Ferric fluoride and iron-silicon alloy composite negative electrode and preparation method thereof
Through the preparation of composite negative electrode of iron fluoride and ferrosilicon alloy, ball milling method and fluorination treatment technology, the insufficient performance of graphite and silicon-based materials in lithium-ion batteries was solved, and the improvement of high cycle and rate performance and cost reduction were achieved. .
Patent Information
- Application Number
- CN202410806094.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-21
- Publication Date
- 2024-11-08
AI Technical Summary
In the existing lithium-ion battery, graphite negative electrode materials have problems such as capacity attenuation, material structure collapse and poor conductivity during rapid charging and discharging, which limits its application. The cyclic performance of silicon-based materials is also subject to volume effects, structural damage and conductivity. Inhomogeneity influence.
The iron fluoride and ferrosilicon alloy composite negative electrode is used to alloy nanosilicon and nanoferrous through ball milling to form a ferrosilicon alloy, and the iron fluoride film coating is formed on its surface by hydrogen fluoride treatment, which improves the circulation and rate performance of the material. .
Improved long-term cycle stability and high rate performance at high current density is achieved, maintaining about 100% Coulomb efficiency and reducing preparation costs.
Smart Images

Figure CN118919638A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of lithium ion secondary battery preparation methods, and specifically relates to a composite negative electrode of ferric fluoride and iron-silicon alloy, and also relates to a preparation method of the composite negative electrode of ferric fluoride and iron-silicon alloy. Background Art
[0002] Commercial lithium-ion batteries generally use graphite materials as negative electrodes, which have a theoretical specific capacity of only 372mAh / g, and the graphite layer peels off during rapid charge and discharge, resulting in significant capacity decay. In addition, the lithium insertion potential of graphite negative electrode materials is close to the lithium precipitation potential. After being assembled into a battery pack, some single cells are prone to lithium dendrites during rapid charge and discharge. These factors seriously restrict its application in power lithium-ion batteries. Therefore, using other materials to replace graphite negative electrodes has become the focus of lithium-ion battery research.
[0003] Therefore, a lot of research has turned to finding new negative electrode material systems that can replace carbon materials, among which silicon is an ideal candidate material because it not only has a high lithium storage capacity, but is also extremely abundant in the earth. However, the low first coulomb efficiency and extremely poor cycle performance of silicon materials limit its practical application. In summary, there are three main reasons that hinder silicon-based materials from being used as negative electrode materials for lithium-ion batteries: first, the serious volume effect of silicon during the charge and discharge cycle leads to the collapse of the material structure; second, the irreversible transformation of silicon from a crystalline state to a disordered state during the lithium insertion and extraction process causes serious damage to the structure of the material; third, silicon has poor electrical conductivity and uneven reaction with lithium, which reduces the cycle performance of silicon materials. In recent years, battery workers have carried out a lot of research on silicon-based materials. Silicon alloys have become a hot spot in the research of silicon powder-based composite materials due to their high volume energy density. However, since these alloys do not fully utilize the synergistic effect of multiple metals, although these alloy materials have greatly improved their electrochemical properties compared with pure silicon, the improvement in cycle performance is still very limited. Summary of the invention
[0004] The purpose of the present invention is to provide a composite negative electrode of ferric fluoride and iron-silicon alloy, which has higher cycle and rate performance.
[0005] Another object of the present invention is to provide a method for preparing a composite negative electrode of iron fluoride and iron-silicon alloy.
[0006] The first technical solution adopted by the present invention is a composite negative electrode of ferric fluoride and iron-silicon alloy, including nano-silicon, nano-iron and iron-fluoride coating layer. Nano-silicon and nano-iron are alloyed by ball milling process to make silicon and iron form iron-silicon alloy. Hydrogen fluoride is used as fluorine source to fluorinate the iron-silicon alloy powder to form a silicon-iron alloy / fluorine composite negative electrode with an iron fluoride film coating layer on the surface.
[0007] The second technical solution adopted by the present invention is a method for preparing a composite negative electrode of ferric fluoride and iron-silicon alloy, which is specifically implemented in the following steps:
[0008] Step 1: Mix silicon powder and iron powder evenly and place them in a stainless steel ball mill for ball milling, and then add deionized water;
[0009] Step 2: ball milling at high speed to obtain alloy powder;
[0010] Step 3: heat-treating the alloy powder obtained in step 2, and then heating it in an argon-hydrogen atmosphere for heat treatment, and cooling it down to room temperature to obtain an iron-silicon alloy powder;
[0011] Step 4: fluoriding the iron-silicon alloy powder, taking a sample and placing it in a tube furnace, introducing hydrogen fluoride gas, and fluoriding the powder to obtain a composite negative electrode material of iron fluoride and iron-silicon alloy.
[0012] Another technical solution of the present invention is characterized in that:
[0013] The mass ratio of silicon powder to iron powder in step 1 is 1:1-2. During the ball milling process, the ball-to-material ratio is 50:1, and 10 ml of deionized water is added dropwise.
[0014] In step 2, the ball milling speed is 200 r / min and the ball milling time is 15-20 h.
[0015] In step 3, the alloy powder is dried in a vacuum drying oven for 12 hours.
[0016] In step 3, the alloy powder is heated to 700° C. in an argon-hydrogen atmosphere and kept at this temperature for 2 h.
[0017] In step 4, take an appropriate amount of sample and place it in a tube furnace, introduce hydrogen fluoride gas, raise the temperature to 200-380° C. and keep it for 1-5 minutes, and cool it with the furnace.
[0018] The beneficial effects of the present invention are:
[0019] The present invention successfully modified silicon materials by ball milling to prepare high-quality iron-silicon alloy / fluorine composite materials. The material showed very good performance in battery performance tests. -1 After 300 cycles, the battery can still provide a capacity of 600 mA h g-1 at a current density of 2000 mA h g-1. After 300 cycles, the battery can still maintain a coulombic efficiency of about 100%, even at a current density of 2000 mA g-1. -1 At high current density, it still provides more than 500mA hg -1capacity. In addition, the modified silicon negative electrode material shows very good rate performance. At the same time, the material is mainly prepared by ball milling process, and the preparation cost is extremely low, which provides convenience for future practical promotion and application. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 This is a SEM image of the iron-silicon alloy powder obtained in step 2 of the present invention;
[0021] Figure 2 This is a SEM image of the iron-silicon alloy @ ferrous fluoride active material obtained in step 5 of the present invention;
[0022] Figure 3 The SiFe@FeF 3 Long cycle performance diagram of the material measured at a current density of 2A / g;
[0023] Figure 4 The SiFe@FeF 3 The first cycle charge and discharge curve of the material measured at a current density of 0.1A / g. DETAILED DESCRIPTION
[0024] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.
[0025] The present invention provides a composite negative electrode of ferric fluoride and iron-silicon alloy, comprising nano-silicon, nano-iron and an iron-fluoride coating layer. The nano-silicon and nano-iron are alloyed by a ball milling process so that silicon and iron form an iron-silicon alloy. The iron-silicon alloy powder is fluorinated by using hydrogen fluoride as a fluorine source to form a silicon-iron alloy / fluorine composite negative electrode with an iron fluoride film coating layer on the surface.
[0026] The present invention also provides a method for preparing a composite negative electrode of ferric fluoride and iron-silicon alloy, which is specifically implemented according to the following steps:
[0027] Step 1: Mix silicon powder and iron powder evenly and place them in a stainless steel ball mill for ball milling, and then add deionized water;
[0028] The mass ratio of silicon powder to iron powder in step 1 is 1:1-2. During the ball milling process, the ball-to-material ratio is 50:1. 10 ml of deionized water is added dropwise.
[0029] Step 2: ball milling at high speed to obtain alloy powder;
[0030] In step 2, the ball milling speed is 200 r / min and the ball milling time is 15-20 h;
[0031] Step 3: heat-treating the alloy powder obtained in step 2, and then heating it in an argon-hydrogen atmosphere for heat treatment, and cooling it down to room temperature to obtain an iron-silicon alloy powder;
[0032] In step 3, the alloy powder is dried in a vacuum drying oven for 12 h;
[0033] In step 3, the alloy powder is heated to 700°C in an argon-hydrogen atmosphere and kept at this temperature for 2 hours;
[0034] Step 4: fluoriding the iron-silicon alloy powder, taking a sample and placing it in a tube furnace, introducing hydrogen fluoride gas, and fluoriding the powder to obtain a composite negative electrode material of iron fluoride and iron-silicon alloy;
[0035] In step 4, take an appropriate amount of sample and place it in a tube furnace, introduce hydrogen fluoride gas, raise the temperature to 200-380° C. and keep it for 1-5 minutes, and cool it with the furnace.
[0036] The present invention firstly mixes silicon powder and iron powder uniformly, and then pre-treats them by ball milling process to obtain iron-silicon alloy powder. Then, the obtained iron-silicon alloy powder is heat-treated in an argon-hydrogen atmosphere to improve its crystal structure and intrinsic performance. Finally, the heat-treated iron-silicon alloy is fluorinated to obtain silicon negative electrode material.
[0037] The material of the present invention is made of an iron-silicon alloy, which can improve the cycle and rate performance of silicon negative electrode materials. During the experiment, it was found that when the iron-silicon alloy that had only been heat-treated was used as a silicon-based negative electrode material, its electrochemical performance was not ideal. However, when the material was fluorinated, the cycle life of the silicon-based negative electrode material was significantly improved.
[0038] The negative electrode of the lithium ion battery adopts the composite negative electrode material of ferrous fluoride and iron-silicon alloy of the present invention.
[0039] The fluorination treatment in the present invention is to use hydrogen fluoride as a fluorinating agent and perform the fluorination treatment in a tube furnace to obtain Si / AlF 3 Composite material. Its fluorination treatment will form a dense iron fluoride film on the surface of the negative electrode material. Whether the outer layer of silicon is covered with an iron fluoride film may affect the electrochemical properties of the silicon negative electrode material, in order to make the silicon negative electrode material have better electrochemical properties.
[0040] Comparative Example 1
[0041] Step 1: Take 300 mg of silicon powder and 300 mg of iron powder, mix them evenly and place them in a stainless steel ball mill, add 30 g of stainless steel ball mill beads, and add 10 ml of deionized water.
[0042] Step 2: Ball mill at 500 r / min for 15 h to obtain alloy powder.
[0043] Step 3: Place the powder obtained in step 2 in a vacuum drying oven and dry for 12 hours, then heat it to 700°C in an argon-hydrogen atmosphere and keep it at that temperature for 2 hours, and cool it down to room temperature to obtain iron-silicon alloy powder.
[0044] Step 4: Forming the heat-treated iron-silicon alloy powder into electrodes.
[0045] Example 2
[0046] Step 1: Take 200 mg of silicon powder and 400 mg of iron powder, mix them evenly and place them in a stainless steel ball mill, add 30 g of stainless steel ball mill beads, and add 10 ml of deionized water.
[0047] Step 2: Ball mill at 400 r / min for 15 h to obtain alloy powder.
[0048] Step 3: Place the powder obtained in step 2 in a vacuum drying oven and dry for 12 hours, then heat it to 700°C in an argon-hydrogen atmosphere and keep it at that temperature for 2 hours, and cool it down to room temperature to obtain iron-silicon alloy powder.
[0049] Step 4: After the heat-treated iron-silicon alloy powder is made into an electrode, the charge-discharge curve is measured at a current density of 0.1A / g. Figure 4 shown.
[0050] Example 1
[0051] Step 1: Mix 300 mg of silicon powder and 300 mg of iron powder evenly in a stainless steel ball mill, set the ball-to-material ratio to 50:1, add 5.5 g of stainless steel ball mill beads, and drop 10 ml of deionized water;
[0052] Step 2: Ball milling at 200 r / min for 20 h to obtain alloy powder, such as Figure 1 As shown;
[0053] Step 3: The powder obtained in step 2 is placed in a vacuum drying oven and dried for 12 hours, then heated to 700° C. in an argon-hydrogen atmosphere and kept at this temperature for 2 hours, and then cooled to room temperature to obtain an iron-silicon alloy powder;
[0054] Step 4: The heat-treated iron-silicon alloy powder is subjected to fluorination treatment. Take an appropriate amount of sample and place it in a tube furnace, introduce hydrogen fluoride gas, heat it to 200°C and keep it for 3 minutes, and cool it with the furnace to prepare a composite negative electrode material of iron fluoride and iron-silicon alloy, such as Figure 2 shown.
[0055] After the iron fluoride and iron-silicon alloy composite negative electrode material powder was made into an electrode, the charge and discharge curves were measured at a current density of 2A / g. Figure 3 shown.
[0056] Example 2
[0057] Step 1: Mix 200 mg silicon powder and 400 mg iron powder evenly in a stainless steel ball mill, set the ball-to-material ratio to 50:1, add 30 g stainless steel ball mill beads, and drop 10 ml deionized water;
[0058] Step 2: ball milling at 200 r / min for 15 h to obtain alloy powder;
[0059] Step 3: The powder obtained in step 2 is placed in a vacuum drying oven and dried for 12 hours, then heated to 800° C. in an argon-hydrogen atmosphere and kept at that temperature for 4 hours, and then cooled to room temperature to obtain an iron-silicon alloy powder;
[0060] Step 4: The heat-treated iron-silicon alloy powder is subjected to fluorination treatment. An appropriate amount of sample is placed in a tube furnace, hydrogen fluoride gas is introduced, the temperature is raised to 200°C and kept for 1 minute, and the furnace is cooled to prepare a composite negative electrode material of iron fluoride and iron-silicon alloy.
[0061] Example 3
[0062] Step 1: Mix 300 mg of silicon powder and 300 mg of iron powder evenly in a stainless steel ball mill, set the ball-to-material ratio to 50:1, add 30 g of stainless steel ball mill beads, and drop 10 ml of deionized water;
[0063] Step 2: ball milling at 200 r / min for 15 h to obtain alloy powder;
[0064] Step 3: The powder obtained in step 2 is placed in a vacuum drying oven and dried for 12 hours, then heated to 700° C. in an argon-hydrogen atmosphere and kept at this temperature for 4 hours, and then cooled to room temperature to obtain an iron-silicon alloy powder;
[0065] Step 4: The heat-treated iron-silicon alloy powder is subjected to fluorination treatment. An appropriate amount of sample is placed in a tubular furnace, hydrogen fluoride gas is introduced, the temperature is raised to 380°C and kept for 5 minutes, and the furnace is cooled to prepare a composite negative electrode material of iron fluoride and iron-silicon alloy.
[0066] The present invention forms an alloy with active material nano-silicon and lithium-philic metal iron with good ductility and conductivity, and forms a dense iron fluoride coating layer on the surface of the iron-silicon alloy by fluorination treatment, thereby alleviating the volume expansion of the silicon nano-particles encapsulated therein during the lithium storage process, thereby improving the utilization rate of the active material. After the silicon-iron alloy@iron fluoride composite negative electrode is prepared into an electrode, in the battery structure, the iron fluoride coating layer on the surface of the composite negative electrode material will react with the electrolyte to induce the generation of lithium fluoride, the main substance in the solid electrolyte membrane, so that the effect of artificially regulating the solid electrolyte membrane can be achieved, effectively solving the performance attenuation problem caused by the breakage and reconstruction of the solid electrolyte membrane during the battery charging and discharging process.
Claims
1. A composite negative electrode of ferric fluoride and iron-silicon alloy, characterized in that: The invention comprises nano-silicon, nano-iron and ferric fluoride coating layers. Nano-silicon and nano-iron are alloyed by ball milling process so that silicon and iron form iron-silicon alloy. Hydrogen fluoride is used as fluorine source to fluorinate the iron-silicon alloy powder so as to form a silicon-iron alloy / fluorine composite negative electrode having an iron fluoride film coating layer on the surface.
2. A method for preparing a composite negative electrode of ferric fluoride and iron-silicon alloy, characterized in that: Please follow the steps below to implement: Step 1: Mix silicon powder and iron powder evenly and place them in a stainless steel ball mill for ball milling, and then add deionized water; Step 2: ball milling at high speed to obtain alloy powder; Step 3: heat-treating the alloy powder obtained in step 2, then heating it in an argon-hydrogen atmosphere, and cooling it to room temperature to obtain an iron-silicon alloy powder; Step 4: fluoriding the iron-silicon alloy powder, taking a sample and placing it in a tube furnace, introducing hydrogen fluoride gas, and fluoriding the powder to obtain a composite negative electrode material of iron fluoride and iron-silicon alloy.
3. The method for preparing the ferric fluoride and iron-silicon alloy composite negative electrode according to claim 2, characterized in that: The mass ratio of silicon powder to iron powder in step 1 is 1:1-2. During the ball milling process, the ball-to-material ratio is 50:1, and 10 ml of deionized water is added dropwise.
4. The method for preparing the ferric fluoride and iron-silicon alloy composite negative electrode according to claim 2, characterized in that: In step 2, the ball milling speed is 200 r / min, and the ball milling time is 15-20 h.
5. The method for preparing the ferric fluoride and iron-silicon alloy composite negative electrode according to claim 2, characterized in that: In the step 3, the alloy powder is dried in a vacuum drying oven for 12 hours.
6. The method for preparing the ferric fluoride and iron-silicon alloy composite negative electrode according to claim 2, characterized in that: In step 3, the alloy powder is heated to 700° C. in an argon-hydrogen atmosphere and kept at this temperature for 2 hours.
7. The method for preparing the ferric fluoride and iron-silicon alloy composite negative electrode according to claim 2, characterized in that: In step 4, a proper amount of sample is placed in a tubular furnace, hydrogen fluoride gas is introduced, the temperature is raised to 200-380° C., the temperature is maintained for 1-5 minutes, and the furnace is cooled.