MLCC in this comparative example refers to Example 1, with the main difference being that nickel oxide-coated nickel powder is prepared using nickel nitrate and urea, specifically: 3 g of nickel powder with a particle size of 150 nm and 0.015 mol PEG-400 were placed in a solution prepared by 300 mL of deionized water and 0.06 mol urea, stirred for 20 min, and ultrasonicated for 10 min. After the ultrasonication, the beaker was placed on a stirrer for continuous stirring, and 0.015 mol Ni(NO 3 ) 2 6H 2 O, stirred for 20 min, and ultrasonicated for 10 min; after the ultrasonication, heated to 80 ° C in a water bath, stirred for 6 h, the mixed solution was centrifuged and washed, and placed in a vacuum oven at 80 ° C for 12 h. After drying, the sample was ground and sieved, calcined at 400 ° C for 30 min under a nitrogen atmosphere, and sieved with a 500 mesh sieve to obtain modified nickel powder Ni@NiO-8. The nickel powder Ni@NiO-8 coated with nickel oxide is used to prepare base metal nickel electrode slurry for MLCC.
[0064] The modified nickel powder and its base metal nickel electrode slurry for MLCC Ni@NiO-1, Ni@NiO-2, Ni@NiO-3, Ni@NiO-4, Ni@NiO-5, Ni, Ni@SiO 2 -1. Ni@SiO 2 -2. Ni@NiO-6, Ni@NiO-7, Ni@TiO 2 , Ni@NiO-8 were used for comparative test verification.
[0065] Figure 1 The XRD diagrams of Ni@NiO-1 prepared in Example 1 and Ni in Comparative Example 1 are shown in FIG. Figure 2-6 The SEM images of Ni@NiO-1, Ni@NiO-2, Ni@NiO-3, Ni@NiO-4 and Ni@NiO-5 prepared in Examples 1 to 5 are shown respectively. It can be seen from the figure that the nickel oxide thin layer in the modified nickel powder prepared in the embodiment of the present invention is evenly dispersed on the surface of the nickel powder, and the homogeneous chemical coating of the nickel powder is successfully achieved.
[0066] Figure 7 This is a SEM image of Ni@NiO-6 prepared in Comparative Example 4. As can be seen from the figure, Ni@NiO-6 has uneven coating, some particles are basically not coated, and there is also a phenomenon of shell material deposition. This is mainly due to the release of CO during the co-precipitation reaction of nickel sulfate and ammonium bicarbonate. 2 Gas, the post-addition of ammonium bicarbonate leads to uneven gas release, which affects the uniformity of the reaction and is not conducive to the formation of a uniform core-shell structure.
[0067] Figure 8This is a SEM image of Ni@NiO-7 prepared in Comparative Example 5. As can be seen from the figure, the nickel powder in Ni@NiO-7 is obviously coated too much, and the nickel powder is sticky and agglomerated. This is mainly due to the inappropriate ratio of nickel powder, inert medium, ammonium bicarbonate and nickel sulfate solution, resulting in too much Ni@NiO shell in the final preparation. Therefore, the order and amount of raw material addition need to be within the range shown in this patent, otherwise it is difficult to obtain uniformly coated Ni@NiO.
[0068] The Ni@NiO-2, Ni@NiO-3 and Ni@NiO-8 nickel pastes prepared in Examples 2-3 and Comparative Example 7 were printed on MLCC dielectric green ceramic tapes, and the printability was compared after drying. Figure 9-11 The SEM images of the printed surfaces of Ni@NiO-2, Ni@NiO-3 and Ni@NiO-8 prepared in Examples 2-3 and Comparative Example 7 are shown. As can be seen from the figure, compared with Ni@NiO-2 and Ni@NiO-3, the printed surface of Ni@NiO-8 is uneven, which is attributed to the poor dispersibility of the coated powder Ni@NiO-8 generated by nickel nitrate and urea. It is easy to aggregate into agglomerates after printing, and a flat electrode layer cannot be obtained. Therefore, the nickel salt preparation technology selected by the present invention is better.
[0069] The coated Ni@NiO-1 and uncoated nickel powder were placed in air and subjected to thermogravimetric analysis at a heating rate of 10°C / min to characterize their antioxidant properties. Fig.12 The TGA graph of Ni@NiO-1 prepared in Example 1 and Ni in Comparative Example 1. It can be seen from the figure that the initial oxidation (weight gain) temperature of Ni@NiO-1 is 672.8°C, which is higher than Ni 521.8°C, and the weight gain of Ni@NiO-1 is 121.6%, which is much lower than Ni 125.7%, indicating that the homogeneous chemical coating of nickel powder improves its antioxidant properties.
[0070] The nickel powders with homogeneous chemical coating, the nickel powders with silicon oxide coating, the nickel powders with titanium oxide coating, the uncoated nickel powders and the dielectric powders BaTiO 3 TMA test was carried out to characterize its co-firing matching characteristics. Fig.13 The modified nickel powder and BaTiO in Examples 1-3, Comparative Examples 1-3 and Comparative Examples 6-7 are 3 Comparison of thermal shrinkage curves. It can be seen from the figure that the nickel powder (Ni@NiO-1, Ni@NiO-2, Ni@NiO-3, Ni@SiO 2 -1. Ni@SiO 2 -2. Ni@TiO 2 The shrinkage starting temperature of Ni@NiO-8) is higher than that of uncoated Ni. Coating modification is beneficial to bridge the gap between Ni and dielectric powder BaTiO 3There is a huge sintering temperature difference between the two. Among them, the silicon oxide coated modified nickel powder (Ni@SiO 2 -1. Ni@SiO 2 -2) Although the shrinkage starting temperature is closer to that of the dielectric powder BaTiO 3 , its shrinkage rate is similar to that of the dielectric powder BaTiO 3 The phase difference is large, which is not conducive to the matching co-firing of the electrode and the dielectric layer; the titanium oxide coated modified nickel powder (Ni@TiO 2 ) has no obvious improvement on the sintering shrinkage starting temperature, and its shrinkage rate is similar to that of the dielectric powder BaTiO 3 There is also a certain gap; the co-firing properties of the coated powder Ni@NiO-8 generated by nickel nitrate and urea are not significantly improved; however, the shrinkage rate of the homogeneous chemically coated nickel powder (Ni@NiO-1, Ni@NiO-2, Ni@NiO-3) provided by the embodiment of the present invention is almost the same as that of the dielectric powder BaTiO 3 This indicates that the homogeneous chemical coating of the nickel powder of the present invention is more conducive to its matching co-firing with the dielectric material and is more suitable for application in MLCC, which can also be verified in the relevant pictures of the co-firing experiment described later.
[0071] Fig.14 This is a photo of the nickel electrode slurry prepared in Example 1 after co-firing with the MLCC medium. As can be seen from the figure, the sample after co-firing with the nickel electrode slurry prepared by the homogeneous chemically coated nickel powder Ni@NiO-1 and the MLCC medium is very flat.
[0072] Fig.15 This is a photo of the nickel electrode slurry prepared in Comparative Example 2 after co-firing with the MLCC medium. As can be seen from the figure, the silicon oxide coated nickel powder Ni@SiO 2 After the -1 slurry was co-fired with the MLCC dielectric, obvious warping occurred.
[0073] Fig.16 , 17 They are respectively the SEM image and the SEM magnified image of the nickel electrode slurry prepared in Example 1 after co-firing with the MLCC dielectric; Fig.18 , 19 The SEM images and SEM magnified images of the nickel electrode slurry prepared in Comparative Example 2 after co-firing with the MLCC medium are shown in the figure. It can be seen from the figure that the electrode continuity of the sample prepared by the homogeneous chemically coated nickel powder Ni@NiO-1 is significantly better than that of the silicon oxide coated nickel powder Ni@SiO 2 -1, and there is no obvious stratification, cracking and other phenomena, which further illustrates that the homogeneous chemical coating of nickel powder is conducive to its matching co-firing with the dielectric material and is suitable for application in MLCC.
[0074] Although the content of the present invention has been described in detail through the above preferred embodiments, it should be appreciated that the above description should not be considered as a limitation of the present invention. After reading the above content, it will be apparent to those skilled in the art that various modifications and substitutions of the present invention will occur. Therefore, the protection scope of the present invention should be limited by the appended claims.
Claims
1. A homogeneous chemically coated modified nickel powder Ni@NiO, It is characterized in that The homogeneous chemically coated modified nickel powder Ni@NiO has a core-shell structure with nickel powder as the core and nano nickel oxide layer as the shell; The particle size of the nickel powder core is 0.1-2 μm.
2. The homogeneous chemically coated modified nickel powder Ni@NiO according to claim 1, It is characterized in that Taking the total mass of the homogeneous chemically coated modified nickel powder Ni@NiO as 100%, the mass of the nickel powder core accounts for 60-90%, and the mass of the nickel oxide layer shell accounts for 10-40%.
3. A method for preparing the homogeneous chemically coated modified nickel powder Ni@NiO according to claim 1 or 2, It is characterized in that The preparation method comprises the following steps: (1) dispersing nickel powder in an ammonium bicarbonate solution formed by mixing ammonium bicarbonate and an inert medium, then adding a nickel sulfate solution thereto, reacting on the surface of the nickel powder by a coprecipitation method to form a basic nickel carbonate coating layer, and after the reaction is completed, centrifuging, washing, vacuum drying, grinding and screening to obtain a nickel powder coated with basic nickel carbonate; (2) calcining the nickel powder coated with basic nickel carbonate, during which the basic nickel carbonate is decomposed into nano nickel oxide, and the nano nickel oxide is sieved to obtain the homogeneous chemically coated modified nickel powder Ni@NiO.
4. The preparation method according to claim 3, It is characterized in that In step (1), the inert medium is deionized water, ethanol, ethylene glycol, or glycerol; The concentration of the nickel sulfate solution is 0.1-2.0 mol / L, preferably 0.1-0.9 mol / L.
5. The preparation method according to claim 3 or 4, It is characterized in that The usage ratio of the nickel powder, the inert medium, the ammonium bicarbonate and the nickel sulfate solution is 1-6 g: 100-600 mL: 0.005-100 mol: 5-50 mL, preferably 1-6 g: 100-600 mL: 1-100 mol: 5-50 mL.
6. The preparation method according to any one of claims 3 to 5, It is characterized in that In step (1), the nickel sulfate solution is added dropwise at a rate of 0.3-1.8 mL / min.
7. The preparation method according to any one of claims 3 to 6, It is characterized in that In step (1), the pH value of the coprecipitation reaction system is controlled at 7-8, the coprecipitation reaction temperature is 20-40° C., and the reaction time is 1-3 h.
8. The preparation method according to any one of claims 3 to 7, It is characterized in that In step (2), the calcination is carried out under an inert atmosphere, preferably argon, nitrogen or helium; The calcination temperature is 350-600° C., and the calcination time is 10-60 min.
9. The preparation method according to any one of claims 3 to 8, It is characterized in that In step (2), the calcined powder is sieved using a 500-mesh sieve.