Electrolyte with low self-discharge at high temperature as well as preparation method and application of electrolyte
By using mixed organic electrolyte, carbonate additives and succinic anhydride in sodium ion capacitors, the SEI and CEI protective layers are constructed, which solves the problem of self-discharge at high temperatures of sodium ion capacitors, and improves electrochemical performance and cycle stability.
Patent Information
- Application Number
- CN202411151154.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-08
AI Technical Summary
Sodium ion capacitors are prone to self-discharge at high temperatures, resulting in voltage attenuation and leakage current, limiting their sodium storage capacity and service life.
Using mixed organic electrolyte, carbonate additives and succinic anhydride, a dense SEI layer is constructed on the surface of the negative electrode and a uniform CEI protective layer is formed on the surface of the positive electrode, which reduces the side reaction between the electrode and the electrolyte and reduces the self-discharge rate. .
It significantly reduces the self-discharge rate of sodium ion capacitors at high temperatures, improves cyclic stability and rate performance, extends the structural stability of the electrode material, and enhances the Coulomb efficiency and cycle life.
Smart Images

Figure CN118919312A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of supercapacitors, and in particular to an electrolyte with low self-discharge at high temperature, and a preparation method and application thereof. Background Art
[0002] With the increasing energy consumption in advanced applications such as aerospace, electric vehicles, drones, robots and various electronic devices, as well as the uneven distribution of clean energy, it is crucial to develop new energy storage devices with high power density, high energy density, long cycle life and low self-discharge rate.
[0003] Sodium ion capacitors are a new type of energy storage device after lithium ion capacitors. Compared with other energy storage devices, their significant advantages are low cost, abundant natural resources, and suitability for large-scale energy storage. Like other electrochemical energy storage devices, sodium ion capacitors will inevitably produce self-discharge, and high temperature will aggravate the self-discharge behavior of the device.
[0004] In sodium ion capacitors, the electrolyte plays an important role as a link between the positive and negative electrodes and a carrier of charge transfer. At high temperatures, the electrolyte is prone to decomposition, which accelerates the occurrence of side reactions and thus accelerates self-discharge, resulting in a large amount of voltage attenuation and increased leakage current, which seriously limits the sodium storage capacity of sodium ion capacitors.
[0005] In order to overcome the above problems, the prior art often uses sodium ion battery positive electrode materials with excellent sodium storage performance to improve the sodium storage capacity of sodium ion capacitors, and at the same time to make up for the generally low energy density of sodium ion batteries. For example, the Chinese patent application with publication number CN114792788A discloses a sodium ion full battery and its preparation method, which utilizes the antioxidant properties and hydrophobicity of sodium iron sulfate composite positive electrode materials to achieve the high operating voltage and excellent cycle stability and rate performance of the entire sodium ion battery, and at the same time utilizes the high electronic conductivity and high hydrophobicity of carbon nanotubes to improve the conductivity while effectively reducing the possibility of oxidation of the positive electrode material, thereby improving the service life of the positive electrode sheet. However, there is currently no report on related research on improving the electrolyte to reduce the self-discharge performance of sodium ion capacitors and improve their service life.
[0006] Therefore, how to improve the electrolyte of sodium ion capacitors so that the sodium ion capacitors have low self-discharge rate and excellent electrochemical properties at high temperatures has become a technical problem to be solved urgently in this field. Summary of the invention
[0007] The object of the present invention is to provide an electrolyte with low self-discharge at high temperature, and a preparation method and application thereof. The sodium ion capacitor assembled with the electrolyte provided by the present invention has the characteristics of low self-discharge rate, good cycle stability and excellent electrochemical performance at high temperature.
[0008] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0009] The present invention provides an electrolyte with low self-discharge at high temperature, comprising a mixed organic electrolyte, a carbonate additive and succinic anhydride;
[0010] The mixed organic electrolyte comprises ethylene carbonate, dimethyl carbonate and electrolyte sodium salt.
[0011] Preferably, the volume ratio of ethylene carbonate to dimethyl carbonate in the mixed organic electrolyte is 1:(0.5-2).
[0012] Preferably, the electrolyte sodium salt is sodium perchlorate.
[0013] Preferably, the concentration of the electrolyte sodium salt in the mixed organic electrolyte is 0.5-1.5 mol / L.
[0014] Preferably, the carbonate additive is fluoroethylene carbonate.
[0015] Preferably, the mass of the carbonate additive is 1-5% of the mass of the mixed organic electrolyte.
[0016] Preferably, the mass of the succinic anhydride is 2-4% of the mass of the mixed organic electrolyte.
[0017] The present invention provides a method for preparing an electrolyte with low self-discharge at high temperature as described in the above technical solution, comprising: mixing a mixed organic electrolyte, a carbonate additive and succinic anhydride to obtain an electrolyte.
[0018] The present invention provides the use of the electrolyte with low self-discharge at high temperature described in the above technical solution or the electrolyte with low self-discharge at high temperature prepared by the preparation method described in the above technical solution in a sodium ion capacitor.
[0019] Preferably, the negative electrode material of the sodium ion capacitor is a niobium-based material, and the positive electrode material of the sodium ion capacitor is an activated carbon-sodium nickel iron manganese oxide composite material.
[0020] The present invention provides an electrolyte with low self-discharge at high temperature, comprising a mixed organic electrolyte, a carbonate additive and succinic anhydride; the composition of the mixed organic electrolyte comprises ethylene carbonate, dimethyl carbonate and electrolyte sodium salt. The present invention can effectively improve the problem that the electrolyte is easy to decompose at high temperature by adding carbonate additives to the electrolyte. The carbonate additives will decompose in advance during the charging and discharging process, preventing other components in the electrolyte from participating in the formation of the SEI layer, which is conducive to constructing a SEI layer with a strong structure, dense and uniform structure and rich in sodium fluoride on the surface of the negative electrode material, which can improve the rate performance and specific capacity of the sodium ion capacitor at high temperature while reducing its self-discharge rate, broaden the working temperature range of the electrolyte, and thus improve the coulomb efficiency and cycle stability of the sodium ion capacitor; succinic anhydride can form a synergistic effect with the carbonate additive, and form a uniform and stable CEI protective layer on the positive electrode surface during the charging and discharging process, reduce the side reaction between the electrode and the electrolyte, and effectively reduce the decomposition of the electrolyte during the charging and discharging process, thereby further improving the structural stability of the electrode material during the cycle process, and significantly improving the coulomb efficiency and rate performance. The results of the examples show that the sodium ion capacitor assembled with the electrolyte provided by the present invention can be normally charged and discharged at 60° C., and after 120 hours, the voltage retention rate is 40%, the leakage current is 0.16 mA, and the self-discharge rate decreases by 18%. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 A transmission electron microscopy image of the SEI formed on the surface of the carbon-coated T-Nb2O5 negative electrode material at 60° C. by the electrolyte provided in Example 6 of the present invention;
[0022] Figure 2 A comparison chart of the rate performance of the electrolytes provided in Example 6 and Comparative Example 2 at 60° C. and different current densities;
[0023] Figure 3 A comparison chart of the cycle performance of the electrolyte provided in Example 6 and Comparative Example 2 at 60° C. and 1.0 A / g current density;
[0024] Figure 4 The cyclic voltammetry curves of the sodium ion capacitor in Application Example 1 at different scan rates at 60°C;
[0025] Figure 5 The cyclic voltammetry curves of the sodium ion capacitor in Application Example 1 at different scan rates are compared at 60°C;
[0026] Figure 6 1 is the self-discharge curve of the sodium ion capacitor in Application Example 1 and Comparative Application Example 1;
[0027] Figure 7 1 is the leakage current curve of the sodium ion capacitor in Application Example 1 and Comparative Application Example 1. DETAILED DESCRIPTION
[0028] The present invention provides an electrolyte with low self-discharge at high temperature, comprising a mixed organic electrolyte, a carbonate additive and succinic anhydride. The present invention can effectively improve the problem that the electrolyte is prone to decomposition at high temperature by adding a carbonate additive to the electrolyte. The carbonate additive will decompose in advance during the charging and discharging process, preventing other components in the electrolyte from participating in the formation of the SEI layer, which is conducive to building a solid SEI layer on the surface of the negative electrode material, thereby improving the coulomb efficiency and cycle stability of the sodium ion capacitor; succinic anhydride can form a synergistic effect with the carbonate additive, and form a uniform and stable CEI protective layer on the positive electrode surface during the charging and discharging process, reducing the side reaction between the electrode and the electrolyte, thereby further improving the structural stability of the electrode material during the cycle.
[0029] In the present invention, the mixed organic electrolyte comprises ethylene carbonate, dimethyl carbonate and electrolyte sodium salt.
[0030] In the present invention, the preparation method of the mixed organic electrolyte is preferably to mix electrolyte sodium salt with ethylene carbonate and dimethyl carbonate to obtain a mixed organic electrolyte. In the present invention, the mixing is preferably carried out under the condition of magnetic stirring. The present invention has no special limitation on the time of the mixing, as long as the mixed organic electrolyte can be mixed to homogeneity. In the present invention, the mixing is preferably carried out under anhydrous and oxygen-free conditions, more preferably in a glove box filled with argon. The present invention can avoid the electrolyte from being contaminated by water and oxygen by controlling the mixing conditions.
[0031] In the present invention, the volume ratio of ethylene carbonate to dimethyl carbonate in the mixed organic electrolyte is preferably 1: (0.5-2), more preferably 1: 1. The present invention can improve the solubility of additives and sodium salts by utilizing the synergistic effect of ethylene carbonate and dimethyl carbonate.
[0032] In the present invention, the electrolyte sodium salt is preferably sodium perchlorate; the concentration of the electrolyte sodium salt in the mixed organic electrolyte is preferably 0.5-1.5 mol / L, more preferably 0.8-1.2 mol / L, and further preferably 1 mol / L. The present invention can form a dense SEI protective layer at the negative electrode with the carbonate additive by adding sodium salt, isolating the contact between the negative electrode and the electrolyte, thereby inhibiting the self-discharge behavior of the sodium ion capacitor; by controlling the type and amount of sodium salt, the thickness and density of the formed SEI protective layer can be further regulated, thereby further inhibiting the self-discharge behavior of the sodium ion capacitor.
[0033] In the present invention, the carbonate additive is preferably fluoroethylene carbonate; the mass of the carbonate additive is preferably 1-5% of the mass of the mixed organic electrolyte, more preferably 2-4%, and further preferably 3%. By controlling the amount of the carbonate additive, the thickness and density of the SEI protective layer formed with the sodium salt can be controlled, thereby further suppressing the self-discharge behavior of the sodium ion capacitor.
[0034] In the present invention, the mass of the succinic anhydride is preferably 2-4% of the mass of the mixed organic electrolyte, and more preferably 3%. By controlling the amount of succinic anhydride used, the present invention can control the uniformity and stability of the CEI layer formed on the positive electrode surface, thereby further improving the high temperature cycle stability of the sodium ion capacitor.
[0035] The present invention can effectively improve the problem that the electrolyte is prone to decomposition at high temperature by adding carbonate additives to the electrolyte. The carbonate additives will decompose in advance during the charge and discharge process, preventing other components in the electrolyte from participating in the formation of the SEI layer, which is conducive to constructing a SEI layer with a strong structure, dense and uniform, and rich in sodium fluoride on the surface of the negative electrode material, while improving the rate performance and specific capacity of the sodium ion capacitor at high temperature, reducing its self-discharge rate, broadening the working temperature range of the electrolyte, and thus improving the coulomb efficiency and cycle stability of the sodium ion capacitor; succinic anhydride can form a synergistic effect with the carbonate additives, and form a uniform and stable CEI protective layer on the positive electrode surface during the charge and discharge process, reducing the side reaction between the electrode and the electrolyte, effectively reducing the decomposition of the electrolyte during the charge and discharge process, thereby further improving the structural stability of the electrode material during the cycle process, and significantly improving the coulomb efficiency and rate performance. The electrolyte provided by the present invention can still maintain good performance at high temperature by reasonably proportioning the components and dosages, and largely suppresses the self-discharge phenomenon of the sodium ion capacitor, and improves the electrochemical performance of the sodium ion capacitor.
[0036] The present invention provides a method for preparing an electrolyte with low self-discharge at high temperature as described in the above technical solution, comprising: mixing a mixed organic electrolyte, a carbonate additive and succinic anhydride to obtain an electrolyte.
[0037] In the present invention, the mixing is preferably carried out under the condition of magnetic stirring. The present invention has no special limitation on the time of the mixing, as long as the components in the electrolyte are mixed to homogeneity. In the present invention, the mixing is preferably carried out under the condition of anhydrous and oxygen-free, and more preferably in a glove box filled with argon. The present invention can avoid the electrolyte being contaminated by water and oxygen by controlling the mixing conditions; and can ensure uniform mixing of the raw materials by mixing by magnetic stirring.
[0038] The preparation method provided by the invention is simple, requires low-cost equipment, and is suitable for large-scale industrial promotion.
[0039] The present invention provides the use of the electrolyte with low self-discharge at high temperature described in the above technical solution or the electrolyte with low self-discharge at high temperature prepared by the preparation method described in the above technical solution in a sodium ion capacitor.
[0040] In the present invention, the negative electrode material of the sodium ion capacitor is preferably a niobium-based material, more preferably carbon-coated T-Nb2O5.
[0041] In the present invention, the preparation method of the carbon-coated T-Nb2O5 is preferably:
[0042] (1) Sodium chloride and glucose powder were dissolved in deionized water, stirred for 2 h, and freeze-dried for 24 h to obtain porous powder;
[0043] (2) grinding, sintering, washing and drying the porous powder obtained in step (1) in sequence to obtain nano-flaky carbon powder;
[0044] (3) mixing the nano-flaky carbon powder obtained in step (2) with the ammonium niobate oxalic acid hydrate solution, stirring for 12 hours, and freeze-drying for 24 hours to obtain a mixture;
[0045] (4) Calcining the mixture obtained in step (3) to obtain carbon-coated T-Nb2O5.
[0046] In the present invention, unless otherwise specified, the raw materials used to prepare carbon-coated T-Nb2O5 are all commercially available products well known to those skilled in the art.
[0047] The present invention preferably dissolves sodium chloride and glucose powder in deionized water, fully stirs for 2 hours, and freeze-dries for 24 hours to obtain porous powder. The present invention can prepare organic powder with a porous structure through the above process, which is convenient for the subsequent preparation of porous activated carbon.
[0048] After obtaining the porous powder, the present invention preferably grinds, sinters, washes and dries the porous powder in sequence to obtain nano-flaky carbon powder.
[0049] In the present invention, the grinding agent used in the grinding is preferably ethanol. The present invention has no special limitation on the specific operation of the grinding, which can be determined according to the technical common sense of those skilled in the art.
[0050] In the present invention, the sintering temperature is preferably 750° C., the sintering time is preferably 2 hours, and the sintering atmosphere is preferably an argon atmosphere. The present invention can carbonize the organic components through sintering.
[0051] In the present invention, the cleaning method is preferably cleaning with deionized water. The present invention has no special limitation on the number of cleaning times, which can be determined according to the technical common sense of those skilled in the art as long as the impurities can be removed.
[0052] In the present invention, the drying temperature is preferably 60° C. and the drying time is preferably 12 hours. In the present invention, moisture can be removed by drying.
[0053] After obtaining the nano-flaky carbon powder, the present invention preferably mixes the nano-flaky carbon powder and the ammonium niobate oxalic acid hydrate solution, fully stirs for 12 hours, and freeze-dries for 24 hours to obtain a mixture.
[0054] In the present invention, the stirring temperature is preferably 40-50° C., more preferably 45° C. The present invention can make the nano-flaky carbon powder dispersed uniformly in the solution through the above method.
[0055] After obtaining the mixture, the present invention preferably calcines the mixture to obtain carbon-coated T-Nb2O5.
[0056] In the present invention, the calcination temperature is preferably 800°C; the calcination time is preferably 2 hours; and the calcination atmosphere is preferably an argon atmosphere. The present invention can transform the niobium element into Nb2O5 through calcination, and due to the presence of carbon, carbon-coated T-Nb2O5 is formed.
[0057] In the present invention, the microscopic morphology of the carbon-coated T-Nb2O5 is preferably nanoparticles with a diameter of 50 to 100 nm.
[0058] In the present invention, the carbon-coated T-Nb2O5 negative electrode is preferably supplemented with sodium by an electrochemical pre-sodiumization method; the electrochemical pre-sodiumization is preferably: first assembling the carbon-coated T-Nb2O5 electrode and the sodium metal electrode into a button half-cell, -1 The constant current charge / discharge was performed for 3 cycles at a current density of , and the last cycle was completely discharged to 0.01V, so that Na + The carbon-coated T-Nb2O5 negative electrode was completely embedded, and then the half-cell was disassembled in the glove box to take out the pre-sodiumized carbon-coated T-Nb2O5 negative electrode, and assembled with the activated carbon-sodium nickel iron manganese oxide composite positive electrode into a sodium ion capacitor.
[0059] In the present invention, the carbon matrix in the carbon coating of the carbon-coated T-Nb2O5 negative electrode material provides effective active sites, improves the electronic conductivity of the material, increases the ion / electron transmission efficiency, and thus improves the rate performance of the sodium ion capacitor. In addition, the carbon coating can also prevent electrons from entering the electrolyte and inhibit the occurrence of some side reactions, thereby making the sodium ion capacitor exhibit a lower self-discharge rate.
[0060] In the present invention, the component of the positive electrode material of the sodium ion capacitor is preferably an activated carbon-sodium nickel iron manganate composite material; the mass ratio of activated carbon to sodium nickel iron manganate in the activated carbon-sodium nickel iron manganate composite material is preferably (1-3):1, more preferably 3:1.
[0061] In the present invention, the preparation method of the positive electrode material is preferably:
[0062] 1) mixing activated carbon and sodium nickel iron manganese oxide and then ball milling to obtain an active substance;
[0063] 2) mixing the active material, conductive agent and binder obtained in step 1) to obtain a mixture;
[0064] 3) The mixture obtained in step 2) is mixed with an N-methylpyrrolidone solution, and then coated on an aluminum foil current collector, and finally dried to obtain a positive electrode material.
[0065] In the present invention, unless otherwise specified, the raw materials used to prepare the positive electrode materials are all commercially available products well known to those skilled in the art.
[0066] In the present invention, the activated carbon and sodium nickel iron manganate are preferably mixed and then ball-milled to obtain the active material.
[0067] In the present invention, the activated carbon is preferably commercial activated carbon. The present invention has no particular limitation on the specific sources of the activated carbon and sodium nickel iron manganate, and commercial products well known to those skilled in the art can be used.
[0068] The present invention has no particular limitation on the specific parameters of the ball milling, as long as the activated carbon and sodium nickel iron manganese oxide can be mixed evenly.
[0069] After obtaining the active material, the present invention preferably mixes the active material, the conductive agent and the binder to obtain a mixture
[0070] In the present invention, the conductive agent is preferably acetylene black; the binder is preferably polyvinylidene fluoride; and the mass ratio of the active material, the conductive agent and the binder is preferably 7:2:1.
[0071] The present invention has no particular limitation on the specific operation of mixing the active material, the conductive agent and the binder, as long as the active material, the conductive agent and the binder are mixed uniformly.
[0072] After obtaining the mixture, the present invention preferably mixes the mixture with an N-methylpyrrolidone solution, then coats the mixture on an aluminum foil current collector, and finally dries the mixture to obtain a positive electrode material.
[0073] The present invention has no particular limitation on the specific concentration and dosage of the N-methylpyrrolidone solution, which can be determined according to the technical common sense of those skilled in the art.
[0074] The present invention has no particular limitation on the specific operation of mixing the mixture with the N-methylpyrrolidone solution, as long as the mixture can be fully dispersed in the N-methylpyrrolidone solution.
[0075] The present invention has no particular limitation on the specific operation of coating the aluminum foil current collector, as long as the coating can be uniform.
[0076] In the present invention, the drying temperature is preferably 110°C; the drying time is preferably 12 hours; and the drying is preferably carried out in a vacuum oven. In the present invention, the commercial activated carbon positive electrode has excellent energy density and power density, which ensures that the carbon-coated T-Nb2O5 negative electrode can fully exert its performance, thereby fully exploring its performance and modification effect.
[0077] In the present invention, the prepared activated carbon-sodium nickel iron manganate composite material effectively utilizes the synergistic effect of the two materials, and fully utilizes the advantages of high capacity and low self-discharge rate of sodium nickel iron manganate while maintaining the high specific surface area, high rate performance and high electrochemical stability of the activated carbon.
[0078] In the present invention, by controlling the mass ratio of activated carbon and sodium nickel iron manganate, the excellent rate performance of activated carbon can be retained on the basis of improving the capacity of activated carbon, while the ion diffusion energy barrier of activated carbon can be increased to achieve the effect of inhibiting self-discharge.
[0079] The present invention has no special limitation on the assembly method of the electrolyte, the positive electrode material and the negative electrode material. It is sufficient to adopt an assembly method of a sodium ion capacitor well known to those skilled in the art as long as the sodium ion capacitor can work normally.
[0080] The sodium ion capacitor provided by the present invention is prepared by combining conventional positive electrode materials and negative electrode materials with an improved electrolyte. Not only is the self-discharge behavior significantly suppressed, but the cycle life of the sodium ion capacitor at high temperature is also significantly improved, indicating that the electrolyte provided by the present invention can significantly suppress the self-discharge behavior of the sodium ion capacitor.
[0081] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0082] Example 1
[0083] An electrolyte with low self-discharge at high temperature, comprising: a mixed organic electrolyte, a carbonate additive and succinic anhydride;
[0084] The mixed organic electrolyte solution is composed of ethylene carbonate, dimethyl carbonate and electrolyte sodium salt, wherein the volume ratio of ethylene carbonate to dimethyl carbonate is 1:1; the electrolyte sodium salt is sodium perchlorate, and the concentration of the electrolyte sodium salt in the mixed organic electrolyte solution is 0.5 mol / L;
[0085] The carbonate additive is fluoroethylene carbonate, and the amount of the carbonate additive is 1% of the mass of the mixed organic electrolyte; the amount of succinic anhydride is 3% of the mass of the mixed organic electrolyte;
[0086] The method for preparing the electrolyte with low self-discharge at high temperature comprises the following steps:
[0087] (1) mixing ethylene carbonate, dimethyl carbonate and electrolyte sodium salt in a glove box filled with argon to obtain a mixed organic electrolyte;
[0088] (2) Adding carbonate additives and succinic anhydride to the mixed organic electrolyte obtained in step (1), and then performing magnetic stirring to form a homogeneous liquid to obtain an electrolyte with low self-discharge at high temperature.
[0089] Example 2
[0090] An electrolyte with low self-discharge at high temperature, comprising: a mixed organic electrolyte, a carbonate additive and succinic anhydride;
[0091] The mixed organic electrolyte solution is composed of ethylene carbonate, dimethyl carbonate and electrolyte sodium salt, wherein the volume ratio of ethylene carbonate to dimethyl carbonate is 1:1; the electrolyte sodium salt is sodium perchlorate, and the concentration of the electrolyte sodium salt in the mixed organic electrolyte solution is 0.5 mol / L;
[0092] The carbonate additive is fluoroethylene carbonate, and the amount of the carbonate additive is 3% of the mass of the mixed organic electrolyte; the amount of succinic anhydride is 3% of the mass of the mixed organic electrolyte;
[0093] The preparation method of the electrolyte with low self-discharge at high temperature is the same as that of Example 1.
[0094] Example 3
[0095] An electrolyte with low self-discharge at high temperature, comprising: a mixed organic electrolyte, a carbonate additive and succinic anhydride;
[0096] The mixed organic electrolyte solution is composed of ethylene carbonate, dimethyl carbonate and electrolyte sodium salt, wherein the volume ratio of ethylene carbonate to dimethyl carbonate is 1:1; the electrolyte sodium salt is sodium perchlorate, and the concentration of the electrolyte sodium salt in the mixed organic electrolyte solution is 0.5 mol / L;
[0097] The carbonate additive is fluoroethylene carbonate, and the amount of the carbonate additive is 5% of the mass of the mixed organic electrolyte; the amount of succinic anhydride is 3% of the mass of the mixed organic electrolyte;
[0098] The preparation method of the electrolyte with low self-discharge at high temperature is the same as that of Example 1.
[0099] Example 4
[0100] An electrolyte with low self-discharge at high temperature, comprising: a mixed organic electrolyte, a carbonate additive and succinic anhydride;
[0101] The mixed organic electrolyte solution is composed of ethylene carbonate, dimethyl carbonate and electrolyte sodium salt, wherein the volume ratio of ethylene carbonate to dimethyl carbonate is 1:1; the electrolyte sodium salt is sodium perchlorate, and the concentration of the electrolyte sodium salt in the mixed organic electrolyte solution is 1 mol / L;
[0102] The carbonate additive is fluoroethylene carbonate, and the amount of the carbonate additive is 1% of the mass of the mixed organic electrolyte; the amount of succinic anhydride is 3% of the mass of the mixed organic electrolyte;
[0103] The preparation method of the electrolyte with low self-discharge at high temperature is the same as that of Example 1.
[0104] Example 5
[0105] An electrolyte with low self-discharge at high temperature, comprising: a mixed organic electrolyte, a carbonate additive and succinic anhydride;
[0106] The mixed organic electrolyte solution is composed of ethylene carbonate, dimethyl carbonate and electrolyte sodium salt, wherein the volume ratio of ethylene carbonate to dimethyl carbonate is 1:1; the electrolyte sodium salt is sodium perchlorate, and the concentration of the electrolyte sodium salt in the mixed organic electrolyte solution is 1 mol / L;
[0107] The carbonate additive is fluoroethylene carbonate, and the amount of the carbonate additive is 3% of the mass of the mixed organic electrolyte; the amount of succinic anhydride is 3% of the mass of the mixed organic electrolyte;
[0108] The preparation method of the electrolyte with low self-discharge at high temperature is the same as that of Example 1.
[0109] Example 6
[0110] An electrolyte with low self-discharge at high temperature, comprising: a mixed organic electrolyte, a carbonate additive and succinic anhydride;
[0111] The mixed organic electrolyte solution is composed of ethylene carbonate, dimethyl carbonate and electrolyte sodium salt, wherein the volume ratio of ethylene carbonate to dimethyl carbonate is 1:1; the electrolyte sodium salt is sodium perchlorate, and the concentration of the electrolyte sodium salt in the mixed organic electrolyte solution is 1 mol / L;
[0112] The carbonate additive is fluoroethylene carbonate, and the amount of the carbonate additive is 5% of the mass of the mixed organic electrolyte; the amount of succinic anhydride is 3% of the mass of the mixed organic electrolyte;
[0113] The preparation method of the electrolyte with low self-discharge at high temperature is the same as that of Example 1.
[0114] Example 7
[0115] An electrolyte with low self-discharge at high temperature, comprising: a mixed organic electrolyte, a carbonate additive and succinic anhydride;
[0116] The mixed organic electrolyte solution is composed of ethylene carbonate, dimethyl carbonate and electrolyte sodium salt, wherein the volume ratio of ethylene carbonate to dimethyl carbonate is 1:1; the electrolyte sodium salt is sodium perchlorate, and the concentration of the electrolyte sodium salt in the mixed organic electrolyte solution is 1.5 mol / L;
[0117] The carbonate additive is fluoroethylene carbonate, and the amount of the carbonate additive is 1% of the mass of the mixed organic electrolyte; the amount of succinic anhydride is 3% of the mass of the mixed organic electrolyte;
[0118] The preparation method of the electrolyte with low self-discharge at high temperature is the same as that of Example 1.
[0119] Example 8
[0120] An electrolyte with low self-discharge at high temperature, comprising: a mixed organic electrolyte, a carbonate additive and succinic anhydride;
[0121] The mixed organic electrolyte solution is composed of ethylene carbonate, dimethyl carbonate and electrolyte sodium salt, wherein the volume ratio of ethylene carbonate to dimethyl carbonate is 1:1; the electrolyte sodium salt is sodium perchlorate, and the concentration of the electrolyte sodium salt in the mixed organic electrolyte solution is 1.5 mol / L;
[0122] The carbonate additive is fluoroethylene carbonate, and the amount of the carbonate additive is 3% of the mass of the mixed organic electrolyte; the amount of succinic anhydride is 3% of the mass of the mixed organic electrolyte;
[0123] The preparation method of the electrolyte with low self-discharge at high temperature is the same as that of Example 1.
[0124] Example 9
[0125] An electrolyte with low self-discharge at high temperature, comprising: a mixed organic electrolyte, a carbonate additive and succinic anhydride;
[0126] The mixed organic electrolyte solution is composed of ethylene carbonate, dimethyl carbonate and electrolyte sodium salt, wherein the volume ratio of ethylene carbonate to dimethyl carbonate is 1:1; the electrolyte sodium salt is sodium perchlorate, and the concentration of the electrolyte sodium salt in the mixed organic electrolyte solution is 1.5 mol / L;
[0127] The carbonate additive is fluoroethylene carbonate, and the amount of the carbonate additive is 5% of the mass of the mixed organic electrolyte; the amount of succinic anhydride is 3% of the mass of the mixed organic electrolyte;
[0128] The preparation method of the electrolyte with low self-discharge at high temperature is the same as that of Example 1.
[0129] Comparative Example 1
[0130] An electrolyte solution is prepared by adding sodium perchlorate to a mixed organic electrolyte solution of ethylene carbonate and dimethyl carbonate in a volume ratio of 1:1 in a glove box filled with argon gas, so that the concentration of the sodium perchlorate is 0.5 mol / L, and then magnetic stirring is performed to form a homogeneous liquid, thereby obtaining the electrolyte solution.
[0131] Comparative Example 2
[0132] An electrolyte solution is prepared by adding sodium perchlorate to a mixed organic electrolyte solution of ethylene carbonate and dimethyl carbonate in a volume ratio of 1:1 in a glove box filled with argon gas, so that the concentration of the sodium perchlorate is 1 mol / L, and then magnetic stirring is performed to form a homogeneous liquid, thereby obtaining the electrolyte solution.
[0133] Comparative Example 3
[0134] An electrolyte solution is prepared by adding sodium perchlorate to a mixed organic electrolyte solution of ethylene carbonate and dimethyl carbonate in a volume ratio of 1:1 in a glove box filled with argon gas, so that the concentration of the sodium perchlorate is 1.5 mol / L, and then magnetic stirring is performed to form a homogeneous liquid, thereby obtaining the electrolyte solution.
[0135] Application Example 1
[0136] Using the electrolyte with low self-discharge at high temperature provided in Example 6, an activated carbon-sodium nickel iron manganese oxide composite material (the mass ratio of activated carbon to sodium nickel iron manganese oxide in the activated carbon-sodium nickel iron manganese oxide composite material is 3:1) as the positive electrode, a carbon-coated T-Nb2O5 as the negative electrode, and a glass fiber as the diaphragm, a sodium ion capacitor was assembled in a glove box filled with argon.
[0137] Comparative application example 1
[0138] Using the electrolyte provided in Comparative Example 2, an activated carbon-sodium nickel iron manganese oxide composite material (the mass ratio of activated carbon to sodium nickel iron manganese oxide in the activated carbon-sodium nickel iron manganese oxide composite material is 3:1) as the positive electrode, a carbon-coated T-Nb2O5 as the negative electrode, and a glass fiber as the diaphragm, a sodium ion capacitor was assembled in a glove box filled with argon.
[0139] The performance of the electrolyte with low self-discharge at high temperature prepared in Example 6 was tested. The testing method was as follows: After Application Example 1 was cycled for 3 times at 60°C, a thick amorphous SEI layer was observed on the interface of the carbon-coated T-Nb2O5 negative electrode, such as Figure 1 The amorphous SEI layer derived from fluoroethylene carbonate additives has an inorganic inner layer rich in sodium fluoride and sodium oxide and an ultra-thin amorphous outer layer. This dense inorganic-dominated SEI film can effectively avoid the occurrence of side reactions.
[0140] The rate performance of the electrolytes prepared in Example 6 and Comparative Example 2 at different current densities was tested. The test method was as follows: the rate cycle test was performed on Application Example 1 and Comparative Example 1 at different current densities. The results were as follows: Figure 2 As shown. Figure 2 It can be seen that the rate performance of the electrolyte prepared in Example 6 under various current density conditions is significantly higher than that of Comparative Example 2, and the specific capacity of Example 6 at large and small current densities has been steadily improved, indicating that the electrolyte provided by the present invention can improve the coulombic efficiency of sodium ion capacitors.
[0141] The cycle performance of the electrolytes prepared in Example 6 and Comparative Example 2 at a current density of 1.0 A / g was tested. The results are as follows: Figure 3 As shown. Figure 3 It can be seen that during the 500-cycle cycle, the charge specific capacity of the electrode in the two electrolytes gradually decays in the first 100 cycles, and the specific capacity tends to be stable from the 100th cycle to the 500th cycle, and the coulombic efficiency in the entire cycle is always close to 100%. During the entire cycle, the specific capacity of the electrolyte prepared in Example 6 is significantly higher than that in Comparative Example 2, indicating that the electrolyte provided by the present invention can improve the coulombic efficiency of the sodium ion capacitor.
[0142] The electrochemical properties of the sodium ion capacitors prepared in Example 1 and Comparative Application Example 1 were tested. The test method was as follows: at 60°C, the electrochemical properties of the prepared sodium ion capacitors were tested using a CHI760E electrochemical workstation. The results showed that the cyclic voltammetry curves of the sodium ion capacitors mentioned in Example 1 and Comparative Application Example 1 at different scan rates were as follows: Figure 4 , Figure 5 As shown, Figure 4 The cyclic voltammetry curves of the sodium ion capacitor in Application Example 1 at different scan rates at 60°C; Figure 5 The cyclic voltammetry curves of the sodium ion capacitor in Application Example 1 at different scan rates are compared at 60°C. By comparison, it can be seen that the capacity of Application Example 1 is higher, indicating that the electrolyte provided by the present invention can improve the structural stability of the electrode material of the sodium ion capacitor during the cycle process.
[0143] At 60°C, the self-discharge performance of the sodium ion capacitors prepared in Example 1 and Comparative Application Example 1 was tested, and the obtained self-discharge curves are as follows: Figure 6 As shown. Figure 6 It can be seen that the voltage of Application Example 1 drops from 3.8V to 1.5V, and the self-discharge time takes 48h, while Application Example 1 takes 121h, indicating that the self-discharge behavior of Application Example 1 is significantly suppressed, indicating that the electrolyte provided by the present invention can significantly reduce the self-discharge behavior of the capacitor.
[0144] At 60°C, the self-discharge performance of the sodium ion capacitor prepared according to Example 1 was tested, and the leakage current curve obtained was as follows: Figure 7 As shown. Figure 7 It can be seen that the leakage current of the sodium ion capacitor prepared in Application Example 1 is 0.16 mA, indicating that at a high temperature of 60° C., the self-discharge behavior of the sodium ion capacitor is significantly suppressed, indicating that the electrolyte provided by the present invention is beneficial to improving the cycle life of the sodium ion capacitor.
[0145] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. An electrolyte with low self-discharge at high temperature, comprising a mixed organic electrolyte, a carbonate additive and succinic anhydride; The mixed organic electrolyte comprises ethylene carbonate, dimethyl carbonate and electrolyte sodium salt.
2. The electrolyte with low self-discharge at high temperature according to claim 1, characterized in that: The volume ratio of ethylene carbonate to dimethyl carbonate in the mixed organic electrolyte is 1:(0.5-2).
3. The electrolyte with low self-discharge at high temperature according to claim 1, characterized in that: The electrolyte sodium salt is sodium perchlorate.
4. The electrolyte with low self-discharge at high temperature according to claim 1 or 3, characterized in that: The concentration of the electrolyte sodium salt in the mixed organic electrolyte is 0.5-1.5 mol / L.
5. The electrolyte with low self-discharge at high temperature according to claim 1, characterized in that: The carbonate additive is fluoroethylene carbonate.
6. The electrolyte with low self-discharge at high temperature according to claim 1 or 5, characterized in that: The mass of the carbonate additive is 1-5% of the mass of the mixed organic electrolyte.
7. The electrolyte with low self-discharge at high temperature according to claim 1, characterized in that: The mass of the succinic anhydride is 2-4% of the mass of the mixed organic electrolyte.
8. The method for preparing the electrolyte with low self-discharge at high temperature according to any one of claims 1 to 7, comprising: The mixed organic electrolyte, the carbonate additive and succinic anhydride are mixed to obtain an electrolyte.
9. Use of the electrolyte with low self-discharge at high temperature according to any one of claims 1 to 7 or the electrolyte with low self-discharge at high temperature prepared by the preparation method according to claim 8 in sodium ion capacitors.
10. The use according to claim 9, characterized in that: The negative electrode material of the sodium ion capacitor is a niobium-based material, and the positive electrode material of the sodium ion capacitor is an activated carbon-sodium nickel iron manganese oxide composite material.
Citation Information
Patent Citations
Sodium ion total battery and preparation method thereof
CN114792788A