Formation method of semiconductor structure and semiconductor structure
By using argon ion beam etching in the deposition machine to remove carbon on the metal silicide layer on the back of the silicon carbide wafer and form a back metal layer in the same machine, the peeling problem caused by carbon precipitation is solved, the process is simplified and the process is reduced. Manufacturing cost.
Patent Information
- Application Number
- CN202411002819.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-08
AI Technical Summary
In the IGBT platform process, carbon precipitates and remains on the metal silicide surface during laser annealing of the silicon carbide material substrate, resulting in subsequent metal layer peeling problems on the back. The existing process requires carbon removal through the ashing machine, adding process steps and manufacturing costs.
Through an etching process, especially argon ion beam etching, the carbon on the surface of the metal silicide layer is removed, and the back metal layer is formed in the same machine to simplify the process flow.
No additional ashing steps are required to remove carbon, simplify the manufacturing process of semiconductor structures, reduce manufacturing costs, and improve manufacturing efficiency, avoiding the problem of peeling off the metal layer on the back.
Smart Images

Figure CN118919400A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of integrated circuit manufacturing, and in particular to a method for forming a semiconductor structure and a semiconductor structure. Background Art
[0002] In the manufacturing process of semiconductor structures such as IGBT (Insulate-Gate Bipolar Transistor) platform process, after the substrate is thinned, it is necessary to deposit a metal material on the back of the substrate to improve the ohmic contact performance of the back of the substrate. In the process of improving the ohmic contact performance of the back of the substrate, it is necessary to deposit a metal material on the back of the substrate, and perform laser annealing on the substrate so that the deposited metal material reacts with the substrate to form a metal silicide. However, in the substrate formed by silicon carbide material, carbon will precipitate from the substrate during the laser annealing process and remain on the surface of the metal silicide. The precipitated carbon needs to be removed from the surface of the metal silicide to avoid peeling problems of the back metal layer formed on the surface of the metal silicide later. Currently, the substrate after the metal silicide is formed is transferred to an ashing machine, and the carbon precipitated on the surface of the metal silicide is removed by an ashing process. After that, the substrate after the ashing process is transferred to a deposition machine to form a back metal layer covering the metal silicide on the substrate. However, since the added ashing process needs to be completed in an ashing machine, not only the steps of the semiconductor structure manufacturing process are increased, but also the manufacturing cost of the semiconductor structure is increased, which is not conducive to improving the manufacturing efficiency of the semiconductor structure.
[0003] Therefore, how to simplify the manufacturing process of the semiconductor structure, reduce the manufacturing cost of the semiconductor structure, and improve the manufacturing efficiency of the semiconductor structure is a technical problem that needs to be solved urgently. Summary of the invention
[0004] The present invention provides a method for forming a semiconductor structure and a semiconductor structure, which are used to simplify the manufacturing process of the semiconductor structure, reduce the manufacturing cost of the semiconductor structure, and improve the manufacturing efficiency of the semiconductor structure.
[0005] According to some embodiments, the present invention provides a method for forming a semiconductor structure, comprising the following steps:
[0006] Providing a silicon carbide wafer, wherein the silicon carbide wafer comprises a front side and a back side that are relatively distributed;
[0007] Forming a metal silicide layer on the back side of the silicon carbide wafer, and precipitating carbon from the silicon carbide wafer to the surface of the metal silicide layer;
[0008] Removing carbon on the surface of the metal silicide layer by an etching process in a deposition machine;
[0009] A back metal layer covering the surface of the metal silicide layer is formed in the deposition machine.
[0010] In some embodiments, a metal silicide layer is formed on the back side of the silicon carbide wafer, and carbon is precipitated from the silicon carbide wafer to the surface of the metal silicide layer. The specific steps include:
[0011] Depositing a first metal material onto the back side of the silicon carbide wafer;
[0012] The silicon carbide wafer is annealed, the first metal material reacts with the silicon carbide wafer to form the metal silicide layer, and the silicon carbide wafer precipitates carbon on the surface of the metal silicide layer.
[0013] In some embodiments, before removing the carbon on the surface of the metal silicide layer by an etching process in a deposition machine, the method further includes the following steps:
[0014] The back side of the silicon carbide wafer is cleaned by a wet cleaning process.
[0015] In some embodiments, the deposition machine is a physical vapor deposition machine, and the physical vapor deposition machine includes a soft etching chamber; the specific steps of removing carbon on the surface of the metal silicide layer by an etching process in the deposition machine include:
[0016] The carbon on the surface of the metal silicide layer is removed by an etching process in the soft etching chamber of the physical vapor deposition machine.
[0017] In some embodiments, the specific steps of removing carbon on the surface of the metal silicide layer by an etching process in the soft etching chamber of the physical vapor deposition machine include:
[0018] The surface of the metal silicide layer is etched by using an argon ion beam in the soft etching chamber to remove carbon on the surface of the metal silicide layer.
[0019] In some embodiments, the specific steps of etching the surface of the metal silicide layer using an argon ion beam in the soft etching chamber include:
[0020] Argon gas of a preset flow rate is transmitted to the soft etching chamber, and the RF power in the soft etching chamber is adjusted to 500 watts to 700 watts, and the temperature in the soft etching chamber is adjusted to 200° C. to 400° C., wherein the preset flow rate is 13 ml / min to 23 ml / min.
[0021] In some embodiments, the specific steps of removing carbon on the surface of the metal silicide layer by an etching process in the soft etching chamber of the physical vapor deposition machine include:
[0022] The etching parameters in the soft etching chamber are adjusted so that the etching rate of carbon on the surface of the metal silicide layer is 0.5 nm / s to 0.7 nm / s.
[0023] In some embodiments, the time for etching carbon on the surface of the metal silicide layer in the soft etching chamber of the physical vapor deposition machine is 10 seconds to 20 seconds.
[0024] In some embodiments, the physical deposition machine further comprises a physical vapor deposition chamber; the specific steps of forming a back metal layer covering the surface of the metal silicide layer in the deposition machine include:
[0025] transferring the silicon carbide wafer to the physical vapor deposition chamber;
[0026] A back metal layer covering the surface of the metal silicide layer is formed in the physical vapor deposition chamber by a physical vapor deposition process.
[0027] According to some other embodiments, the present invention further provides a semiconductor structure formed by the method for forming a semiconductor structure as described above; the semiconductor structure comprises:
[0028] A silicon carbide wafer, wherein the silicon carbide wafer comprises a front side and a back side that are relatively distributed;
[0029] a metal silicide layer, located on the back side of the silicon carbide wafer;
[0030] A back metal layer covers the surface of the metal silicide layer facing away from the silicon carbide wafer.
[0031] The semiconductor structure formation method and semiconductor structure provided by the present invention, after forming a metal silicide layer on the back side of a silicon carbide wafer, the process of removing the carbon precipitated on the surface of the metal silicide layer and the process of forming the back metal layer on the surface of the metal silicide layer are implemented in the same deposition machine, without the need for an additional ashing step to remove the precipitated carbon on the surface of the metal silicide layer, thereby simplifying the semiconductor structure formation process and improving the manufacturing efficiency of the semiconductor structure. Moreover, the process of removing the carbon precipitated on the surface of the metal silicide layer and the process of forming the back metal layer on the surface of the metal silicide layer are implemented in the same deposition machine, without the need for an additional ashing machine, thereby reducing the manufacturing cost of the semiconductor structure. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1is a flow chart of a method for forming a semiconductor structure in a specific embodiment of the present invention;
[0033] Figure 2 is a schematic structural diagram of a silicon carbide wafer in a specific embodiment of the present invention;
[0034] Figure 3 is a schematic diagram of the structure after a metal silicide layer is formed on the back side of a silicon carbide wafer in a specific embodiment of the present invention;
[0035] Figure 4 is a schematic diagram of the structure after removing carbon precipitated on the surface of the metal silicide layer according to a specific embodiment of the present invention;
[0036] Figure 5 It is a schematic diagram of the structure after a back metal layer is formed on the surface of the metal silicide layer in a specific embodiment of the present invention. DETAILED DESCRIPTION
[0037] The method for forming a semiconductor structure and a specific implementation of the semiconductor structure provided by the present invention are described in detail below with reference to the accompanying drawings.
[0038] This specific embodiment provides a method for forming a semiconductor structure. Figure 1 1 is a flow chart of a method for forming a semiconductor structure in a specific embodiment of the present invention. Figure 1 As shown, the method for forming the semiconductor structure comprises the following steps:
[0039] Step S11, providing a silicon carbide wafer, wherein the silicon carbide wafer comprises a front side and a back side that are relatively distributed;
[0040] Step S12, forming a metal silicide layer on the back side of the silicon carbide wafer, and precipitating carbon from the silicon carbide wafer to the surface of the metal silicide layer;
[0041] Step S13, removing carbon on the surface of the metal silicide layer by an etching process in a deposition machine;
[0042] Step S14, forming a back metal layer covering the surface of the metal silicide layer in the deposition machine.
[0043] Figure 2 is a schematic diagram of the structure of a silicon carbide wafer in a specific embodiment of the present invention, Figure 3 is a schematic diagram of the structure after a metal silicide layer is formed on the back side of a silicon carbide wafer in a specific embodiment of the present invention. Figure 2 and Figure 3 As shown, the metal silicide layer 30 is formed on the back side 202 of the silicon carbide wafer 20, and the specific steps of precipitating carbon from the silicon carbide wafer 20 to the surface of the metal silicide layer 30 include:
[0044] Depositing a first metal material onto the back side 202 of the silicon carbide wafer 20;
[0045] The silicon carbide wafer 20 is annealed, and the first metal material reacts with the silicon carbide wafer 20 to form the metal silicide layer 30 , and the silicon carbide wafer 20 precipitates carbon on the surface of the metal silicide layer 30 .
[0046] Specifically, silicon carbide materials have the advantages of stable chemical properties, high thermal conductivity, small thermal expansion coefficient, and good wear resistance. Therefore, silicon carbide wafers formed by silicon carbide materials can significantly improve the physical and chemical properties of semiconductor structures. Figure 2 As shown, the silicon carbide wafer 20 includes the front side 201 and the back side 202 opposite to the front side 201. After the device structure is formed on the front side 201 of the silicon carbide wafer 20, the back side thinning treatment is performed on the silicon carbide wafer 20 to reduce the thickness of the silicon carbide wafer 20. In order to improve the ohmic contact performance of the back side 202 of the silicon carbide wafer 20, after the back side thinning treatment is performed on the silicon carbide wafer 20, a first metal material such as Ti or Ni is deposited on the back side 202 of the silicon carbide wafer 20, and the back side 202 of the silicon carbide wafer 20 is laser annealed so that the first metal material reacts with the silicon carbide wafer 20 to form the metal silicide layer 30. During the laser annealing treatment, the carbon in the silicon carbide wafer 20 will precipitate onto the surface of the metal silicide layer 30 to form a precipitated carbon layer 31 covering the surface of the metal silicide layer 30, as shown in FIG. Figure 3 After the laser annealing process is completed, the precipitated carbon layer 31 remains on the surface of the metal silicide layer 30 .
[0047] Figure 4 1 is a schematic diagram of the structure after removing the carbon precipitated on the surface of the metal silicide layer according to a specific embodiment of the present invention. In some embodiments, before removing the carbon on the surface of the metal silicide layer 30 by an etching process in a deposition machine, the following steps are also included:
[0048] The back side 202 of the silicon carbide wafer 20 is cleaned by a wet cleaning process.
[0049] Specifically, before removing the precipitated carbon on the surface of the metal silicide layer 30, a wet cleaning process is used to clean the back side 202 of the silicon carbide wafer 20 to remove the unreacted first metal material and some impurities generated during the reaction process, so as to improve the cleanliness of the back side 202 of the silicon carbide wafer 20. However, since the precipitated carbon has a strong adhesion to the metal silicide layer 30, it is difficult to remove it by a wet cleaning process.
[0050] In some embodiments, the deposition machine is a physical vapor deposition machine, and the physical vapor deposition machine includes a soft etching chamber; the specific steps of removing carbon on the surface of the metal silicide layer 30 by an etching process in the deposition machine include:
[0051] In the soft etching chamber of the physical vapor deposition machine, the carbon on the surface of the metal silicide layer 30 is removed by an etching process, such as Figure 4 shown.
[0052] Specifically, since the physical vapor deposition machine is equipped with both a soft etching chamber and a physical vapor deposition chamber, the precipitated carbon layer 31 on the surface of the metal silicide 30 is removed by implementing a dry etching process in the soft etching chamber in the physical vapor deposition machine, and the back metal layer is formed by the physical vapor deposition chamber in the same physical vapor deposition machine, so that the process of removing the precipitated carbon layer 31 and the process of forming the back metal layer are completed in the same machine, without the need to set up an additional ashing machine, and without the need to transfer the silicon carbide wafer between different machines (such as an ashing machine and a back metal layer deposition machine), and the problem of easy contamination of the silicon carbide wafer when transferring the silicon carbide wafer between different machines is avoided, which not only simplifies the manufacturing process of the semiconductor structure, improves the manufacturing efficiency of the semiconductor structure, but also reduces the manufacturing cost of the semiconductor structure.
[0053] In some embodiments, the specific steps of removing carbon on the surface of the metal silicide layer 30 by etching in the soft etching chamber of the physical vapor deposition machine include:
[0054] The surface of the metal silicide layer 30 is etched by using an argon ion beam in the soft etching chamber to remove carbon on the surface of the metal silicide layer 30 .
[0055] In some embodiments, the specific steps of etching the surface of the metal silicide layer 30 using an argon ion beam in the soft etching chamber include:
[0056] Argon gas of a preset flow rate is transmitted to the soft etching chamber, and the RF power in the soft etching chamber is adjusted to 500 watts to 700 watts, and the temperature in the soft etching chamber is adjusted to 200° C. to 400° C., wherein the preset flow rate is 13 ml / min to 23 ml / min.
[0057] Specifically, since the carbon precipitated from the silicon carbide wafer 20 is located on the entire surface of the metal silicide layer 30, that is, the precipitated carbon layer 31 covers the entire surface of the metal silicide layer 30 away from the silicon carbide wafer 20, an argon ion beam can be used to bombard the entire surface of the metal silicide layer 30 in the soft etching chamber to fully remove the precipitated carbon layer 31. When etching the deposited carbon layer 31, argon gas with a purity of 6N (99.9999%) can be transmitted to the soft etching chamber, and the flow rate of the argon gas is 13 ml / min to 23 ml / min (for example, 18 ml / min), the RF power in the soft etching chamber is adjusted to 500 watts to 700 watts (for example, 600 watts), and the temperature in the soft etching chamber is adjusted to 200°C to 400°C (for example, 300°C), so as to ensure that while further removing the deposited carbon layer 31, damage to the metal silicide layer 30 and the silicon carbide wafer 20 is avoided.
[0058] In some embodiments, the specific steps of removing carbon on the surface of the metal silicide layer 30 by etching in the soft etching chamber of the physical vapor deposition machine include:
[0059] The etching parameters in the soft etching chamber are adjusted so that the etching rate of carbon on the surface of the metal silicide layer 30 is 0.5 nm / s to 0.7 nm / s.
[0060] In one example, the etching rate of the precipitated carbon layer 31 on the surface of the metal silicide layer 30 is 0.6 nanometers per second. In this specific embodiment, the etching rate of the precipitated carbon layer 31 on the surface of the metal silicide layer 30 is controlled within the range of 0.5 nanometers per second to 0.7 nanometers per second, thereby avoiding the problem that the precipitated carbon layer 31 cannot be fully removed due to the etching rate being too slow, and avoiding damage to the metal silicide layer 30 and the silicon carbide wafer 20 due to the etching rate being too fast. The etching parameters include any one of etching temperature, etching pressure, radio frequency power, and argon gas flow rate, or a combination of two or more thereof.
[0061] In some embodiments, the time for etching carbon on the surface of the metal silicide layer 30 in the soft etching chamber of the physical vapor deposition machine is 10 seconds to 20 seconds.
[0062] In one example, the time for etching the carbon on the surface of the metal silicide layer 30 in the soft etching chamber in the physical vapor deposition machine is 15 seconds. In this specific embodiment, the time for etching the carbon on the surface of the metal silicide layer 30 in the soft etching chamber is controlled within 10 seconds to 20 seconds, so that the precipitated carbon layer 31 on the surface of the metal silicide layer 30 can be fully removed and damage to the metal silicide layer 30 and the silicon carbide wafer 20 can be avoided.
[0063] Figure 5 is a schematic diagram of the structure after a back metal layer is formed on the surface of the metal silicide layer in a specific embodiment of the present invention. Figure 5 As shown, the physical deposition machine further includes a physical vapor deposition chamber; the specific steps of forming the back metal layer 50 covering the surface of the metal silicide layer 30 in the deposition machine include:
[0064] Transferring the silicon carbide wafer 20 to the physical vapor deposition chamber;
[0065] A back metal layer 50 covering the surface of the metal silicide layer 30 is formed in the physical vapor deposition chamber by a physical vapor deposition process.
[0066] This specific embodiment adjusts the etching rate and etching time of the deposited carbon layer 31 so that the removal rate (i.e., removal effect) of the deposited carbon layer 31 in the soft etching chamber is greater than or equal to the removal rate of the deposited carbon layer 31 through the ashing process, thereby not only reducing the residual deposited carbon on the surface of the metal silicide layer 30, but also avoiding the problem of peeling of the back metal layer 50 which is easily caused by the residual deposited carbon.
[0067] This specific embodiment also provides a semiconductor structure, which is formed by the semiconductor structure forming method as described above. Figure 1-Figure 5 The schematic diagram of the semiconductor structure provided in this specific embodiment can be found in Figure 5 .like Figure 2-Figure 5 As shown, the semiconductor structure comprises:
[0068] A silicon carbide wafer 20, wherein the silicon carbide wafer 20 comprises a front side 201 and a back side 202 which are relatively distributed;
[0069] A metal silicide layer 30 , located on the back side 202 of the silicon carbide wafer 20 ;
[0070] The back metal layer 50 covers the surface of the metal silicide layer 30 facing away from the silicon carbide wafer 20 .
[0071] The method for forming a semiconductor structure and the semiconductor structure provided in this specific embodiment, after forming a metal silicide layer on the back side of a silicon carbide wafer, the process for removing the carbon precipitated on the surface of the metal silicide layer and the process for forming a back metal layer on the surface of the metal silicide layer are implemented in the same deposition machine, without the need for an additional ashing step to remove the precipitated carbon on the surface of the metal silicide layer, thereby simplifying the process for forming the semiconductor structure and improving the manufacturing efficiency of the semiconductor structure. Moreover, the process for removing the carbon precipitated on the surface of the metal silicide layer and the process for forming a back metal layer on the surface of the metal silicide layer are implemented in the same deposition machine, without the need for an additional ashing machine, thereby reducing the manufacturing cost of the semiconductor structure.
[0072] The above is only a preferred embodiment of the present invention. It should be pointed out that ordinary technicians in this technical field can make several improvements and modifications without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for forming a semiconductor structure, It is characterized in that The steps include: Providing a silicon carbide wafer, wherein the silicon carbide wafer comprises a front side and a back side that are relatively distributed; Forming a metal silicide layer on the back side of the silicon carbide wafer, and precipitating carbon from the silicon carbide wafer to the surface of the metal silicide layer; Removing carbon on the surface of the metal silicide layer by an etching process in a deposition machine; A back metal layer covering the surface of the metal silicide layer is formed in the deposition machine.
2. The method for forming a semiconductor structure according to claim 1, It is characterized in that The specific steps of forming a metal silicide layer on the back side of the silicon carbide wafer and precipitating carbon from the silicon carbide wafer to the surface of the metal silicide layer include: Depositing a first metal material onto the back side of the silicon carbide wafer; The silicon carbide wafer is annealed, the first metal material reacts with the silicon carbide wafer to form the metal silicide layer, and the silicon carbide wafer precipitates carbon on the surface of the metal silicide layer.
3. The method for forming a semiconductor structure according to claim 1, It is characterized in that Before removing the carbon on the surface of the metal silicide layer by an etching process in a deposition machine, the method further includes the following steps: The back side of the silicon carbide wafer is cleaned by a wet cleaning process.
4. The method for forming a semiconductor structure according to claim 1, It is characterized in that The deposition machine is a physical vapor deposition machine, and the physical vapor deposition machine includes a soft etching chamber; The specific step of removing the carbon on the surface of the metal silicide layer by an etching process in the deposition machine includes: removing the carbon on the surface of the metal silicide layer by an etching process in the soft etching chamber in the physical vapor deposition machine.
5. The method for forming a semiconductor structure according to claim 4, It is characterized in that The specific steps of removing carbon on the surface of the metal silicide layer by an etching process in the soft etching chamber in the physical vapor deposition machine include: The surface of the metal silicide layer is etched by using an argon ion beam in the soft etching chamber to remove carbon on the surface of the metal silicide layer.
6. The method for forming a semiconductor structure according to claim 5, It is characterized in that The specific steps of etching the surface of the metal silicide layer by using an argon ion beam in the soft etching chamber include: Argon gas of a preset flow rate is transmitted to the soft etching chamber, and the RF power in the soft etching chamber is adjusted to 500 watts to 700 watts, and the temperature in the soft etching chamber is adjusted to 200° C. to 400° C., wherein the preset flow rate is 13 ml / min to 23 ml / min.
7. The method for forming a semiconductor structure according to claim 4, It is characterized in that The specific steps of removing carbon on the surface of the metal silicide layer by an etching process in the soft etching chamber in the physical vapor deposition machine include: The etching parameters in the soft etching chamber are adjusted so that the etching rate of carbon on the surface of the metal silicide layer is 0.5 nm / s to 0.7 nm / s.
8. The method for forming a semiconductor structure according to claim 4, It is characterized in that The time for etching carbon on the surface of the metal silicide layer in the soft etching chamber in the physical vapor deposition machine is 10 seconds to 20 seconds.
9. The method for forming a semiconductor structure according to claim 4, It is characterized in that The physical deposition machine further includes a physical vapor deposition chamber; the specific steps of forming a back metal layer covering the surface of the metal silicide layer in the deposition machine include: transferring the silicon carbide wafer to the physical vapor deposition chamber; A back metal layer covering the surface of the metal silicide layer is formed in the physical vapor deposition chamber by a physical vapor deposition process.
10. A semiconductor structure, It is characterized in that The semiconductor structure is formed by the method for forming a semiconductor structure according to claim 1; the semiconductor structure comprises: A silicon carbide wafer, wherein the silicon carbide wafer comprises a front side and a back side that are relatively distributed; a metal silicide layer, located on the back side of the silicon carbide wafer; A back metal layer covers the surface of the metal silicide layer facing away from the silicon carbide wafer.