In-situ nanoscale thick zinc oxide (at) cathode and preparation and application thereof in zinc battery

By forming a nanoscale thick zinc oxide layer in situ on the zinc anode, the problems of hydrogen evolution reaction and zinc dendrite growth in aqueous zinc-ion batteries are solved, and the stability and activity of zinc batteries under high discharge depth and high current conditions are improved.

CN118919633APending Publication Date: 2024-11-08CENT SOUTH UNIV +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411163178.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing zinc anode materials in aqueous zinc-ion batteries suffer from problems such as zinc electrode dissolution, by-product proliferation, and zinc dendrite growth caused by hydrogen evolution reaction, which affect the stability and lifespan of the battery, especially under high discharge depth and high current conditions.

Method used

An in-situ nanoscale thick zinc oxide@zinc anode preparation method is adopted. By acid etching, oxidation treatment and modification treatment of zinc substrate, combined with heat treatment, a nanoscale ultrathin zinc oxide layer is formed, and the microstructure of the material is optimized to improve the interface stability and zinc ion conductivity.

Benefits of technology

Electrochemical stability and activity of zinc anode under high discharge depth and high current conditions were achieved, improving the performance of zinc battery, especially stability and cycle performance under high current density and large areal capacity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919633A_ABST
    Figure CN118919633A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of zinc batteries, and particularly relates to an in-situ nanoscale thick zinc oxide (at) negative electrode which comprises a zinc substrate and a nanoscale-thickness zinc oxide layer compounded on the surface of the zinc substrate in situ. The invention also comprises preparation of the in-situ nanoscale thick zinc oxide (at) negative electrode and application of the in-situ nanoscale thick zinc oxide (at) negative electrode in preparation of a zinc battery. The zinc negative electrode disclosed by the invention has excellent activity and structural stability, can meet the application requirements under high discharge depth and large current, and can obtain excellent electrochemical performance under the condition.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of zinc ion batteries, and in particular to the field of zinc metal negative electrode materials. Background Art

[0002] With the increasing severity of environmental problems, the continuous depletion of fossil energy and the continuous decline in the grade of mineral resources, it is urgent to develop a new electrochemical energy storage system. -1 Aqueous zinc-ion batteries (ZIBs) are becoming one of the most attractive candidates due to their low redox potential of -0.76 V relative to the standard hydrogen electrode (SHE) and their non-toxic characteristics. One of the primary issues limiting the commercial application of aqueous zinc-ion batteries is the dissolution of the zinc electrode caused by the hydrogen evolution reaction (HER) of the zinc metal electrode in the aqueous electrolyte. Secondly, the local increase in pH caused by the hydrogen evolution reaction leads to the continuous proliferation of by-products, resulting in the loss of the zinc electrode. In addition, the uneven surface of the zinc electrode leads to the growth of zinc dendrites, which eventually pierce the diaphragm and cause a short circuit in the battery, which limits its commercial application.

[0003] At present, the solution to solve the side reactions of zinc negative electrode and inhibit the growth of zinc dendrites is to use coatings to modify the interface of zinc negative electrode. The main methods of interface modification include vapor deposition, pyrolysis, hydrothermal, coating, etc. However, the improvement of zinc negative electrode by interface modification is not significant. Only relying on the one-time coating or deposition of modified materials has limited effect on alleviating side reactions and zinc dendrites. The coating or growth materials without electrochemical activity greatly reduce the conductivity of zinc negative electrode, covering up the advantage of huge theoretical specific capacity of zinc negative electrode. Therefore, the application of using coatings to modify zinc negative electrode is very limited.

[0004] In view of the problems faced by zinc negative electrode coatings, some improvement methods have also been reported in the prior art. For example, a Chinese patent document with publication number CN118398751A discloses a method for preparing a zinc negative electrode protected by an eggshell membrane-polymer composite material, comprising: dissolving indium chloride and a polymer in an organic solvent to obtain an organic solvent solution of indium chloride-polymer; peeling the eggshell membrane from the egg, washing it with deionized water to obtain the eggshell membrane; dripping the organic solvent solution of indium chloride-polymer on the surface of a clean zinc negative electrode, then covering it with an eggshell membrane, and drying it naturally to obtain an eggshell membrane-polymer protected zinc negative electrode. A Chinese patent document with publication number CN118281229A discloses a method for preparing an organic polymer-metal copper composite coating for a zinc negative electrode, which constructs an organic polymer-metal copper composite coating on a zinc negative electrode through a one-step, in-situ, spontaneous replacement reaction. The composite coating exhibits a unique double-layer structure, with an outer layer being a porous organic layer and an inner layer being a zinc-philic copper layer. The outer layer with functional groups can serve as migration sites and transport channels for zinc ions, promoting the transfer kinetics. Meanwhile, the organic components can enhance the interfacial adhesion between the copper layer and the zinc anode.

[0005] Although the prior art discloses some improved coating solutions, the electrochemical stability of the obtained materials at high discharge depth and high current density still needs to be improved. Summary of the invention

[0006] In view of the problems of side reactions and zinc dendrite growth in existing zinc negative electrode materials, especially the unsatisfactory life at high discharge depth, the first purpose of the present invention is to provide an in-situ nano-scale thick zinc oxide @ zinc negative electrode, aiming to provide a kind of electrochemical stability with excellent performance, especially high discharge depth and high current density.

[0007] The second object of the present invention is to provide a method for preparing the in-situ nanoscale thick zinc oxide @ zinc negative electrode, aiming to prepare the in-situ nanoscale thick zinc oxide @ zinc negative electrode with excellent performance.

[0008] The third object of the present invention is to provide the application of the in-situ nano-scale thick zinc oxide@zinc negative electrode in the negative electrode of a zinc ion battery.

[0009] The fourth object of the present invention is to provide a zinc battery comprising the in-situ nano-scale thick zinc oxide@zinc negative electrode.

[0010] Most of the existing zinc oxide coated zinc cathodes are prepared by coating. The thickness of the zinc oxide coating is relatively thick, usually reaching the millimeter level, and the interface composite stability is not ideal. It is easy to expand and peel off, and it is difficult to adapt to the application requirements under high current and high discharge depth conditions. In view of this problem, the present invention has been studied in depth and provides the following solutions:

[0011] An in-situ nanometer-thick zinc oxide@zinc negative electrode comprises a zinc substrate and a nanometer-thick zinc oxide layer in-situ composited on the surface of the zinc substrate.

[0012] The present invention provides a zinc negative electrode on which an ultra-thin zinc oxide coating with a thickness of nanometers is in-situ composited, which has excellent activity and interface stability, can adapt to application requirements under high discharge depth and large current, and can improve its performance under high discharge depth and large current.

[0013] In the present invention, there is a chemical reaction between the zinc substrate and the zinc oxide layer.

[0014] Preferably, the zinc substrate is an ultra-thin zinc foil with a thickness of 10 to 50 μm.

[0015] Preferably, the crystal form of zinc oxide is wurtzite structure.

[0016] Preferably, the thickness of the zinc oxide layer is 100-500 nm.

[0017] The present invention also provides a method for preparing the in-situ nano-scale thick zinc oxide @ zinc negative electrode, wherein the zinc substrate is pre-etched with an acid solution, and then heated in an oxidizing atmosphere for surface pre-oxidation to obtain a pre-treated zinc substrate;

[0018] The pretreated zinc substrate is immersed in a modification solution containing the compound of formula 1 for surface modification to obtain a modified zinc substrate; the modified zinc substrate is then subjected to a first heat preservation treatment at a temperature T1, and then subjected to a second heat preservation treatment at a temperature T2, to obtain the in-situ nano-scale thick zinc oxide @ zinc negative electrode;

[0019]

[0020] The R1 is a C1-C6 alkyl or substituted alkyl; the R2 is H, amino, substituted amino or sulfonic acid; the R3 is amino or sulfonic acid; the R4 is H, hydroxyl or a C1-C6 alkyl; the Ar is an aromatic ring;

[0021] The 50≤T1<200℃; the temperature T2 is 200~400℃.

[0022] The present invention innovatively pre-treats the zinc substrate with acid and oxidizing atmosphere, then performs the modification treatment according to formula 1, and then cooperates with the subsequent T1 / T2 combined heat treatment. This unexpectedly forms an ultra-thin zinc oxide layer at the nanoscale in situ on the surface of the zinc substrate and optimizes the microscopic physicochemical structure of the material. In this way, a zinc negative electrode with excellent activity and adapted to high discharge depth and large current application requirements can be prepared.

[0023] In the present invention, the thickness of the zinc substrate is controlled to be between 10 and 60 μm, and can further be between 30 and 55 μm.

[0024] The present invention pre-etches the surface of the zinc substrate with acid and performs pre-oxidation treatment, which is beneficial to optimizing the surface structure, facilitating the combination with subsequent processes, inducing the growth of ultra-thin zinc oxide and high chemical reaction recombination, and further facilitating improving the performance of the prepared zinc negative electrode under high discharge depth and high current.

[0025] Preferably, the acid solution is an aqueous solution of an inorganic acid; the inorganic acid preferably includes at least one of sulfuric acid, hydrochloric acid, and nitric acid, preferably hydrochloric acid. Studies have shown that the use of hydrochloric acid can be further combined with the process of the present invention to further enhance the performance of the prepared electrode at high discharge depth and high current.

[0026] Preferably, the concentration of the inorganic acid in the acid solution is 0.05 to 5 mol / l, preferably 0.1 to 0.4 mol / l, and further can be 0.1 to 0.2 M. In the present invention, at the preferred concentration, it can be further combined with the subsequent process to further enhance the performance of the obtained negative electrode at high discharge depth and current.

[0027] In the present invention, the temperature and time of the surface etching treatment stage can be adjusted as needed. For example, the temperature can be 25 to 65°C, and further 25 to 40°C.

[0028] In the present invention, the surface etching time is 0.2 to 2 hours, preferably 1 to 1.25 hours.

[0029] In the present invention, the liquid-to-solid ratio of the acid solution to the zinc substrate is 1 to 50 ml / g, preferably 10 to 30 ml / g.

[0030] In the present invention, the oxidizing atmosphere is an atmosphere containing oxygen, preferably at least one of oxygen and an oxygen-diluent mixed gas.

[0031] Preferably, the diluent gas includes at least one of nitrogen and an inert gas.

[0032] Preferably, the oxygen content in the oxidizing atmosphere is above 10%, preferably 10% to 90%, preferably 45% to 55%. The present invention shows that at this oxygen content, it can be further combined with other processes to further enhance the performance of the obtained negative electrode at high discharge depth and current.

[0033] Preferably, the temperature of the surface pre-oxidation treatment is 45°C to 100°C, preferably 75°C to 95°C.

[0034] Preferably, the surface pre-oxidation treatment time is 0.5 h to 3 h, preferably 1.5 h to 2 h.

[0035] The present invention innovatively modifies the pre-treated zinc in Formula 1, which is conducive to growing a nano-scale zinc oxide coating on a zinc substrate, improving the chemical connection between the coating and the zinc substrate, optimizing the crystal orientation order, accelerating the conduction rate of zinc ions, and reducing the transmission barrier of zinc ions. The method of the present invention can obtain a new material with completely new physical and chemical characteristics, and the new material can exhibit excellent high discharge depth and stability under high current density.

[0036] In the present invention, in Formula 1, R1 is a C1-C6 alkyl group;

[0037] Preferably, said R2 is H, amino or sulfonic acid;

[0038] Preferably, the R3 is an amino group or a sulfonic acid group;

[0039] Preferably, said R4 is H;

[0040] Preferably, Ar is a benzene ring or a benzene ring with a substituent; the substituent includes at least one of halogen, C1-C6 alkyl, C1-C6 alkoxy, hydroxyl, nitro, trifluoromethyl, and ester.

[0041] In the present invention, in the modified solution, the concentration of Formula 1 can be above 0.5 mg / ml, preferably 1 to 10 mg / ml, and further 1 to 5 mg / ml. Studies have shown that under the preferred ratio, a better synergistic effect can be obtained, which can further enhance the performance of the material under high discharge depth and high current.

[0042] Preferably, the weight ratio of Formula 1 in the modified solution to the zinc substrate (relative to the zinc substrate before surface etching treatment) is 0.01 to 2:1, further 0.05 to 0.5:1, and further 0.05 to 0.1:1.

[0043] In the present invention, the temperature in the modification stage is 20 to 40°C, preferably 24 to 28°C.

[0044] Preferably, the modification treatment time is more than 5 hours, preferably 12 to 36 hours, and preferably 20 to 28 hours.

[0045] In the present invention, after the modified immersion treatment, washing and drying treatment can be performed to obtain the modified zinc substrate. The washing process includes water washing and alcohol washing treatments performed in sequence. The drying method can be vacuum drying, the drying temperature is 60 to 80° C., and the drying time is preferably 12 to 14 hours.

[0046] In the present invention, the first stage of heat preservation and the second stage of heat preservation are carried out in a protective atmosphere.

[0047] Preferably, the protective atmosphere includes at least one of nitrogen and an inert gas.

[0048] In the present invention, on the basis of the acid etching, surface oxidation and modification of formula 1, a two-stage heat treatment process and a combined control of temperature are further combined to further strengthen the crystal structure and interface effect of the material, which helps to further enhance the performance of the obtained negative electrode at high discharge depth and current.

[0049] Preferably, the temperature T1 is 75-150°C, preferably 130-145°C.

[0050] Preferably, the temperature T2 is 220-380°C, further 280-320°C.

[0051] Preferably, the first insulation time t1 is 2 to 5 hours.

[0052] Preferably, the second insulation time t2 is 1 to 5 hours.

[0053] The present invention also provides an application of the in-situ nano-scale thick zinc oxide@zinc negative electrode, which is used as a negative electrode to prepare a zinc battery.

[0054] In the present invention, the in-situ nano-scale thick zinc oxide@zinc negative electrode described in the present invention can be used as a negative electrode, and the required zinc battery can be prepared based on conventional ideas and principles.

[0055] In the present invention, the zinc battery is an aqueous zinc ion battery.

[0056] The present invention also provides a zinc battery, which comprises the in-situ nano-scale thick zinc oxide@zinc negative electrode.

[0057] The zinc battery of the present invention, except for the in-situ nano-scale thick zinc oxide@zinc negative electrode, other components and parts can be conventional.

[0058] Beneficial Effects

[0059] 1. The present invention provides a new in-situ nano-scale zinc oxide thick zinc negative electrode, which has excellent activity, interface stability, water corrosion resistance, structural stability and zinc ion conductivity, can adapt to the application requirements under high discharge depth and high current, and can improve its performance under high discharge depth and high current.

[0060] 2. The present invention innovatively pre-treats the zinc substrate with acid and oxidizing atmosphere, then performs modification treatment according to formula 1, and then cooperates with the subsequent T1 / T2 combined heat treatment. This can unexpectedly form a nano-scale ultra-thin zinc oxide layer in situ on the surface of the zinc substrate and optimize the microscopic physicochemical structure of the material. In this way, a zinc negative electrode with excellent activity and adapted to high discharge depth and large current application requirements can be prepared.

[0061] The method of the invention can obtain a zinc electrode with a stable coating, and the new material can show stability under high current density and large surface capacity. BRIEF DESCRIPTION OF THE DRAWINGS

[0062] Figure 1 This is the XPS etching spectrum of the zinc electrode finally prepared in Example 1;

[0063] Figure 2 This is the Zn2p track XPS etching spectrum of the in-situ nanoscale thick zinc oxide@zinc negative electrode finally prepared in Example 1.

[0064] Figure 3 This is a long cycle test chart of the symmetrical battery assembled with in-situ nano-scale thick zinc oxide@zinc negative electrode finally prepared in Example 1 at 10mA / cm2-10mAh / cm2. DETAILED DESCRIPTION

[0065] The present invention will be further described in detail below in conjunction with specific embodiments, but the present invention is not limited to the following embodiments.

[0066] In the present invention, the compound of formula 1 can be It is obtained based on a simple amidation reaction.

[0067] In the present invention, for the modification of the present invention, there is no requirement for the chirality of the compound of formula 1.

[0068] Embodiment 1:

[0069] ① Take 100 ml of 0.1 mol / l dilute hydrochloric acid, take 5 g of ultra-pure zinc foil with a thickness of 50 μm and immerse it in the dilute hydrochloric acid, control the ambient temperature to 30°C, etch for 1 hour, wash with pure water and anhydrous ethanol successively, and place in an oven to dry.

[0070] ② The product of step ① is placed in a tube furnace under an oxidizing atmosphere (in this case, a mixed atmosphere of oxygen and argon, with a ratio of oxygen to argon of 1:1), heated to 90°C, kept warm for 1.75 hours, and then naturally cooled to room temperature.

[0071] ③ Take 0.25g of additive (Formula 1-A, ) was dissolved in 250 ml of solvent (ultrapure water), recorded as liquid A. The product of step ② was soaked in 250 ml of liquid A, and the ambient temperature was controlled at 28°C. After soaking for 25 hours, it was washed with water and dried.

[0072] ④ The product of step ③ is placed in a tubular furnace under a protective atmosphere (argon atmosphere in this case), heated to 140°C (marked as T1), kept warm for 3.5 hours (marked as t1), then heated to 300°C (marked as T2) at a heating rate of 3°C / min, kept warm for 1.5 hours (marked as t2), and then naturally cooled to room temperature to obtain the ultra-thin zinc electrode with zinc oxide coating.

[0073] The zinc oxide of the electrode of the present invention has a thickness of only nanometers (100 to 500 nm) and is Figure 1 and Figure 2 From the XPS graph, it can be seen that there is a strong chemical interaction between the in-situ formed zinc oxide and the zinc substrate.

[0074] Half-cell assembly and performance determination:

[0075] In the atmosphere, zinc electrode, glass fiber separator, prepared zinc electrode, and nickel foam were sequentially assembled into a CR2025 button battery, and a zinc ion battery electrolyte containing 2 mol / l zinc sulfate was added, and finally sealed using a battery packaging machine. At 25°C, a current density of 1 mA / cm 2 , with a surface capacity of 1 mAh / cm 2 and a current density of 10 mA / cm 2 , surface capacity is 10 mAh / cm 2 The assembled symmetrical battery was charged and discharged to explore the electrochemical properties of the material. The test instrument was the Blue Electric electrochemical measurement system.

[0076] Embodiment 2:

[0077] Compared with Example 1, the only difference is that the conditions of step ① are changed, and the other operations and parameters are the same as Example 1. The experimental groups are:

[0078] Group A: the hydrochloric acid concentration was changed to 0.3 mol / l, and the etching time was the same as in Example 1;

[0079] Group B: the hydrochloric acid concentration was changed to 0.05 mol / l, and the etching time was the same as in Example 1;

[0080] Group C: the inorganic acid was changed to sulfuric acid, and other conditions were the same as those in Example 1;

[0081] Group D: The operating temperature during treatment was changed to 60°C, the treatment time was changed to 0.25h, and the other conditions were the same as in Example 1.

[0082] Other operations and parameters are the same as in Example 1.

[0083] Embodiment 3:

[0084] Compared with Example 1, the only difference is that the conditions of step ② are changed, and the other operations and parameters are the same as Example 1. The experimental groups are:

[0085] Group A: The ratio of oxygen to protective gas was changed to 1:9, and other conditions were the same as those in Example 1;

[0086] Group B: The ratio of oxygen to protective gas was changed to 9:1, and other conditions were the same as those in Example 1;

[0087] Group C: the treatment temperature was changed to 50°C, the treatment time was changed to 0.5h, and the other conditions were the same as those in Example 1;

[0088] Other operations and parameters are the same as in Example 1.

[0089] Embodiment 4:

[0090] Compared with Example 1, the only difference is that the conditions of step ③ are changed, and the other operations and parameters are the same as Example 1. The experimental groups are:

[0091] Group A: Change the additive to Formula 1-B The amount of additives used is the same as in Example 1;

[0092] Group B: Change the additive to Formula 1-C The amount of additives used is the same as in Example 1;

[0093] Group C: Change the additive to Formula 1-D The amount of additives used is the same as in Example 1;

[0094] Group D: In liquid A, the addition amount of formula 1-A was changed to 2.5 g, the concentration in liquid A was 10 mg / ml, the treatment time was 5 h, and the other conditions were the same as in Example 1.

[0095] Other operations and parameters are the same as in Example 1.

[0096] Example 5

[0097] Compared with Example 1, the only difference is that the conditions of step ④ are changed, and the other operations and parameters are the same as Example 1. The experimental groups are:

[0098] Group A: T1 is 80°C, t1 is 4h, T2 is 380°C, t2 is 1h, and other operations and parameters are the same as those in Example 1;

[0099] Group B: T1 is 125°C, t1 is 3h, T2 is 230°C, t2 is 3h, and other operations and parameters are the same as those in Example 1;

[0100] Other operations and parameters are the same as in Example 1.

[0101] Comparative Example 1:

[0102] The other conditions and steps are consistent with those in Example 1, except that the etching step in step 1 is omitted, and the zinc substrate in step 1 is directly subjected to step 2 and subsequent treatments. The other processes and test conditions are the same as those in Example 1.

[0103] Comparative Example 2:

[0104] The other conditions and steps are consistent with those in Example 1, except that the pre-oxidation step in step 2 is omitted, and the zinc foil treated in step 1 is directly subjected to step 3 and subsequent treatments. The other processes and test conditions are the same as those in Example 1.

[0105] Comparative Example 3:

[0106] The other conditions and steps are consistent with those in Example 1, except that the modification treatment in step 3 is omitted, and the product in step 2 is directly subjected to the treatment in step 4. The other processes and test conditions are the same as those in Example 1.

[0107] Comparative Example 4:

[0108] The other conditions and steps are consistent with those in Example 1, with the only difference being that, in step 4, the insulation process of T1 is omitted, and the insulation treatment at temperature T2 is directly performed, and the insulation time is the same as the total heat treatment time in Example 1, and the other operations and parameters are the same as those in Comparative Example 2.

[0109] Comparative Example 5:

[0110] The other conditions and steps are consistent with those in Example 1, except that in step 4, the heat preservation process of T2 is missing, and only the heat preservation treatment at temperature T1 is performed, and the heat preservation time is the same as the total heat treatment time of Example 1. Other processes and test conditions are the same as those in Example 1.

[0111] Comparative Example 6:

[0112] The other conditions and steps are the same as those in Example 1, except that step 4 is omitted, and the product of step 3 is directly used as the electrode. The other processes and test conditions are the same as those in Example 1.

[0113] Comparative Example 7:

[0114] The other conditions and steps are the same as those in Example 1, except that the additive is changed to Other process and test conditions are the same as in Example 1.

[0115] Table 1: Examples and Comparative Examples at a current density of 1 mA / cm 2 , with a surface capacity of 1 mAh / cm 2 Test results

[0116]

[0117]

[0118] Table 2: Examples and Comparative Examples at a current density of 10 mA / cm 2 , surface capacity is 10 mAh / cm 2 Test results

[0119]

[0120]

[0121] In summary, the technical solution of the present application has excellent high surface load and cycle stability under large current.

Claims

1. An in-situ nano-scale thick zinc oxide @ zinc negative electrode, characterized in that: The invention comprises a zinc substrate and a zinc oxide layer with a nanometer thickness in-situ compounded on the surface of the zinc substrate.

2. The in-situ nanoscale thick zinc oxide@zinc negative electrode as claimed in claim 1, characterized in that: There is a chemical reaction between the zinc substrate and the zinc oxide layer; Preferably, the zinc substrate is an ultra-thin zinc foil with a thickness between 10 and 50 μm; Preferably, the crystal form of zinc oxide is a wurtzite structure; Preferably, the thickness of the zinc oxide layer is 100-500 nm.

3. A method for preparing an in-situ nano-thick zinc oxide@zinc negative electrode according to any one of claims 1 to 2, characterized in that: The zinc substrate is pre-etched with an acid solution, and then heated in an oxidizing atmosphere for surface pre-oxidation to obtain a pre-treated zinc substrate; Immersing the pretreated zinc substrate in a modification solution containing the compound of formula 1 for surface modification to obtain a modified zinc substrate; The modified zinc substrate is then subjected to a first heat preservation treatment at a temperature T1, and then subjected to a second heat preservation treatment at a temperature T2, thereby obtaining the in-situ nano-scale thick zinc oxide@zinc negative electrode; The R1 is a C1-C6 alkyl or substituted alkyl; the R2 is H, amino, substituted amino or sulfonic acid; the R3 is amino or sulfonic acid; the R4 is H, hydroxyl or a C1-C6 alkyl; the Ar is an aromatic ring; The 50≤T1<200℃; the temperature T2 is 200~400℃.

4. The method for preparing the in-situ nano-scale thick zinc oxide@zinc negative electrode as claimed in claim 3, characterized in that: The thickness of the zinc substrate is controlled between 10 and 60 μm; Preferably, the acid solution is an aqueous solution of an inorganic acid; the inorganic acid preferably includes at least one of sulfuric acid, hydrochloric acid, and nitric acid; Preferably, the concentration of the inorganic acid in the acid solution is 0.05 to 5 mol / l, preferably 0.1 to 0.4 mol / l; Preferably, the temperature of the surface etching treatment stage is 25 to 65° C.; the surface etching time is 0.2 to 2 hours; Preferably, the liquid-to-solid ratio of the acid solution to the zinc substrate is 1-50 ml / g.

5. The method for preparing the in-situ nano-scale thick zinc oxide@zinc negative electrode as claimed in claim 3, characterized in that: The oxidizing atmosphere is an atmosphere containing oxygen, preferably at least one of oxygen and an oxygen-diluent mixed gas; Preferably, the diluent gas includes at least one of nitrogen and an inert gas; Preferably, the oxygen content in the oxidizing atmosphere is above 10%, preferably 10% to 90%, preferably 45% to 55%; Preferably, the temperature of the surface pre-oxidation treatment is 45°C to 100°C, preferably 75°C to 95°C; Preferably, the surface pre-oxidation treatment time is 0.5 h to 3 h, preferably 1.5 h to 2 h.

6. The method for preparing the in-situ nano-scale thick zinc oxide@zinc negative electrode as claimed in claim 3, characterized in that: In the formula 1, R1 is a C1-C6 alkyl group; Preferably, said R2 is H, amino or sulfonic acid; Preferably, the R3 is an amino group or a sulfonic acid group; Preferably, said R4 is H; Preferably, Ar is a benzene ring or a benzene ring with a substituent; the substituent includes at least one of halogen, C1-C6 alkyl, C1-C6 alkoxy, hydroxyl, nitro, trifluoromethyl, and ester.

7. The method for preparing an in-situ nanoscale thick zinc oxide@zinc negative electrode as claimed in claim 3 or 6, characterized in that: In the modified liquid, the concentration of Formula 1 is above 0.5 mg / ml, preferably above 0.5 mg / ml, and further 1 to 8 mg / ml; Preferably, the weight ratio of Formula 1 to the zinc substrate in the modified solution is 0.01 to 2:1; Preferably, the temperature in the modification stage is 20 to 40°C; Preferably, the modification treatment time is more than 5 hours, preferably 12 to 36 hours.

8. The method for preparing the in-situ nano-scale thick zinc oxide@zinc negative electrode as claimed in claim 3, characterized in that: The first and second heat preservation processes are carried out in a protective atmosphere; Preferably, the protective atmosphere comprises at least one of nitrogen and an inert gas; Preferably, the temperature T1 is 75 to 150°C, preferably 130 to 145°C; Preferably, the temperature T2 is 220-380°C, further 280-320°C; Preferably, the first insulation time t1 is 2 to 5 hours; Preferably, the second insulation time t2 is 1 to 5 hours.

9. An application of the in-situ nano-scale thick zinc oxide @ zinc negative electrode as claimed in any one of claims 1 to 2 or the in-situ nano-scale thick zinc oxide @ zinc negative electrode prepared by the preparation method as claimed in any one of claims 3 to 8, characterized in that: It is used as negative electrode to prepare zinc battery; Preferably, the zinc battery is an aqueous zinc ion battery.

10. A zinc battery, characterized in that: It comprises the in-situ nanoscale thick zinc oxide @ zinc negative electrode described in any one of claims 1 to 2 or the in-situ nanoscale thick zinc oxide @ zinc negative electrode prepared by the preparation method described in any one of claims 3 to 8.

Citation Information

Patent Citations

  • Preparation method of zinc negative electrode organic polymer-metal copper composite coating

    CN118281229A

  • Zinc negative electrode protected by eggshell membrane-polymer composite material as well as preparation method and application of zinc negative electrode

    CN118398751A