Alkalinized heterostructure MXene membrane electrode material and preparation method thereof

By forming an alkaline heterostructure on MXene nanosheets, and preparing MXene membrane electrodes by gas-phase hydrothermal method is solved, the problem of easy stacking and oxidation of MXene nanosheets is achieved, high-performance electrochemical performance and structural stability are achieved, and the preparation is simplified. Process and reduce costs.

CN118919315APending Publication Date: 2024-11-08SHANDONG ZHONGSHI YITONG GRP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410886574.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-03
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

When MXene nanosheets are film electrode materials, they are prone to agglomeration and stacking due to high surface energy, which loses excellent physical and chemical properties, and are easily oxidized under the conditions of coexistence of water and oxygen, which limits their performance and application.

Method used

The preparation method of alkalized heterostructure MXene membrane electrode material includes vacuum suction filtering and freeze-drying of MXene nanosheet suspension, soaking in alkali solution, and then performing a gas-phase hydrothermal reaction in ammonium hydroxide aqueous solution to form a uniform Heterogeneous derivatives regulate structure and improve electrochemical properties.

Benefits of technology

The MXene film electrode has uniform morphology, adjustable structure, good conductivity and flexibility, avoid stacking problems, improve electrochemical capacity and structural stability, simplify the preparation process and reduce costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919315A_ABST
    Figure CN118919315A_ABST
Patent Text Reader

Abstract

The invention discloses an alkalized heterostructure MXene membrane electrode material and a preparation method thereof, and belongs to the technical field of electrode material preparation. The preparation method of the alkalized heterostructure MXene membrane electrode material comprises the following steps: carrying out vacuum filtration on an MXene nanosheet suspension, and freeze-drying to obtain an MXene membrane; soaking the MXene membrane in an alkali solution, washing and drying to obtain an alkali-infiltrated MXene membrane; and adding an ammonium hydroxide aqueous solution into a reaction kettle, then horizontally or vertically fixing the alkali-infiltrated MXene membrane right above the liquid level of the ammonium hydroxide aqueous solution, carrying out a gas-phase hydrothermal reaction, and after the reaction is finished, washing and drying to obtain the alkali-infiltrated MXene membrane. The preparation method is simple, easy to operate and low in cost, the prepared alkalized heterostructure MXene membrane electrode material is loose in structure and good in structural stability, the problem of stacking of MXene nanosheets is effectively solved, the alkalized heterostructure MXene membrane electrode material can be directly used as a working electrode of a secondary battery or a supercapacitor, use of a binder is avoided, the conductivity and flexibility are good, and the preparation method is suitable for industrial production. Compared with MXene prepared by a liquid-phase hydrothermal method, the MXene prepared by the method has better electrochemical performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of electrode material preparation, and in particular to an alkalized heterostructure MXene membrane electrode material and a preparation method thereof. Background Art

[0002] The information disclosed in the background of the invention is only intended to enhance the understanding of the overall background of the invention and should not be necessarily regarded as an acknowledgment or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.

[0003] MXene is a two-dimensional layered structure material, which is etched from the MAX phase of ceramic material. It has metal-like conductivity, excellent hydrophilicity, rich surface functional groups and pseudocapacitance. It has attracted widespread attention from researchers in the field of electrochemical energy storage such as secondary batteries, supercapacitors and catalysis.

[0004] However, when MXene is used as a membrane electrode material, due to the high surface energy of MXene nanosheets, it is easy to agglomerate and stack, thus losing the excellent physical and chemical properties of the original nanosheets; in addition, the surface of MXene nanosheets is easily oxidized, especially under the condition of coexistence of water and oxygen, it is easy to oxidize in a short time, and anatase is gradually generated from the edge of the nanosheet to the middle, thus losing the inherent advantages of MXene nanosheets, greatly limiting the performance of MXene nanosheets and their further large-scale application. The existing technology usually chooses to dope MXene with other materials to improve its self-stacking performance, or to use the metastable structure of MXene and use it as an M metal source to derive other materials, but it is often impossible to take into account the structural advantages and composition advantages of MXene itself at the same time, and the addition amount of different materials needs to be carefully controlled to exert the synergistic effect between the materials.

[0005] Therefore, how to provide a method for preparing MXene-based membrane electrode materials with a simple process, while giving full play to the layered structure advantages of MXene materials, and utilizing their composition advantages to derive new high-performance M-based materials, thereby improving the electrochemical properties of MXene-based electrode materials. Summary of the invention

[0006] In view of this, the present invention provides an alkalized heterostructured MXene membrane electrode material and a preparation method thereof. The preparation method provided is simple and can improve the electrochemical performance of the MXene-based electrode while taking advantage of the layered structure of the MXene material.

[0007] In a first aspect, the present invention provides a method for preparing an alkalized heterostructured MXene membrane electrode material, comprising the following steps:

[0008] The MXene nanosheet suspension was vacuum filtered and freeze-dried to obtain a MXene membrane;

[0009] The MXene film is immersed in an alkaline solution, washed and dried to obtain an alkaline-impregnated MXene film;

[0010] An ammonium hydroxide aqueous solution is added to the reactor, and then the alkali-soaked MXene membrane is fixed horizontally or vertically just above the liquid surface of the ammonium hydroxide aqueous solution to carry out a gas-phase hydrothermal reaction. After the reaction is completed, the membrane is washed and dried to obtain the membrane.

[0011] Preferably, the MXene nanosheets are obtained by etching MAX material with a mixed solution of LiF and HCl.

[0012] Preferably, in the alkaline solution, the alkali is selected from sodium hydroxide or potassium hydroxide.

[0013] Preferably, the concentration of the alkaline solution is 3-10 wt %, and the solvent of the alkaline solution is water.

[0014] Preferably, the MXene film is immersed in the alkaline solution for 2 to 6 hours at a temperature of 20 to 40°C.

[0015] Preferably, in the step of obtaining the alkali-impregnated MXene film after washing and drying, the washing solvent is water and ethanol; the drying temperature is 30 to 60° C., and the drying time is 5 to 20 hours.

[0016] Preferably, the concentration of the aqueous ammonium hydroxide solution is 25-28 wt %.

[0017] Preferably, the distance between the bottom of the alkali-infiltrated MXene membrane and the liquid surface of the ammonium hydroxide aqueous solution is 2 to 5 cm.

[0018] Preferably, the temperature of the gas phase hydrothermal reaction is 130-170° C., and the reaction time is 60-80 hours.

[0019] In a second aspect, the present invention provides an alkalized heterostructure MXene membrane electrode material prepared by the above preparation method.

[0020] In a third aspect, the present invention provides an application of the above-mentioned alkalinized heterostructure MXene membrane electrode material in secondary batteries or supercapacitors.

[0021] Compared with the prior art, the present invention has achieved the following beneficial effects:

[0022] (1) The present invention uses alkalization and gas phase hydrothermal method to prepare an alkalized heterostructured MXene membrane electrode material, which has uniform morphology and controllable structure. It can derive heterogeneous derivatives that are evenly dispersed and have good electrochemical properties on the surface of MXene nanosheets. While fully utilizing the good conductivity, flexibility and low ion transport barrier of MXene, the electrochemical capacity of the MXene-based electrode material is fully improved by the heterogeneous derivatives. At the same time, the heterostructured MXene membrane has a large interlayer spacing, a loose structure, and good structural stability, which effectively overcomes the problem of MXene nanosheet stacking; the preparation process is simple, easy to operate, and low cost.

[0023] (2) The alkaline heterostructured MXene membrane electrode material prepared by the present invention can be directly used as the working electrode of a secondary battery or a supercapacitor, avoiding the use of a binder, and has good conductivity and flexibility. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] The drawings constituting part of the present invention are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their description are used to explain the present invention and do not constitute an improper limitation of the present invention. Obviously, for those skilled in the art, other drawings can be obtained based on these drawings without creative work.

[0025] Figure 1 is a surface scanning electron microscope image of the alkalized heterostructure MXene membrane electrode material prepared in Example 1 of the present invention;

[0026] Figure 2 is a surface scanning electron microscope image of the alkalized heterostructured MXene membrane electrode material prepared in Example 2 of the present invention;

[0027] Figure 3 It is a surface scanning electron microscope image of the alkalized heterostructure MXene membrane electrode material prepared in the comparative example of the present invention;

[0028] Figure 4 It is an electrochemical performance image of a sodium ion battery assembled with the alkalinized heterostructure MXene membrane electrode material of Example 1 of the present invention and the MXene membrane electrode material of the comparative example. DETAILED DESCRIPTION

[0029] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.

[0030] The present invention provides a method for preparing an alkalized heterostructured MXene membrane electrode material, comprising the following steps:

[0031] The MXene nanosheet suspension was vacuum filtered and freeze-dried to obtain a MXene membrane;

[0032] The MXene film is immersed in an alkaline solution, washed and dried to obtain an alkaline-impregnated MXene film.

[0033] An ammonium hydroxide aqueous solution is added to the reactor, and then the alkali-soaked MXene membrane is fixed horizontally or vertically above the liquid surface of the ammonium hydroxide aqueous solution to carry out a gas-phase hydrothermal reaction. After the reaction is completed, the membrane is washed and dried to obtain the membrane.

[0034] The present invention first obtains a self-supporting MXene membrane by vacuum filtration, and the strong alkaline environment of the alkaline solution provides the conditions for the formation of titanate; then a gas phase hydrothermal method is used, and the NH3 saturated water vapor in the gas phase of the ammonium hydroxide aqueous solution can adjust the morphology of the titanate, thereby obtaining an alkaline heterostructured MXene membrane electrode material.

[0035] In the present invention, the MXene nanosheets are obtained by etching the MAX material with a mixed solution of LiF and HCl. The present invention does not impose any special restrictions on the specific steps of etching the MAX material with a mixed solution of LiF and HCl, and the etching method commonly used by those skilled in the art can be used. The present invention does not impose any special restrictions on the types of MXene, including but not limited to Ti3C2, Ti3N2, Ti2C, Ti2N, V2N, V2C, Mo2Ti2C3, Mo2TiC2, Nb4C3, etc., which are obtained by etching with corresponding MAX phase materials.

[0036] The present invention does not impose any special restrictions on the process of vacuum filtration, and the method for preparing MXene membranes by vacuum filtration commonly used by those skilled in the art can be used. The pore size of the filter paper in the vacuum filtration process is preferably 0.2 to 0.45 μm. The present invention does not impose any special restrictions on the material of the vacuum filtration filter paper, and the vacuum filter paper material commonly used in the art can be used. The present invention is preferably a mixed cellulose ester microporous filter membrane.

[0037] In the alkaline solution of the present invention, the alkali is selected from one of sodium hydroxide, potassium hydroxide or barium hydroxide. The concentration of the alkaline solution of the present invention is 3-10wt%, more preferably 4-6wt%; the solvent of the alkaline solution is water.

[0038] In the present invention, the MXene film is immersed in the alkaline solution for 2 to 6 hours at a temperature of 20 to 40° C. In the present invention, it is necessary to ensure that the MXene film is completely immersed in the alkaline solution.

[0039] In the present invention, in the step of washing and drying to obtain an alkali-impregnated MXene film, the drying temperature is 30 to 60° C. and the drying time is 5 to 20 hours; the washing is performed by alternately washing with water and ethanol to remove the alkali remaining on the surface of the MXene.

[0040] In the present invention, the concentration of the aqueous ammonium hydroxide solution is 25-28 wt %.

[0041] In the present invention, the distance between the bottom of the alkali-infiltrated MXene film and the liquid surface of the ammonium hydroxide aqueous solution is 2 to 5 cm, more preferably 3 to 4 cm. The appropriate distance can ensure that the alkali-infiltrated MXene film undergoes a hydrothermal reaction in a gas phase environment.

[0042] The present invention does not impose any special restrictions on the method of fixing the alkali-impregnated MXene membrane horizontally or vertically just above the liquid surface of the ammonium hydroxide aqueous solution. For example, a polytetrafluoroethylene clamp can be used to clamp the alkali-impregnated MXene membrane and fix the position of the membrane.

[0043] In the present invention, the temperature of the gas phase hydrothermal reaction is 130-170°C, more preferably 140-160°C, further preferably 145-155°C; the reaction time is 60-80h, more preferably 70-75h, most preferably 72h.

[0044] The present invention also provides an alkalized heterostructure MXene membrane electrode material prepared by the above preparation method.

[0045] The present invention also provides the use of the above-mentioned alkalinized heterostructure MXene membrane electrode material in secondary batteries or supercapacitors.

[0046] The secondary battery of the present invention can be a lithium ion battery, a sodium ion battery or a potassium ion battery, etc., and the alkalinized heterostructured MXene membrane electrode material can be used as the negative electrode of a secondary battery such as a lithium ion battery, a sodium ion battery or a potassium ion battery. The alkalinized heterostructured MXene membrane electrode material provided by the present invention can be directly used as an electrode without the need for a complicated pulping and coating process, while also avoiding the use of a binder, thereby improving the conductivity of the MXene membrane electrode to a certain extent, and having better electrochemical properties than the MXene membrane electrode prepared by a liquid phase hydrothermal method.

[0047] The technical solution of the present invention is further described below in conjunction with specific embodiments.

[0048] In the following examples, Ti3C2T x The preparation method of MXene-based MXene nanosheet suspension is as follows:

[0049] (1) 1 g LiF was mixed with 25 mL 6 M HCl solution in a 100 mL polytetrafluoroethylene (PTFE) beaker and stirred for 40 min at 35 °C.

[0050] (2) adding 1 g of Ti3AlC2 MAX phase powder (powder particle size of 300 mesh) into the beaker of step (1) for etching, with a stirring speed of 250 rpm, a reaction temperature of 35°C, and a reaction time of 48 h;

[0051] (3) After etching, centrifuge washing is performed at a centrifugal speed of 5000 rpm, and deionized water is used to wash until the pH value is neutral;

[0052] (4) High-purity alcohol (99.99%) is used for stripping treatment. After the stripping treatment, the centrifugal speed is 4000 rpm, and the supernatant is collected to obtain a MXene nanosheet suspension.

[0053] Example 1

[0054] This embodiment provides a method for preparing an alkalized heterostructure Ti3C2T by a gas phase hydrothermal method. x Methods for MXene-based membrane electrode materials.

[0055] (1) Mixed cellulose ester microporous membrane (MCE membrane, pore size 0.45 μm) was used to filter Ti3C2T x The base nanosheet suspension is vacuum filtered, and the MXene membrane after vacuum filtration is freeze-dried at a temperature of -80°C for 12 hours to obtain a dried MXene membrane;

[0056] (2) The dried MXene film was placed in a 5 wt% NaOH aqueous solution, alkalized at 30 °C for 4 h, and then dried in an oven at 60 °C for 12 h to obtain an alkali-impregnated MXene film;

[0057] (3) The alkali-impregnated MXene membrane was horizontally clamped with a polytetrafluoroethylene clamp, and the alkali-impregnated MXene membrane was exposed to 3 cm above the liquid surface of a 25 wt % ammonium hydroxide aqueous solution in a polytetrafluoroethylene liner. The polytetrafluoroethylene liner was sealed in a stainless steel high-pressure reactor, and a gas-phase hydrothermal reaction was carried out in an oven at a temperature of 150 ° C for 72 h.

[0058] (4) After the gas phase hydrothermal reaction, the alkali-soaked MXene film was washed three times with deionized water and ethanol alternately, and then dried in vacuum at room temperature to obtain the alkali-treated heterostructure Ti3C2T x MXene membrane electrode materials.

[0059] Figure 1 This is the surface scanning electron microscope image of the alkaline heterostructure MXene membrane electrode material prepared in this example. It can be seen that the Ti3C2T xUniform titanate nanoparticles are derived from the surface of MXene nanosheets. This is because the strong alkaline environment of the alkalization process during the preparation process provides the formation conditions of titanate, and the NH3 saturated water vapor during the gas phase hydrothermal reaction adjusts the morphology of titanate, thereby generating uniform titanate nanoparticles.

[0060] Example 2

[0061] (1) vacuum filtering the MXene nanosheet suspension using a mixed cellulose ester microporous filter membrane (MCE filter membrane, pore size 0.45 μm), freeze-drying the vacuum-filtered MXene membrane at a temperature of -80 ° C for 12 h to obtain a dried MXene membrane;

[0062] (2) The dried MXene film was placed in a 6 wt % KOH aqueous solution, alkalized at 25 ° C for 5 h, and then dried in an oven at 60 ° C for 12 h to obtain an alkali-impregnated MXene film;

[0063] (3) The alkali-impregnated MXene membrane was vertically clamped with a polytetrafluoroethylene clamp, and the alkali-impregnated MXene membrane was exposed 4 cm above the polytetrafluoroethylene liner with a 25 wt% ammonium hydroxide aqueous solution. The polytetrafluoroethylene liner was sealed in a stainless steel high-pressure reactor, and a gas-phase hydrothermal reaction was carried out in an oven at a temperature of 160 °C for 72 h.

[0064] (4) After the gas phase hydrothermal reaction is completed, the alkali-soaked MXene membrane after the reaction is washed three times with deionized water and ethanol alternately, and then vacuum dried at room temperature to obtain the alkaline heterostructure MXene membrane electrode material.

[0065] Figure 2 This is the surface scanning electron microscope image of the alkaline heterostructure MXene membrane electrode material prepared in this example. It can be seen that the Ti3C2T x Uniform titanate nanoparticles are derived from the surface of MXene nanosheets. This is because the strong alkaline environment of the alkalization process during the preparation process provides the conditions for the formation of titanate, and the NH3 saturated water vapor during the gas phase hydrothermal reaction adjusts the titanate morphology, thereby generating uniform titanate nanoparticles.

[0066] Comparative Example

[0067] Compared with Example 1, the difference is that step (3) of this comparative example adopts a liquid phase hydrothermal method. The specific steps of step (3) of this comparative example are as follows:

[0068] The alkali-impregnated MXene membrane was placed in a 25 wt% aqueous solution of ammonium hydroxide in a polytetrafluoroethylene liner, and then placed in a stainless steel high-pressure reactor for a liquid-phase hydrothermal reaction in an oven at a temperature of 150 °C for 72 h.

[0069] Figure 3 The surface scanning electron microscope image of the MXene membrane electrode material prepared in this comparative example shows that no obvious new phase is generated on the surface of the MXene nanosheets.

[0070] Test example

[0071] The alkalinized heterostructured MXene membrane electrode materials of Example 1 and the comparative example are directly used as the negative electrode of the sodium ion battery to assemble the sodium ion battery.

[0072] like Figure 4 As shown, it can be seen that the electrode material prepared by gas phase hydrothermal reaction in Example 1 is applied to the negative electrode of sodium ion battery and exhibits excellent electrochemical performance. At a current density of 1.0A / g, the initial discharge capacity is 161.8mAh / g and there is no obvious capacity decay after 100 cycles. The comparative example is a MXene membrane electrode material prepared by liquid phase hydrothermal reaction as a negative electrode material for sodium ion battery, and its discharge capacity is 34.6mAh / g at a current density of 1.0A / g.

[0073] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing an alkalinized heterostructured MXene membrane electrode material, characterized in that: The steps include: The MXene nanosheet suspension was vacuum filtered and freeze-dried to obtain a MXene membrane; The MXene film is immersed in an alkaline solution, washed and dried to obtain an alkaline-impregnated MXene film; An ammonium hydroxide aqueous solution is added to the reactor, and then the alkali-soaked MXene membrane is fixed horizontally or vertically just above the liquid surface of the ammonium hydroxide aqueous solution to carry out a gas-phase hydrothermal reaction. After the reaction is completed, the membrane is washed and dried to obtain the membrane.

2. The preparation method according to claim 1, characterized in that The MXene nanosheets are obtained by etching MAX material with a mixed solution of LiF and HCl.

3. The preparation method according to claim 1, characterized in that: In the alkaline solution, the alkali is selected from sodium hydroxide or potassium hydroxide; the concentration of the alkaline solution is 3-10wt%, and the solvent of the alkaline solution is water.

4. The preparation method according to claim 1, characterized in that: The MXene film is immersed in the alkaline solution for 2 to 6 hours at a temperature of 20 to 40°C.

5. The preparation method according to claim 1, characterized in that: In the step of obtaining the alkali-impregnated MXene film after washing and drying, the washing solvent is water and ethanol; the drying temperature is 30 to 60° C., and the drying time is 5 to 20 hours.

6. The preparation method according to claim 1, characterized in that: The concentration of the aqueous ammonium hydroxide solution is 25-28 wt %.

7. The preparation method according to claim 1, characterized in that: The distance between the bottom of the alkali-soaked MXene membrane and the liquid surface of the ammonium hydroxide aqueous solution is 2 to 5 cm.

8. The preparation method according to claim 1, characterized in that: The temperature of the gas phase hydrothermal reaction is 130-170° C., and the reaction time is 60-80 hours.

9. An alkalized heterostructured MXene membrane electrode material prepared by the preparation method according to any one of claims 1 to 8.

10. Use of the alkalinized heterostructured MXene membrane electrode material as claimed in claim 9 in secondary batteries or supercapacitors.