Ferroelectric semiconductor material, preparation method and application thereof, and scandium nitride ferroelectric semiconductor field effect transistor
By doping Sc and Sb in AlN, Al1-xScxSbyN1-y material was prepared, which solved the problem of coexistence of ferroelectricity and conductivity, achieved efficient application of ferroelectric semiconductor materials, and improved the scandium nitride ferroelectric semiconductor field Performance of effect transistors.
Patent Information
- Application Number
- CN202410973891.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-08
AI Technical Summary
It is difficult to find semiconductor materials that have both ferroelectricity and conductivity in the prior art, which are used in the channel layer of scandium nitride ferroelectric semiconductor field effect transistors, resulting in performance bottlenecks.
By doping Sc and Sb in AlN, Al1-xScxSbyN1-y material was prepared, and the ferroelectric semiconductor material was deposited by laser molecular beam epitaxial method to achieve the coexistence of ferroelectricity and conductivity.
The polarization flip barrier is reduced, the band gap is reduced, the switching ratio, storage window and sensitivity of the device are improved, compatibility with semiconductor processes is enhanced, and the memory performance of FeFET is improved.
Smart Images

Figure CN118919557A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of semiconductor materials, and in particular relates to a ferroelectric semiconductor material, a preparation method and application thereof, and a scandium nitride ferroelectric semiconductor field effect transistor. Background Art
[0002] In the traditional von Neumann architecture, memory and arithmetic units exist independently and communicate with each other through the system bus. The speed difference between memory and arithmetic units constitutes the performance bottleneck of the von Neumann architecture. This problem has become increasingly serious with the advent of the era of artificial intelligence. As a new computing architecture, storage and computing integration can eliminate the delay and power consumption caused by unnecessary data movement, and is considered to be a revolutionary technology with great potential. Scandium nitride ferroelectric semiconductor field effect transistor (FeSFET) is a potential storage and computing integration technology path. It uses conductive ferroelectric materials in the channel layer to simplify the gate structure and enhance the durability of the device. Research on two-dimensional ferroelectric semiconductor field effect transistor devices has found that FeSFET has better storage performance than ferroelectric field effect transistor (FeFET), proving that this device configuration has more advantages. Judging from the current development status, finding ferroelectric semiconductor materials with good compatibility with semiconductor processes has important practical significance for the application of FeSFET.
[0003] Al 1-x Sc x N films have excellent ferroelectric properties, including large remnant polarization (80-120 μC / cm 2 ), piezoelectric coefficient, higher Curie temperature and coercive field (1.5~6MV / cm -1 ). Since AlN has very mature commercial applications in the industry, Al 1-x Sc x N is easily integrated with GaN and CMOS processes. When used as logic and memory devices, using nitrogen-based materials as electrodes will result in thinner interface layers and smaller depolarization fields, thereby reducing power consumption and leakage current. More importantly, the carrier concentration of group III nitrides is very high. When in-plane biaxial stress is applied, the carrier mobility of AlN is anisotropic, with the c-axis direction being smaller than the in-plane direction. Al 1-x Sc x The effective electron mass of N has also been shown to be anisotropic. 1-x Sc x The band gap of N is still too large to be used in the channel layer, so finding a semiconductor material that has both ferroelectricity and conductivity becomes an urgent problem to be solved. Summary of the invention
[0004] The purpose of the present invention is to provide a ferroelectric semiconductor material and its preparation method and application, and a scandium nitride ferroelectric semiconductor field effect transistor. The ferroelectric semiconductor material provided by the present invention has both ferroelectricity and conductivity and can be used as a ferroelectric channel material.
[0005] In order to achieve the above object, the present invention provides the following technical solutions:
[0006] The present invention provides a ferroelectric semiconductor material, the chemical formula of which is Al 1- x Sc x Sb y N 1-y ; Among them, 0.1≤x≤0.5, 0.001≤y≤0.1.
[0007] Preferably, 0.2≤x≤0.4, 0.005≤y≤0.08.
[0008] Preferably, in the ferroelectric semiconductor material, the doping concentration of the Sc element is 2.2-10.8%, and the doping concentration of the Sb element is 0.06-5.9%.
[0009] The present invention also provides a method for preparing the ferroelectric semiconductor material described in the above technical solution, comprising the following steps:
[0010] Under the condition of providing N source, Al evaporation source, Sc evaporation source and Sb evaporation source are used as raw materials and deposited on the surface of the substrate by laser molecular beam epitaxy to obtain the ferroelectric semiconductor material.
[0011] Preferably, the N source is provided by a radio frequency plasma source;
[0012] The nitrogen flow rate of the radio frequency plasma source is 0.2-0.6 sccm, and the power of the plasma generator used is 300-380W.
[0013] Preferably, in the laser molecular beam epitaxy, the Al source beam flow rate is 4.2 to 9.0×10 -8 Torr, the Sc source beam flux is 2.5×10 -9 ~2.8×10 -8 Torr, Sb source beam current is 5.0×10 -9 ~3.0×10 -8 Torr.
[0014] Preferably, the temperature of the substrate is 650-850°C.
[0015] The present invention also provides the use of the ferroelectric semiconductor material described in the above technical solution or the ferroelectric semiconductor material obtained by the preparation method described in the above technical solution in a transistor.
[0016] The present invention also provides a scandium nitride ferroelectric semiconductor field effect transistor, comprising a substrate, a gate electrode, a gate dielectric layer, a ferroelectric semiconductor channel layer, a source electrode and a drain electrode; the substrate, the gate electrode, the gate dielectric layer and the ferroelectric semiconductor channel layer are stacked in sequence; the source electrode and the drain electrode are independently distributed on the ferroelectric semiconductor channel layer and the surface of the gate dielectric layer not covered by the ferroelectric semiconductor channel layer;
[0017] The material of the ferroelectric semiconductor channel layer is the ferroelectric semiconductor material described in the above technical solution or the ferroelectric semiconductor material obtained by the preparation method described in the above technical solution.
[0018] The present invention provides a ferroelectric semiconductor material, the chemical formula of which is Al 1- x Sc x Sb y N 1-y ; Wherein, 0.1≤x≤0.5, 0.001≤y≤0.1. In the ferroelectric semiconductor material provided by the present invention, by doping Sc in AlN, the polarization switching barrier can be reduced to obtain ferroelectricity. 1-x Sc x The band gap of N is still too large to be used in the channel layer. In order to obtain a ferroelectric semiconductor material for the channel, Al with both ferroelectricity and conductivity is obtained by co-doping Sb and Sc. 1-x Sc x Sb y N 1-y Materials. A small amount of Sb doping can significantly reduce Al 1-x Sc x N band gap, and has little effect on ferroelectricity. The reduction of the band gap is mainly due to the Sb impurity states appearing in the valence band. These impurity states have almost no effect on the conduction band and are relatively independent and can be used for conduction dominated by Sb impurity states. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.
[0020] Figure 1 Schematic diagram of the structure of the scandium ferroelectric nitride semiconductor field effect transistor obtained in Example 1, wherein 1 is a substrate, 2 is a gate electrode, 3 is a gate dielectric layer, 4 is a scandium ferroelectric nitride semiconductor, 5 is a source electrode, and 6 is a drain electrode;
[0021] Figure 2 The schematic diagram of the working principle and the current-voltage curve of the scandium nitride ferroelectric semiconductor field effect transistor obtained in Example 1;
[0022] Figure 3 The figure is a relationship diagram between Sb element doping and band gap, Sc element doping and polarization intensity and energy barrier in the ferroelectric semiconductor material obtained by the present invention;
[0023] Figure 4 For AlN and doped system Al 1-x Sc x N、AlSb y N 1-y 、Al 1-x Sc x Sb y N 1-y The state density (top) and projected state density (bottom) when x = 0.167, y = 0.056;
[0024] Figure 5 The ferroelectric semiconductor material Al 1-x Sc x Sb y N 1-y Polarization reversal barrier curve. DETAILED DESCRIPTION
[0025] The present invention provides a ferroelectric semiconductor material, the chemical formula of which is Al 1- x Sc x Sb y N 1-y ; Among them, 0.1≤x≤0.5, 0.001≤y≤0.1.
[0026] In the present invention, unless otherwise specified, all raw material components are commercially available products well known to those skilled in the art.
[0027] In the present invention, 0.1≤x≤0.5, preferably 0.2≤x≤0.4; 0.001≤y≤0.1, preferably 0.005≤y≤0.08, more preferably 0.02≤y≤0.06.
[0028] In the present invention, in the ferroelectric semiconductor material, the doping concentration of the Sc element is preferably 2.2-10.8%, more preferably 4.3-8.7%, and the doping concentration of the Sb element is preferably 0.06-5.9%, more preferably 1.2-3.5%.
[0029] In the ferroelectric semiconductor material provided by the present invention, Sc is doped into AlN to reduce its polarization reversal barrier so as to obtain ferroelectricity. 1-x Scx The band gap of N is still too large to be used in the channel layer. In order to obtain a ferroelectric semiconductor material for the channel, Al with both ferroelectricity and conductivity is obtained by co-doping Sb and Sc. 1-x Sc x Sb y N 1-y The Sb impurity state produced by a small amount of Sb doping and the strong quantum interaction with neighboring N atoms can significantly reduce the Al 1-x Sc x N band gap, and has little effect on ferroelectricity. These impurity states have almost no effect on the conduction band and are relatively independent, and can be used for conduction dominated by Sb impurity states. For example, when the doping concentration is x = 0.17, y = 0.06, Al 1-x Sc x Sb y N 1-y Compared to Al 1-x Sc x The N polarization intensity is reduced to 0.87C / m 2 , which is still a large value, while the coercive field does not change much; the band gap decreases from 4.8eV to 1.76eV, which is close to the band gap of traditional semiconductor materials.
[0030] The present invention also provides a method for preparing the ferroelectric semiconductor material described in the above technical solution, comprising the following steps:
[0031] Under the condition of providing N source, Al evaporation source, Sc evaporation source and Sb evaporation source are used as raw materials and deposited on the surface of the substrate by laser molecular beam epitaxy to obtain the ferroelectric semiconductor material.
[0032] In the present invention, the N source is preferably provided by a radio frequency plasma source; the nitrogen flow rate of the radio frequency plasma source is preferably 0.2-0.6 sccm, more preferably 0.2-0.4 sccm, and the power of the plasma generator used is preferably 300-380 W, more preferably 320-350 W.
[0033] In the present invention, in the laser molecular beam epitaxy, the Al source beam flow rate is preferably 4.2 to 9.0×10 -8 Torr, more preferably 4.5 to 7.0 × 10 -8 Torr; the Sc source beam flux is preferably 2.5×10 -9 ~2.8×10 -8 Torr, more preferably 5.0×10 -9 ~1.5×10 -8 Torr; the Sb source beam flow rate is preferably 5.0×10 -9 ~3.0×10 -8Torr, more preferably 6.0×10 -9 ~2.0×10 -8 Torr.
[0034] In the present invention, the raw materials for laser molecular beam epitaxy are preferably Al evaporation source, Sc evaporation source and Sb evaporation source; the purity of the Al evaporation source is preferably above 99.99995%, more preferably 99.99995%; the purity of the Sc evaporation source is preferably above 99.9%, more preferably 99.9%; the purity of the Sb evaporation source is preferably above 99.999%, more preferably 99.999%.
[0035] In the present invention, the temperature of the substrate is preferably 650-850°C, more preferably 700-800°C.
[0036] The preparation method provided by the present invention can easily and accurately control the beam intensity, and the film composition and doping concentration can be adjusted with the change of the source. It can reduce the defect concentration in the film, reduce the leakage current of the ferroelectric film and increase its breakdown voltage, grow a high-quality single crystal film, and thus be easier to integrate with semiconductor processes.
[0037] The present invention also provides the use of the ferroelectric semiconductor material described in the above technical solution or the ferroelectric semiconductor material obtained by the preparation method described in the above technical solution in a transistor.
[0038] In the present invention, the ferroelectric semiconductor material is preferably used as a channel material in a transistor.
[0039] The present invention does not have any special limitation on the application process of the ferroelectric semiconductor material in transistors, and the application process may be carried out in a manner familiar to those skilled in the art.
[0040] The present invention also provides a scandium nitride ferroelectric semiconductor field effect transistor, comprising a substrate, a gate electrode, a gate dielectric layer, a ferroelectric semiconductor channel layer, a source electrode and a drain electrode; the substrate, the gate electrode, the gate dielectric layer and the ferroelectric semiconductor channel layer are stacked in sequence; the source electrode and the drain electrode are independently distributed on the ferroelectric semiconductor channel layer and the surface of the gate dielectric layer not covered by the ferroelectric semiconductor channel layer;
[0041] The material of the ferroelectric semiconductor channel layer is the ferroelectric semiconductor material described in the above technical solution or the ferroelectric semiconductor material obtained by the preparation method described in the above technical solution.
[0042] In the present invention, the substrate is preferably a silicon substrate; the thickness is preferably 100 nm to 300 nm, more preferably 150 nm to 250 nm.
[0043] In the present invention, the material of the gate electrode is preferably Ti, Au, Pt, Ni, Pd or Cr, more preferably Ti, Au and Pt; the thickness is preferably 10 to 30 nm, more preferably 15 to 25 nm; the preparation method is preferably chemical vapor deposition or physical vapor deposition; the physical vapor deposition is preferably electron beam evaporation coating; the present invention does not have any special limitation on the process of chemical vapor deposition, and a method familiar to those skilled in the art may be used.
[0044] In the present invention, the material of the gate dielectric layer is preferably HfO2 or Al2O3, more preferably HfO2; the thickness is preferably 10-30 nm, more preferably 15-25 nm; the preparation method is preferably atomic deposition or chemical vapor deposition; the present invention does not have any special limitation on the process of atomic deposition or chemical vapor deposition, and can be prepared by methods familiar to those skilled in the art.
[0045] In the present invention, due to the voltage-dividing effect of the dielectric layer, when the dielectric layer is very thin, the voltage applied to the ferroelectric channel layer can completely reverse the ferroelectric polarization; the thicker the dielectric layer, the voltage applied to the ferroelectric channel layer can partially reverse the ferroelectric polarization. The present invention mainly describes the case where the dielectric layer is thicker.
[0046] In the present invention, the ferroelectric semiconductor channel layer is the ferroelectric semiconductor material described in the above technical solution or the ferroelectric semiconductor material obtained by the preparation method described in the above technical solution; the preparation method of the ferroelectric semiconductor channel layer is preferably the preparation method of the ferroelectric semiconductor material described in the above technical solution; wherein, the substrate is preferably a gate dielectric layer; the thickness of the ferroelectric semiconductor channel layer is preferably 10 to 100 nm, more preferably 20 to 80 nm; the present invention does not have any special limitation on the deposition time, as long as the ferroelectric semiconductor channel layer can reach the above thickness range.
[0047] In the present invention, the materials of the source and drain are independently preferably Al, Pt, Cr, Pd, Au or TiN, more preferably Al, Pt or Cr; the thickness is preferably 10-50 nm, more preferably 20-40 nm; the preparation method is preferably to first set the mask pattern by photolithography technology, and then use chemical vapor deposition or physical vapor deposition to prepare the source and drain; the physical vapor deposition is preferably electron beam evaporation coating; the present invention does not have any special limitation on the process of setting the mask pattern, and can be used in a manner familiar to those skilled in the art.
[0048] The scandium nitride ferroelectric semiconductor field effect transistor provided by the present invention places the scandium nitride ferroelectric material in the channel layer, and its polarized charge can directly affect the transmission of carriers without coupling through the gate dielectric layer. This more direct and stronger charge coupling effect can improve the switching ratio, storage window and sensitivity of the device, and further enhance the storage and computing performance of FeFET.
[0049] To further illustrate the present invention, the ferroelectric semiconductor material, preparation method and application thereof, and scandium nitride ferroelectric semiconductor field effect transistor provided by the present invention are described in detail below in conjunction with the accompanying drawings and embodiments, but they should not be construed as limiting the scope of protection of the present invention.
[0050] Example 1
[0051] Step 1: Deposit gate electrode Au on the silicon substrate by electron beam evaporation with a thickness of 20 nm.
[0052] Step 2: Using atomic deposition technology, prepare a HfO2 insulating dielectric layer with a thickness of 30nm on the gate electrode.
[0053] Step 3: Prepare ferroelectric channel material on the dielectric layer. Al 1-x Sc x Sb y N 1-y Epitaxial film, N is provided by radio frequency plasma source, Sc evaporation source purity is 99.9%, Al evaporation source purity is 99.99995%, Sb evaporation source purity is 99.999%. Specific preparation conditions: nitrogen flow rate is maintained at 0.3sccm, plasma generator power is 350W, Sc source beam flow rate is 5.6×10 -9 Torr, Al source beam current 4.5×10 -8 Torr, Sb source beam current 6.2×10 -9 Torr. The substrate temperature was maintained at 700°C. The resulting ferroelectric semiconductor channel material was co-doped Al 0.833 Sc 0.167 Sb 0.056 N 0.944 , wherein the Sb doping concentration is 5.6%, the Sc doping concentration is 16.7%, and the thickness is 100 nm.
[0054] Step 4: Use photolithography technology to set mask patterns on the source and drain of the device, and then use electron beam evaporation to deposit electrode material Au on the channel material with a thickness of 30nm.
[0055] The schematic diagram of the structure of the obtained scandium nitride ferroelectric semiconductor field effect transistor is shown in Figure 1, wherein 1 is a substrate, 2 is a gate electrode, 3 is a gate dielectric layer, 4 is a scandium nitride ferroelectric semiconductor, 5 is a source electrode, and 6 is a drain electrode.
[0056] The working principle diagram and current-voltage curve of the obtained scandium nitride ferroelectric semiconductor field effect transistor are shown in Figure 2 .like Figure 2 As shown in (a) and (b), +- represents bound charge, and + represents Sb vacancies. When a reverse voltage is applied to the gate, the polarization direction is downward, the threshold voltage increases, and the device presents a high resistance state; when a forward voltage is applied to the gate, the polarization direction is upward, the Sb vacancies that dominate the conduction accumulate on the lower surface of the channel, the threshold voltage decreases, and the device presents a low resistance state. The corresponding current-voltage curve is shown in Figure 2 (c) shows a counterclockwise loop. Therefore, under the regulation of different gate voltages, the device has different threshold voltages, and FeSFET has two different resistance states.
[0057] Comparative Example 1
[0058] The semiconductor material and transistor are prepared according to the technical solution provided in Example 1, with the only difference being that the channel material is not doped with Sc and Sb.
[0059] Comparative Example 2
[0060] The semiconductor material and transistor are prepared according to the technical solution provided in Example 1, with the only difference being that the channel material is not doped with Sc.
[0061] Comparative Example 3
[0062] The semiconductor material and transistor are prepared according to the technical solution provided in Example 1, with the only difference being that the channel material is not doped with Sb.
[0063] Test Case
[0064] Existing ferroelectric field effect transistors (FeFETs) have limited fatigue resistance due to problems such as trapped charge and leakage current at the interface between the ferroelectric layer and the channel. FeSFET uses ferroelectric semiconductor materials in the channel layer, which is 3 in the structure diagram, integrating the functions of ferroelectricity and conductivity. Its polarization charge can directly affect the transmission of carriers without coupling through the gate dielectric layer. This more direct and stronger charge coupling effect can improve the device's switching ratio, sensitivity, memory window, etc., and further enhance the storage and computing performance of FeFET.
[0065] Al obtained by co-doping method 1-x Sc x Sb y N 1-yFerroelectric semiconductor materials have better compatibility with semiconductor processes and can be applied more quickly than the two-dimensional ferroelectric channel materials that are currently being studied more. Sc can reduce the polarization reversal barrier of AlN to make it ferroelectric, and Sb can significantly reduce the band gap to make AlN conductive. Different doping elements in this co-doping method play different roles and have a synergistic effect, thus achieving the coexistence of ferroelectricity and conductivity.
[0066] The ferroelectric semiconductor material of the present invention is calculated by the first principle method, wherein the relationship between Sb element doping and band gap, Sc element doping and polarization intensity and energy barrier is shown in Figure 3 The band gaps of all systems were calculated using hybrid functional (HSE06).
[0067] like Figure 3 (a) It can be seen that a small amount of Sb can significantly reduce the band gap of AlN and also significantly reduce the Al 1-x Sc x N band gap; As shown in Figure (b), doping Sb makes Al 1-x Sc x The polarization intensity of N decreases slightly; from (c), we can see that with the increase of Sc concentration, the polarization reversal barrier of AlN gradually decreases. After Sb doping, the polarization reversal barrier does not change much, which means that the corresponding coercive field does not change much. Specifically, when x=0.167 and y=0.056, Al 1-x Sc x Sb y N 1-y The band gap is reduced to 1.76 eV and the polarization strength is 0.87 C / m 2 , which shows that its ferroelectricity and conductivity coexist.
[0068] AlN and different doping systems (Al 1-x Sc x N、AlSb y N 1-y 、Al 1-x Sc x Sb y N 1-y ) Take x = 0.167, y = 0.056 for the state density (above) and the projected state density (below) Figure 4 .
[0069] Depend on Figure 4 It can be seen that the band gap of AlN is 5.56eV, Al 1-x Sc x The band gap of N (x = 0.167) is 4.81 eV, AlSb y N 1-y (y=0.056) band gap is 2.38eV, Al 1-x Scx Sb y N 1-y The band gap of (x=0.167,y=0.056) is 1.76eV. From (b), we can see that Sc dominates the conduction band, from (c), we can see that the Sb impurity state dominates the valence band, and from (d), we can see that Sc and Sb work together to further reduce the band gap. The band gap of the co-doped system is smaller than the band gap of only one element, so the two doping elements have a synergistic effect in reducing the band gap.
[0070] The ferroelectric semiconductor material Al 1-x Sc x Sb y N 1-y The polarization reversal barrier curve is shown in Figure 5 .Depend on Figure 5 It can be seen that the polarization intensity and the reversal barrier do not change much after doping with Sb.
[0071] The polarization reversal barrier can be used to 1-x Sc x Sb y N 1-y The coercive field of the system is calculated, and the specific steps are as follows.
[0072] 1. Combined with the Landau-Ginzburg equation G = EP + 1 / 2aP 2 +1 / 4bP 4 And the formula a(T)=a0*(TT c ) / T c Fit the polarization reversal barrier curve and obtain the polarization reversal barrier E at room temperature b .
[0073] 2. Assume that E is the electric field strength required for flipping polarization, and its energy density is w = 1 / 2EP. The energy density can be calculated by w = E b / V f.u. get.
[0074] The above method can be used to estimate the Al 1-x Sc x Sb y N 1-y The coercive field of Al is 31.6 MV / cm. 1-x Sc x The coercive field of N is 24.8-32.1 MV / cm, while the experimentally measured Al 1-x Sc x The coercive field value of N is 2-6 MV / cm, which means that the estimated value should be reduced by about 5 to 10 times, so Al 1-x Sc x Sby N 1-y The experimental value of the coercive field is about 5.9 MV / cm. 1-x Sc x The coercive field and breakdown voltage of N (E c / E bd ) ratio is in the range of 33%-83%. Due to the extremely low doping concentration of Sb, the breakdown voltage of the co-doped system is mainly caused by the matrix Al 1-x Sc x N determines, from which Al can be deduced 1- x Sc x Sb y N 1-y The breakdown voltage ranges from 7.1 to 17.8 MV / cm, which is greater than its coercive field. In addition, the breakdown voltage can also be regulated by stress, composition, structure, etc. Therefore, in the ferroelectric semiconductor material provided by the present invention, by doping Sc in AlN, its polarization reversal barrier can be reduced to obtain ferroelectricity, and by co-doping Sb and Sc, AlN with both ferroelectricity and conductivity can be obtained. 1-x Sc x Sb y N 1-y materials, the system is feasible.
[0075] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.
Claims
1. A ferroelectric semiconductor material, It is characterized in that The chemical formula of the ferroelectric semiconductor material is Al 1-x Sc x Sb y N 1-y ; Among them, 0.1≤x≤0.5, 0.001≤y≤0.
1.
2. The ferroelectric semiconductor material according to claim 1, It is characterized in that 0.2≤x≤0.4, 0.005≤y≤0.
08.
3. The ferroelectric semiconductor material according to claim 1, It is characterized in that In the ferroelectric semiconductor material, the doping concentration of the Sc element is 2.2-10.8%, and the doping concentration of the Sb element is 0.06-5.9%.
4. A method for preparing the ferroelectric semiconductor material according to any one of claims 1 to 3, It is characterized in that The following steps are involved: Under the condition of providing N source, Al evaporation source, Sc evaporation source and Sb evaporation source are used as raw materials and deposited on the surface of the substrate by laser molecular beam epitaxy to obtain the ferroelectric semiconductor material.
5. The preparation method according to claim 4, It is characterized in that The N source is provided by a radio frequency plasma source; The nitrogen flow rate of the radio frequency plasma source is 0.2-0.6 sccm, and the power of the plasma generator used is 300-380W.
6. The preparation method according to claim 4, It is characterized in that In the laser molecular beam epitaxy, the Al source beam flow rate is 4.2 to 9.0×10 -8 Torr, the Sc source beam flux is 2.5×10 -9 ~2.8×10 -8 Torr, Sb source beam current is 5.0×10 -9 ~3.0×10 -8 Torr.
7. The preparation method according to claim 4, It is characterized in that The temperature of the substrate is 650-850°C.
8. Use of the ferroelectric semiconductor material according to any one of claims 1 to 3 or the ferroelectric semiconductor material obtained by the preparation method according to any one of claims 4 to 7 in transistors.
9. A scandium nitride ferroelectric semiconductor field effect transistor, It is characterized in that The invention comprises a substrate, a gate electrode, a gate dielectric layer, a ferroelectric semiconductor channel layer, a source electrode and a drain electrode; the substrate, the gate electrode, the gate dielectric layer and the ferroelectric semiconductor channel layer are stacked in sequence; the source electrode and the drain electrode are independently distributed on the ferroelectric semiconductor channel layer and the surface of the gate dielectric layer not covered by the ferroelectric semiconductor channel layer; The material of the ferroelectric semiconductor channel layer is the ferroelectric semiconductor material according to any one of claims 1 to 3 or the ferroelectric semiconductor material obtained by the preparation method according to any one of claims 4 to 7.
10. The scandium nitride iron electric semiconductor field effect transistor according to claim 9, It is characterized in that The thickness of the ferroelectric semiconductor channel layer is 10-100 nm.