Composite substrate with element-doped diamond modified layer and semiconductor device
By forming overlapping tensile and compressive stress buffer layers on the surface of the diamond substrate, element doping technology is used to alleviate the thermal stress mismatch problem between diamond and other semiconductor materials, improve bonding strength and stability, and solve the existing technology The problem of high thermal stress in the middle bonding interface.
Patent Information
- Application Number
- CN202410967734.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-08
AI Technical Summary
The bonding interface caused by the mismatch between diamond and other semiconductor materials at high temperatures caused by the mismatch of the crystal lattice and thermal expansion coefficient, resulting in the problems of low bonding strength and low yield.
The overlapping tensile stress buffer layer and compressive stress buffer layer are formed on the surface of the diamond substrate. Elements with lattice constants greater than or less than diamond are injected through element doping technology to form a gradient stress distribution to alleviate the problem of thermal stress mismatch, replacing traditional micro Structural design.
It significantly improves the interface stability and bonding strength between diamond and other semiconductor materials, and improves bonding quality and yield.
Smart Images

Figure CN118919404A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of semiconductor material composite substrate manufacturing, and in particular relates to a composite substrate with an element-doped diamond modified layer and a semiconductor device. Background Art
[0002] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention, and should not necessarily be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.
[0003] Heterogeneous heterogeneous integration is an inevitable trend in the development of integrated circuit technology in the post-Moore era. This technology can achieve smaller process scales, higher device integration density, and more functional integration to meet the higher requirements of future integrated circuit systems. As one of the key technologies of heterogeneous integration technology, heterogeneous wafer bonding technology has become the preferred technology for heterogeneous integration due to the high quality and easy processing of integrated devices. It is widely used in advanced packaging, efficient thermal management, new photonic platforms, and optoelectronic integration.
[0004] Diamond film has the advantages of high thermal conductivity, strong chemical stability, high carrier mobility and high carrier saturation concentration. Therefore, it is expected to obtain the production and application of diamond film in high-temperature, high-frequency and high-power semiconductor devices, especially in the field of heat dissipation. Diamond is one of the materials with the highest thermal conductivity among known semiconductor materials. Its thermal conductivity is as high as 2200W / m·K, which is 4 times that of SiC material and 13 times that of Si material. These characteristics make diamond a heat dissipation substrate. On the one hand, it can reduce the thermal resistance of semiconductor devices, thereby greatly improving the operating power of precision instruments and avoiding damage to various electronic devices caused by heat accumulation; on the other hand, it can also manufacture semiconductor power devices with higher power density under the same size.
[0005] However, there is a large lattice mismatch and thermal expansion coefficient mismatch between diamond and other semiconductor materials, which causes great thermal stress to be generated at the bonding interface during high-temperature annealing and cooling. The bonding interface cannot resist the thermal expansion stress, which may lead to the collapse of the high-temperature bonding layer. Etching the bonding surface of the wafer to form a microstructure is the mainstream method to solve this problem. It can effectively release the thermal stress generated during the annealing process to provide space margin and reduce the adverse effects of the thermal stress generated in the composite structure during the annealing process. However, the microstructure design will reduce the effective bonding area and thus affect the bonding strength. In addition, when the diamond wafer is directly bonded to semiconductors such as Si, SiC and GaN, a large pressure needs to be applied. The presence of the microstructure will make it difficult to effectively control the force uniformity of the bonded wafer, resulting in the sample being easy to break during the bonding process and a low yield rate.
[0006] Therefore, in order to address the pain points and difficulties in the heterogeneous wafer bonding process, it is of great significance to provide a high thermal conductivity diamond modified layer that can effectively buffer the thermal mismatch problem of heterogeneous materials in bonding to improve the bonding quality and have a highly flat substrate to improve the bonding strength by improving the structural design and production process of the bonding sheet. Summary of the invention
[0007] In order to address the deficiencies of the prior art, the purpose of the present invention is to provide a composite substrate and a semiconductor device having an element-doped diamond modified layer. The composite substrate provided by the present invention forms overlapping tensile stress buffer layers and compressive stress buffer layers on the surface of the diamond substrate, thereby replacing the structural design and alleviating the thermal stress matching problem generated at the bonding interface through element doping.
[0008] In order to achieve the above object, the technical solution of the present invention is:
[0009] A first aspect of the present invention provides a method for preparing a composite substrate having an element-doped diamond modified layer, comprising the following steps:
[0010] A first ion implantation region and a non-ion implantation region are formed on the surface of the diamond substrate by using photolithography technology; a plurality of non-ion implantation regions are arranged at intervals, and a first ion implantation region is arranged between two adjacent non-ion implantation regions;
[0011] Implanting element ions having a lattice constant greater than that of diamond into the first ion implantation region to form an element-doped diamond modified layer;
[0012] High temperature activation of element-doped diamond modified layer;
[0013] The element-doped diamond modified layer activated at high temperature is processed to obtain a composite substrate having the element-doped diamond modified layer.
[0014] The present invention forms a tensile stress buffer layer on the surface of the diamond substrate by injecting an element with a lattice constant greater than that of diamond. Due to the large difference in lattice constants, a compressive stress buffer layer is formed in the non-ion implanted area, thereby forming an overlapping tensile stress buffer layer and a compressive stress buffer layer, thereby replacing the structural design and alleviating the thermal stress matching problem generated by the bonding interface through element doping. The principle of the tensile stress buffer layer is to generate tensile stress in a local area of the diamond surface by injecting an element with a lattice constant greater than that of diamond. This tensile stress can effectively absorb and disperse the thermal stress caused by lattice mismatch under high temperature conditions, thereby reducing the destructive effect of thermal stress on the bonding interface. The principle of the compressive stress buffer layer is to introduce compressive stress on the diamond surface by injecting an element with a lattice constant less than that of diamond. This compressive stress can partially offset the stress concentration phenomenon caused by thermal expansion at high temperature, thereby further balancing the thermal stress at the interface. By alternately injecting elements with different lattice constants, a periodic structure of tensile stress and compressive stress buffer layers is formed, and a gradient stress distribution can be effectively formed. This gradient stress distribution makes the stress at the bonding interface more evenly distributed, thereby significantly improving the interface stability and bonding strength between diamond and other semiconductor materials at high temperatures.
[0015] In some embodiments of the present invention, the shape of the first ion implantation area includes but is not limited to strip, ring, grid or radial. The shape of the first ion implantation area of the present invention is the shape of the first ion implantation area in its top view, and the width and spacing of the first ion implantation areas of different shapes need to be determined according to the actual situation and specific target effect.
[0016] In the present invention, a plurality of non-ion implantation regions are arranged at intervals, and a first ion implantation region is arranged between two adjacent non-ion implantation regions, which can avoid heating of the ion implantation regions, reduce the aggregation of heating regions, and increase the power capacity of the resistor.
[0017] In some embodiments of the present invention, the photolithography technology is a conventional photolithography technology, for example, it may include the following:
[0018] S1. Thoroughly clean the diamond substrate to ensure that the surface is free of contamination, and coat the surface with a mask material to form a mask layer;
[0019] S2, using a mask having a geometric pattern to accurately expose the mask layer;
[0020] S3, etching the mask to expose the first ion implantation area for element ion implantation, and the unetched portion is the non-ion implantation area.
[0021] Preferably, the mask material includes but is not limited to photoresist, metal film, oxide film, etc. When the mask material is photoresist, the photoresist can be positive or negative, and the method of preparing the photoresist coating includes but is not limited to spraying, spin coating or inkjet printing.
[0022] Preferably, the geometric pattern on the mask includes but is not limited to a stripe pattern, a concentric circle pattern, a grid pattern or a radial pattern, and the pattern width and spacing need to be determined according to the actual situation and the specific target effect. It can be understood that the geometric pattern on the mask is the same as the shape of the first ion implantation area.
[0023] Preferably, the precise exposure, exposure technology includes but is not limited to holographic exposure, optical exposure, ion beam exposure or electron beam exposure technology. Preferably, the mask layer after exposure is developed, and the development technology includes but is not limited to positive photoresist development, negative photoresist development, wet development or dry development.
[0024] In some embodiments of the present invention, the element having a lattice constant greater than that of diamond includes but is not limited to phosphorus (P), sulfur (S), selenium (Se), boron (B), aluminum (Al) or silicon (Si).
[0025] In some embodiments of the present invention, after an element ion with a lattice constant greater than that of diamond is implanted into a first ion implantation region, the first ion implantation region is protected, and a non-ion implantation region is etched using a photolithography technique to form a second ion implantation region with the same thickness as the first ion implantation region; a plurality of second ion implantation regions are arranged at intervals, and a first ion implantation region is arranged between two adjacent second ion implantation regions;
[0026] Element ions with a lattice constant smaller than that of diamond are implanted into the second ion implantation region to form an element-doped diamond modified layer.
[0027] In some embodiments of the present invention, the element ions with a lattice constant greater than that of diamond and the element ions with a lattice constant less than that of diamond are implanted in the same manner, and the implantation method includes direct implantation or patterned ion implantation using a lift-off process, and both can be implanted in a single or multiple times manner, and the implantation dose is 10 12 ~10 18 ions / cm 2 The injection energy is 40-80 KeV, the injection angle is vertical incidence, and the injection time depends on the energy and dose of the injected particles.
[0028] Preferably, the direct implantation includes applying ion implantation of elements to the diamond substrate to construct an element-doped diamond modified layer.
[0029] Preferably, the patterned ion implantation using the Lift-Off process comprises the following steps:
[0030] (1) depositing a layer of protective material on the patterned diamond substrate;
[0031] (2) removing the photoresist and the protective material covering the photoresist using a solvent, leaving the implantation area on the substrate;
[0032] (3) Ion implantation of elements is performed, the exposed areas are implanted, and the other areas are protected.
[0033] Further preferably, the protective material includes but is not limited to metal films (such as aluminum, copper, titanium, gold, silver or platinum, etc.) and oxide films (such as silicon dioxide, aluminum oxide, zinc oxide, titanium oxide or magnesium oxide, etc.).
[0034] Further preferably, the solvent includes but is not limited to acetone, isopropyl alcohol, N-methylpyrrolidone (NMP), deionized water and a dedicated photoresist remover.
[0035] In some embodiments of the present invention, after element ions with a lattice constant greater than that of diamond are implanted into the first ion implantation area, the residual photoresist or protective material (metal film or oxide film) is removed to prepare for the second ion implantation, and a photoresist coating is prepared; a second photolithography exposure is performed using a mask with an inverse pattern; and development, etching and grinding are performed again to expose the second ion implantation area where the element ions are implanted.
[0036] Preferably, the solvent used to remove the metal film and the oxide film includes, but is not limited to, nitric acid, sulfuric acid, hydrochloric acid, hydrofluoric acid, hydrogen peroxide and sodium hydroxide.
[0037] In some embodiments of the present invention, the element having a lattice constant smaller than that of diamond includes, but is not limited to, nitrogen (N), lithium (Li) or beryllium (Be).
[0038] In some embodiments of the present invention, the high temperature activation is a high temperature annealing treatment to activate ions and repair lattice defects, and the temperature of the high temperature activation is 1100-1400° C. and the time is 20-120 min.
[0039] In some embodiments of the present invention, the processing makes the thickness deviation of the element-doped diamond modified layer on the surface of the diamond substrate less than 3 μm and the surface roughness reaches 0.2-20 nm. The element-doped diamond modified layer is precisely processed to ensure its surface bonding compatibility.
[0040] The second aspect of the present invention provides a composite substrate with an element-doped diamond modified layer. The composite substrate is prepared by the preparation method described above and consists of a diamond substrate and an element-doped diamond modified layer on its surface.
[0041] In some embodiments of the present invention, the thickness of the element-doped diamond modified layer is 10 nm to 10 μm. It can be understood that the element-doped diamond modified layer refers to the element-doped diamond modified layer composed of the first ion implantation area and the non-ion implantation area after ion implantation or the element-doped diamond modified layer composed of the first ion implantation area and the second ion implantation area after ion implantation.
[0042] A third aspect of the present invention provides a semiconductor device, comprising the composite substrate and a semiconductor material of an element-doped diamond modified layer bonded to the composite substrate.
[0043] In some embodiments of the present invention, the semiconductor material includes but is not limited to Si, SiO2, GaN, InP, SiC, GaAs, AlN or Li3PO4.
[0044] A fourth aspect of the present invention provides a method for preparing the semiconductor device, comprising the following steps:
[0045] The semiconductor material is bonded to the element-doped diamond modified layer of the composite substrate at low temperature to obtain the composite substrate.
[0046] In some embodiments of the present invention, the semiconductor material includes but is not limited to Si, SiO2, GaN, InP, SiC, GaAs, AlN or Li3PO4.
[0047] In some embodiments of the present invention, the low temperature bonding includes but is not limited to plasma activated bonding, hydrophilic bonding, hydrophobic bonding, anodic bonding or BCB bonding.
[0048] The beneficial effects of the present invention are:
[0049] In order to solve the problem of huge thermal stress generated at the bonding interface at high temperature due to the mismatch of lattice constant and thermal expansion coefficient between diamond and other semiconductor materials, the present invention proposes a composite substrate with an element-doped diamond modified layer. The present invention gives full play to the excellent thermal conductivity of the diamond substrate, and modifies the diamond substrate by element doping through staggered ion implantation to form overlapping tensile stress buffer layers and compressive stress buffer layers, thereby alleviating the thermal stress mismatch problem generated at the bonding interface. In addition, by using an element-doped diamond modified layer instead of the traditional microstructure design to solve the thermal stress problem, the effective bonding area is increased, and the bonding strength of the wafer is significantly improved.
[0050] The present invention forms a tensile stress buffer layer on the surface of the diamond substrate by injecting elements with a lattice constant greater than that of diamond. Due to the large difference in lattice constants, a compressive stress buffer layer is formed in the non-ion implanted area, thereby forming overlapping tensile stress buffer layers and compressive stress buffer layers, thereby replacing the structural design and alleviating the thermal stress matching problem generated at the bonding interface through element doping. To further alleviate the thermal stress matching problem generated at the bonding interface, elements with a lattice constant greater than that of diamond are injected on the surface of the diamond substrate to form a tensile stress buffer layer on the surface of the diamond; elements with a lattice constant less than that of diamond are alternately injected to form a compressive stress buffer layer on the surface of the diamond, thereby forming overlapping tensile stress buffer layers and compressive stress buffer layers, further alleviating the thermal stress mismatch problem generated at the bonding interface. BRIEF DESCRIPTION OF THE DRAWINGS
[0051] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.
[0052] Figure 1 : is a structural diagram of a diamond substrate, wherein A is a side view and B is a top view;
[0053] Figure 2 A schematic diagram of the structure of a diamond substrate after the first ion implantation in an embodiment of the present invention;
[0054] Figure 3 A schematic structural diagram of a diamond substrate after the second ion implantation in an embodiment of the present invention;
[0055] Figure 4 A schematic structural diagram of a bonded semiconductor device according to an embodiment of the present invention.
[0056] In the figure, 1. diamond substrate; 2. diamond modified layer doped with element 1; 3. diamond modified layer doped with element 2; 4. bonded semiconductor film. DETAILED DESCRIPTION
[0057] In order to enable those skilled in the art to more clearly understand the technical solution of the present invention, the technical solution of the present invention will be described in detail below in conjunction with specific embodiments.
[0058] Example 1
[0059] like Figure 3 As shown, the composite substrate with element-doped diamond modified layer consists of a diamond substrate 1, an alternately arranged element 1-doped diamond modified layer 2 and an element 2-doped diamond modified layer 3. The diamond substrate 1 has a thickness of 350 μm and a diameter of 1 inch. The thickness of the element-doped diamond modified layer is 200 nm.
[0060] The preparation method of the composite substrate having the element-doped diamond modified layer is as follows:
[0061] (1) First prepare the diamond substrate and ensure that the surface is clean and dust-free.
[0062] (2) Spin-coat the photoresist onto the diamond substrate and cover the stripe pattern mask with a stripe width and stripe spacing of 50 μm. Use holographic exposure technology to accurately expose the photoresist layer, develop it, and etch it to obtain the first ion implantation area. Inject P ions into the first ion implantation area with an implantation dose of 10 14 ions / cm 2 The implantation energy is 20 KeV to form an element 1 doped diamond modified layer.
[0063] (3) Remove the photoresist residue and prepare for the second ion implantation.
[0064] (4) Spin-coat the photoresist onto the diamond substrate and cover the reverse pattern mask with a stripe width and stripe spacing of 50 μm. Use holographic exposure technology to accurately expose the photoresist layer, develop it, and etch it to obtain the second ion implantation area. Inject N ions into the second ion implantation area with an implantation dose of 10 14 ions / cm 2 The implantation energy is 20 KeV to form an element 2-doped diamond modified layer and remove the photoresist residue.
[0065] (5) The element-doped diamond modified layer is activated at high temperature, with an annealing temperature of 1300°C and an annealing time of 30 min.
[0066] (6) The element-doped diamond modified layer is finely processed by double-sided grinding and ion beam polishing technology, so that the overall thickness deviation is 3 μm and the surface roughness reaches about 0.5 nm, thereby meeting the surface flatness and roughness conditions for low-temperature bonding, and obtaining a composite substrate with an element-doped diamond modified layer.
[0067] The composite substrate with the element-doped diamond modified layer prepared in this embodiment is bonded with other semiconductor materials to prepare a semiconductor device, including the following steps:
[0068] The hydrophilic bonding method is used to bond the element-doped diamond modified layer and the SiC semiconductor material at low temperature to obtain a semiconductor device, the structure of which is as follows: Figure 4 shown.
[0069] Example 2
[0070] like Figure 3As shown, the composite substrate with element-doped diamond modified layer consists of a diamond substrate 1, an alternately arranged element 1-doped diamond modified layer 2 and an element 2-doped diamond modified layer 3. The diamond substrate 1 has a thickness of 600 μm and a diameter of 2 inches. The thickness of the element-doped diamond modified layer is 300 nm.
[0071] The preparation method of the composite substrate having the element-doped diamond modified layer is as follows:
[0072] (1) First prepare the diamond substrate and ensure that the surface is clean and dust-free.
[0073] (2) Spin-coat the photoresist onto the diamond substrate and cover the stripe pattern mask with a stripe width and stripe spacing of 250 μm. Use optical exposure technology to accurately expose the photoresist layer, develop it, and etch it to obtain the first ion implantation area. S ions are implanted into the first ion implantation area with an implantation dose of 10 15 ions / cm 2 The implantation energy is 30 KeV to form an element 1 doped diamond modified layer.
[0074] (3) Remove the photoresist residue and prepare for the second ion implantation.
[0075] (4) Spraying a photoresist onto a diamond substrate and covering it with an inverse pattern mask having a stripe width and stripe spacing of 250 μm. Using optical exposure technology, the photoresist layer is precisely exposed, developed, and etched to obtain a second ion implantation region. Li ions are implanted into the second ion implantation region at a dose of 10 15 ions / cm 2 The implantation energy is 30 KeV to form an element 2-doped diamond modified layer and remove the photoresist residue.
[0076] (5) The element-doped diamond modified layer is activated at high temperature, with an annealing temperature of 1250°C and an annealing time of 30 min.
[0077] (6) The element-doped diamond modified layer is finely processed by double-sided grinding and electrochemical mechanical polishing (ECMP) so that the overall thickness deviation is 2 μm and the surface roughness reaches about 1 nm, thereby meeting the surface flatness and roughness conditions for low-temperature bonding and obtaining a composite substrate with an element-doped diamond modified layer.
[0078] The composite substrate with the element-doped diamond modified layer prepared in this embodiment is bonded with other semiconductor materials to prepare a semiconductor device, including the following steps:
[0079] The element-doped diamond modified layer and the InP semiconductor material are bonded at low temperature by plasma activated bonding method to obtain a semiconductor device.
[0080] Example 3
[0081] like Figure 3 As shown, the composite substrate with element-doped diamond modified layer consists of a diamond substrate 1, an alternately arranged element 1-doped diamond modified layer 2 and an element 2-doped diamond modified layer 3. The diamond substrate 1 has a thickness of 500 μm and a diameter of 2 inches. The thickness of the element-doped diamond modified layer is 80 nm.
[0082] The preparation method of the composite substrate having the element-doped diamond modified layer is as follows:
[0083] (1) First prepare the diamond substrate and ensure that the surface is clean and dust-free.
[0084] (2) Spraying a photoresist onto a diamond substrate and covering a stripe pattern mask with a stripe width and stripe spacing of 500 μm. Using ion beam exposure technology, the photoresist layer is precisely exposed and then developed. A layer of Al is deposited on the patterned diamond substrate using chemical vapor deposition to form a metal protective layer. A special photoresist remover is used to remove the photoresist and the Al covering the photoresist, leaving the first ion implantation area on the substrate. Si ions are implanted into the first ion implantation area with an implantation dose of 10 16 ions / cm 2 The implantation energy is 45KeV to form an element 1-doped diamond modified layer.
[0085] (3) Remove the photoresist residue and prepare for the second ion implantation.
[0086] (4) Spin-coat the photoresist onto the diamond semiconductor substrate and cover the reverse pattern mask with a stripe width and stripe spacing of 500 μm. Use ion beam exposure technology to accurately expose the photoresist layer and then develop it. Deposit a layer of Al on the patterned diamond substrate using chemical vapor deposition to form a metal protective layer. Use a special photoresist remover to remove the photoresist and the Al covering the photoresist, leaving the second ion implantation area on the substrate. Inject Be ions into the second ion implantation area with an implantation dose of 10 16 ions / cm 2 The implantation energy is 45 KeV to form an element 2-doped diamond modified layer and remove the residual protective material.
[0087] (5) The element-doped diamond modified layer is activated at high temperature, with an annealing temperature of 1100°C and an annealing time of 20 min.
[0088] (6) The element-doped diamond modified layer is precisely processed by ultra-precision grinding and atomic layer polishing, so that the overall thickness deviation is 1 μm and the surface roughness reaches about 3 nm, thereby meeting the surface flatness and roughness conditions for low-temperature bonding, and obtaining a composite substrate with an element-doped diamond modified layer.
[0089] The composite substrate with the element-doped diamond modified layer prepared in this embodiment is bonded with other semiconductor materials to prepare a semiconductor device, including the following steps:
[0090] The element-doped diamond modified layer and the GaN semiconductor material are bonded at low temperature by an anodic bonding method to obtain a semiconductor device.
[0091] Example 4
[0092] like Figure 3 As shown, the composite substrate with element-doped diamond modified layer consists of a diamond substrate 1, an alternately arranged element 1-doped diamond modified layer 2, and a non-ion implanted region. The diamond substrate 1 has a thickness of 300 μm and a diameter of 1 inch. The thickness of the element-doped diamond modified layer is 60 nm.
[0093] The preparation method of the composite substrate having the element-doped diamond modified layer is as follows:
[0094] (1) First prepare the diamond substrate and ensure that the surface is clean and dust-free.
[0095] (2) The photoresist is coated on the diamond substrate by inkjet printing and covered with a stripe pattern mask with a stripe width and stripe spacing of 600 μm. The photoresist layer is precisely exposed by electron beam exposure technology, developed, and etched to obtain the first ion implantation area. Se ions are implanted in the first ion implantation area with an implantation dose of 10 14 ions / cm 2 The implantation energy is 80KeV to form an element 1-doped diamond modified layer.
[0096] (3) Remove the photoresist residue.
[0097] (4) A stress buffer layer formed by alternating arrangement of a tensile stress modifying layer formed by Se ion implantation and a diamond substrate not doped with elements is formed on the upper surface of the diamond substrate.
[0098] (5) The element-doped diamond modified layer is activated at high temperature, with an annealing temperature of 1400°C and an annealing time of 40 minutes.
[0099] (6) The element-doped diamond modified layer is precisely processed by ultra-precision grinding and ultrasonic polishing, so that the overall thickness deviation is 1 μm and the surface roughness reaches about 0.5 nm, thereby meeting the surface flatness and roughness conditions for low-temperature bonding, and obtaining a composite substrate with an element-doped diamond modified layer.
[0100] The composite substrate with the element-doped diamond modified layer prepared in this embodiment is bonded with other semiconductor materials to prepare a semiconductor device, including the following steps:
[0101] The element-doped diamond modified layer and the GaAs semiconductor material are bonded at low temperature using the BCB bonding method to obtain a semiconductor device.
[0102] Example 5
[0103] like Figure 3 As shown, the composite substrate with element-doped diamond modified layer is composed of a diamond substrate 1, an alternately arranged element 1-doped diamond modified layer 2 and an element 2-doped diamond modified layer 3. The diamond substrate 1 has a thickness of 500 μm and a diameter of 2 inches. The thickness of the element-doped diamond modified layer is 300 nm.
[0104] The preparation method of the composite substrate having the element-doped diamond modified layer is as follows:
[0105] (1) First prepare the diamond substrate and ensure that the surface is clean and dust-free.
[0106] (2) Spin-coat the photoresist onto the diamond substrate and cover the stripe pattern mask with a stripe width and stripe spacing of 1000 μm. Use holographic exposure technology to accurately expose the photoresist layer and then develop it. Deposit a layer of Ag on the patterned diamond substrate using chemical vapor deposition to form a metal protective layer. Use a special photoresist remover to remove the photoresist and the Ag covering the photoresist, leaving the first ion implantation area on the substrate. Inject P ions into the first ion implantation area with an implantation dose of 10 17 ions / cm 2 The implantation energy is 60KeV to form an element 1-doped diamond modified layer.
[0107] (3) Remove Ag residues and prepare for the second ion implantation.
[0108] (4) Spin-coat the photoresist onto the diamond substrate and cover the reverse pattern mask with a stripe width and stripe spacing of 1000 μm. Use holographic exposure technology to accurately expose the photoresist layer and then develop it. Deposit a layer of Ag on the patterned diamond substrate using chemical vapor deposition to form a metal protective layer. Use a special photoresist remover to remove the photoresist and the Ag covering the photoresist, leaving the second ion implantation area on the substrate. Inject N ions into the second ion implantation area with an implantation dose of 10 17 ions / cm 2 The implantation energy is 60KeV to form an element 2-doped diamond modified layer and remove the Ag residue.
[0109] (5) The element-doped diamond modified layer is activated at high temperature, with an annealing temperature of 1350° C. and an annealing time of 25 min.
[0110] (6) The element-doped diamond modified layer is finely processed by double-sided grinding and ultrasonic polishing technology, so that the overall thickness deviation is 2 μm and the surface roughness reaches about 3 nm, thereby meeting the surface flatness and roughness conditions for low-temperature bonding, and obtaining a composite substrate with an element-doped diamond modified layer.
[0111] The composite substrate with the element-doped diamond modified layer prepared in this embodiment is bonded with other semiconductor materials to prepare a semiconductor device, including the following steps:
[0112] The hydrophilic bonding method is used to perform low temperature bonding of the element-doped diamond modified layer and the AlN semiconductor material to obtain a semiconductor device.
[0113] Example 6
[0114] like Figure 3 As shown, the composite substrate with element-doped diamond modified layer consists of a diamond substrate 1, an alternately arranged element 1-doped diamond modified layer 2 and an element 2-doped diamond modified layer 3. The diamond substrate 1 has a thickness of 450 μm and a diameter of 1 inch. The thickness of the element-doped diamond modified layer is 45 nm.
[0115] The preparation method of the composite substrate having the element-doped diamond modified layer is as follows:
[0116] (1) First prepare the diamond substrate and ensure that the surface is clean and dust-free.
[0117] (2) Spraying a photoresist onto a diamond substrate and covering it with a stripe pattern mask having a stripe width and stripe spacing of 450 μm. Using optical exposure technology, the photoresist layer is precisely exposed, developed, and etched to obtain a first ion implantation region. Al ions are implanted into the first ion implantation region at a dose of 1015 ions / cm 2 The implantation energy is 55KeV to form an element 1-doped diamond modified layer.
[0118] (3) Remove the photoresist residue and prepare for the second ion implantation.
[0119] (4) Spraying a photoresist onto a diamond substrate and covering it with an inverse pattern mask having a stripe width and stripe spacing of 450 μm. Using optical exposure technology, the photoresist layer is precisely exposed, developed, and etched to obtain a second ion implantation region. Li ions are implanted into the second ion implantation region at a dose of 10 15 ions / cm 2 The implantation energy is 55 KeV to form an element 2-doped diamond modified layer and remove the photoresist residue.
[0120] (5) The element-doped diamond modified layer is activated at high temperature, with an annealing temperature of 1200°C and an annealing time of 60 min.
[0121] (6) The element-doped diamond modified layer is finely processed by ultra-precision grinding and ion beam polishing technology, so that the overall thickness deviation is 1 μm and the surface roughness reaches about 0.8 nm, thereby meeting the surface flatness and roughness conditions for low-temperature bonding, and obtaining a composite substrate with an element-doped diamond modified layer.
[0122] The composite substrate with the element-doped diamond modified layer prepared in this embodiment is bonded with other semiconductor materials to prepare a semiconductor device, including the following steps:
[0123] The hydrophilic bonding method is used to perform low-temperature bonding of the element-doped diamond modified layer and the GaN semiconductor material to obtain a semiconductor device.
[0124] Example 7
[0125] like Figure 3 As shown, the composite substrate with element-doped diamond modified layer consists of a diamond substrate 1, an alternately arranged element 1-doped diamond modified layer 2 and an element 2-doped diamond modified layer 3. The diamond substrate 1 has a thickness of 500 μm and a diameter of 2 inches. The thickness of the element-doped diamond modified layer is 200 nm.
[0126] The preparation method of the composite substrate having the element-doped diamond modified layer is as follows:
[0127] (1) First prepare the diamond substrate and ensure that the surface is clean and dust-free.
[0128] (2) Spraying a photoresist onto a diamond substrate and covering it with a stripe pattern mask having a stripe width and stripe spacing of 500 μm. Using electron beam exposure technology, the photoresist layer is precisely exposed, developed, and etched to obtain a first ion implantation region. P ions are implanted into the first ion implantation region at a dose of 10 13 ions / cm 2 The implantation energy is 40KeV to form an element 1-doped diamond modified layer.
[0129] (3) Remove the photoresist residue and prepare for the second ion implantation.
[0130] (4) Spin-coat the photoresist onto the diamond substrate and cover the reverse pattern mask with a stripe width and stripe spacing of 500 μm. Use electron beam exposure technology to precisely expose the photoresist layer, then develop and etch to obtain the second ion implantation area. Inject N ions into the second ion implantation area with an implantation dose of 10 13 ions / cm 2 The implantation energy is 40 KeV to form an element 2-doped diamond modified layer and remove the photoresist residue.
[0131] (5) The element-doped diamond modified layer is activated at high temperature, with an annealing temperature of 1100°C and an annealing time of 50 min.
[0132] (6) The element-doped diamond modified layer is finely processed by double-sided grinding and ultrasonic polishing, so that the overall thickness deviation is 0.5 μm and the surface roughness reaches about 2 nm, thereby meeting the surface flatness and roughness conditions for low-temperature bonding, and obtaining a composite substrate with an element-doped diamond modified layer.
[0133] The composite substrate with the element-doped diamond modified layer prepared in this embodiment is bonded with other semiconductor materials to prepare a semiconductor device, including the following steps:
[0134] The element-doped diamond modified layer and the GaAs semiconductor material are bonded at low temperature by plasma activated bonding to obtain a semiconductor device.
[0135] Example 8
[0136] like Figure 3 As shown, the composite substrate with element-doped diamond modified layer consists of a diamond substrate 1, an alternately arranged element 1-doped diamond modified layer 2 and an element 2-doped diamond modified layer 3. The diamond substrate 1 has a thickness of 600 μm and a diameter of 2 inches. The thickness of the element-doped diamond modified layer is 30 nm.
[0137] The preparation method of the composite substrate having the element-doped diamond modified layer is as follows:
[0138] (1) First prepare the diamond substrate and ensure that the surface is clean and dust-free.
[0139] (2) The photoresist is coated on the diamond substrate by inkjet printing and covered with a stripe pattern mask with a stripe width and stripe spacing of 750 μm. The photoresist layer is precisely exposed by electron beam exposure technology, developed, and etched. A layer of titanium oxide is deposited on the patterned diamond substrate by chemical vapor deposition to form an oxide protective layer. A special photoresist remover is used to remove the photoresist and the oxide covering the photoresist, leaving the first ion implantation area on the substrate. S ions are implanted in the first ion implantation area with an implantation dose of 10 15 ions / cm 2 The implantation energy is 80KeV to form an element 1-doped diamond modified layer.
[0140] (3) Remove oxide residues and prepare for the second ion implantation.
[0141] (4) The photoresist is coated on the diamond substrate by inkjet printing and covered with an inverse pattern mask with a stripe width and stripe spacing of 750 μm. The photoresist layer is precisely exposed by electron beam exposure technology and then developed and etched. A layer of titanium oxide is deposited on the patterned diamond substrate by chemical vapor deposition to form an oxide protective layer. A special photoresist remover is used to remove the photoresist and the oxide covering the photoresist, leaving the second ion implantation area on the substrate. Li ions are implanted in the second ion implantation area with an implantation dose of 10 15 ions / cm 2 The implantation energy is 80 KeV to form an element 2-doped diamond modified layer and remove oxide residues.
[0142] (5) The element-doped diamond modified layer is activated at high temperature, with an annealing temperature of 1250°C and an annealing time of 60 min.
[0143] (6) The element-doped diamond modified layer is finely processed by ultra-precision grinding and electrochemical mechanical polishing (ECMP) so that the overall thickness deviation is 1 μm and the surface roughness reaches about 0.8 nm, thereby meeting the surface flatness and roughness conditions for low-temperature bonding and obtaining a composite substrate with an element-doped diamond modified layer.
[0144] The composite substrate with the element-doped diamond modified layer prepared in this embodiment is bonded with other semiconductor materials to prepare a semiconductor device, including the following steps:
[0145] The hydrophobic bonding method is used to perform low-temperature bonding of the element-doped diamond modified layer and the GaN semiconductor material to obtain a semiconductor device.
[0146] Example 9
[0147] like Figure 3 As shown, the composite substrate with element-doped diamond modified layer is composed of a diamond substrate 1, an alternately arranged element 1-doped diamond modified layer 2 and an element 2-doped diamond modified layer 3. The diamond substrate 1 has a thickness of 400 μm and a diameter of 1 inch. The thickness of the element-doped diamond modified layer is 100 nm.
[0148] The preparation method of the composite substrate having the element-doped diamond modified layer is as follows:
[0149] (1) First prepare the diamond substrate and ensure that the surface is clean and dust-free.
[0150] (2) Spraying a photoresist onto a diamond substrate and covering it with a stripe pattern mask having a stripe width and stripe spacing of 300 μm. Using optical exposure technology, the photoresist layer is precisely exposed, developed, and etched to obtain a first ion implantation region. Si ions are implanted into the first ion implantation region at a dose of 10 14 ions / cm 2 The implantation energy is 40KeV to form an element 1-doped diamond modified layer.
[0151] (3) Remove the photoresist residue and prepare for the second ion implantation.
[0152] (4) Spraying a photoresist onto a diamond substrate and covering it with an inverse pattern mask having a stripe width and stripe spacing of 300 μm. Using optical exposure technology, the photoresist layer is precisely exposed, developed, and etched to obtain a second ion implantation region. Li ions are implanted into the second ion implantation region at a dose of 10 14 ions / cm 2 The implantation energy is 40 KeV to form an element 2-doped diamond modified layer and remove the photoresist residue.
[0153] (5) The element-doped diamond modified layer is activated at high temperature, with an annealing temperature of 1350° C. and an annealing time of 40 min.
[0154] (6) The element-doped diamond modified layer is finely processed by double-sided grinding and ion beam polishing technology, so that the overall thickness deviation is 0.8 μm and the surface roughness reaches about 1 nm, thereby meeting the surface flatness and roughness conditions for low-temperature bonding, and obtaining a composite substrate with an element-doped diamond modified layer.
[0155] The composite substrate with the element-doped diamond modified layer prepared in this embodiment is bonded with other semiconductor materials to prepare a semiconductor device, including the following steps:
[0156] The hydrophobic bonding method is used to perform low-temperature bonding of the element-doped diamond modified layer and the InP semiconductor material to obtain a semiconductor device.
[0157] Example 10
[0158] like Figure 3 As shown, the composite substrate with element-doped diamond modified layer consists of a diamond substrate 1, an alternately arranged element 1-doped diamond modified layer 2, and a non-ion implanted region. The diamond substrate 1 has a thickness of 600 μm and a diameter of 2 inches. The thickness of the element-doped diamond modified layer is 50 nm.
[0159] The preparation method of the composite substrate having the element-doped diamond modified layer is as follows:
[0160] (1) First prepare the diamond substrate and ensure that the surface is clean and dust-free.
[0161] (2) Spraying a photoresist onto a diamond substrate and covering it with a stripe pattern mask having a stripe width and stripe spacing of 500 μm. Using electron beam exposure technology, the photoresist layer is precisely exposed, developed, and etched to obtain a first ion implantation region. P ions are implanted into the first ion implantation region at a dose of 10 12 ions / cm 2 The implantation energy is 60KeV to form an element 1-doped diamond modified layer.
[0162] (3) Remove the photoresist residue.
[0163] (4) A stress buffer layer formed by alternating arrangement of a tensile stress modified layer formed by P ion implantation and a diamond substrate not doped with elements is formed on the upper surface of the diamond substrate.
[0164] (5) The element-doped diamond modified layer is activated at high temperature, with an annealing temperature of 1150°C and an annealing time of 35 min.
[0165] (6) The element-doped diamond modified layer is precisely processed by double-sided grinding and electrochemical mechanical polishing (ECMP) so that the overall thickness deviation is 2 μm and the surface roughness reaches about 2 nm, thereby meeting the surface flatness and roughness conditions for low-temperature bonding and obtaining a composite substrate with an element-doped diamond modified layer.
[0166] The composite substrate with the element-doped diamond modified layer prepared in this embodiment is bonded with other semiconductor materials to prepare a semiconductor device, including the following steps:
[0167] The element-doped diamond modified layer and the Si semiconductor material are bonded at low temperature by plasma activated bonding method to obtain a semiconductor device.
[0168] In summary, the present invention makes full use of the excellent thermal conductivity of the diamond substrate and modifies the diamond through element doping by staggered ion implantation to form overlapping tensile stress buffer layers and compressive stress buffer layers, thereby alleviating the thermal stress mismatch problem generated at the bonding interface. In addition, by using element-doped diamond modified layers instead of traditional microstructure design to solve the thermal stress problem, the effective bonding area is increased, and the bonding strength of the wafer is significantly improved.
[0169] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a composite substrate having an element-doped diamond modified layer, characterized in that: The steps include: A first ion implantation region and a non-ion implantation region are formed on the surface of the diamond substrate by using photolithography technology; a plurality of non-ion implantation regions are arranged at intervals, and a first ion implantation region is arranged between two adjacent non-ion implantation regions; Implanting element ions having a lattice constant greater than that of diamond into the first ion implantation region to form an element-doped diamond modified layer; High temperature activation of element-doped diamond modified layer; The element-doped diamond modified layer activated at high temperature is processed to obtain a composite substrate having the element-doped diamond modified layer.
2. The method for preparing a composite substrate having an element-doped diamond modified layer according to claim 1, characterized in that: The shape of the first ion implantation area includes strip, ring, grid or radial.
3. The method for preparing a composite substrate having an element-doped diamond modified layer according to claim 1, characterized in that: The element having a lattice constant greater than that of diamond includes phosphorus, sulfur, selenium, boron, aluminum or silicon.
4. The method for preparing a composite substrate having an element-doped diamond modified layer according to claim 1, characterized in that: After implanting ions of an element having a lattice constant greater than that of diamond into a first ion implantation region, the first ion implantation region is protected, and a non-ion implantation region is etched using a photolithography technique to form a second ion implantation region having the same thickness as the first ion implantation region; a plurality of second ion implantation regions are arranged at intervals, and a first ion implantation region is arranged between two adjacent second ion implantation regions; Implanting element ions with a lattice constant smaller than that of diamond into the second ion implantation region to form an element-doped diamond modified layer; Preferably, the element having a lattice constant smaller than that of diamond includes nitrogen, lithium or beryllium.
5. The method for preparing a composite substrate having an element-doped diamond modified layer according to claim 1 or 4, characterized in that: The implantation method includes direct implantation or patterned ion implantation using a lift-off process, with an implantation dose of 10 12 ~10 18 ions / cm 2 The injection energy is 40~80KeV, and the injection angle is vertical incidence.
6. The method for preparing a composite substrate having an element-doped diamond modified layer according to claim 1, characterized in that: The high temperature activation temperature is 1100-1400° C. and the time is 20-120 minutes.
7. The method for preparing a composite substrate having an element-doped diamond modified layer according to claim 1, characterized in that: The processing makes the thickness deviation of the element-doped diamond modified layer on the surface of the diamond substrate less than 3 μm, and the surface roughness reaches 0.2-20 nm.
8. A composite substrate having an element-doped diamond modified layer, characterized in that: The composite substrate is prepared by the preparation method according to any one of claims 1 to 7, and is composed of a diamond substrate and an element-doped diamond modified layer on its surface; Preferably, the thickness of the element-doped diamond modified layer is 10 nm to 10 μm.
9. A semiconductor device, characterized in that: A semiconductor material comprising the composite substrate as claimed in claim 8 and an element-doped diamond modified layer bonded to the composite substrate; Preferably, the semiconductor material includes Si, SiO2, GaN, InP, SiC, GaAs, AlN or Li3PO4.
10. A method for preparing a semiconductor device according to claim 9, characterized in that: The steps include: The semiconductor material is bonded to the element-doped diamond modified layer of the composite substrate according to claim 8 at low temperature; Preferably, the semiconductor material includes Si, SiO2, GaN, InP, SiC, GaAs, AlN or Li3PO4; Preferably, the low temperature bonding includes plasma activated bonding, hydrophilic bonding, hydrophobic bonding, anodic bonding or BCB bonding.