Three-dimensional self-supporting electrode, preparation method thereof and lithium ion battery
By forming carbon-covered nano Fe3O4 in situ on a three-dimensional self-supporting substrate, the problem of the electrochemical performance of Fe3O4 electrode material due to volume expansion is solved, the energy density and cycle stability of lithium-ion batteries are improved, and more efficient electrons are achieved /ion transport.
Patent Information
- Application Number
- CN202410972663.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-19
AI Technical Summary
The irreversible volume expansion of the Fe3O4 electrode material during the lithium ion embedding/detachment process caused by changes in the crystal structure, which affects the electrochemical performance. The lower theoretical specific capacity of graphite materials limits the high energy density application of lithium ion batteries.
Carbon-coated nanoFe3O4 is formed in situ on the three-dimensional self-supporting substrate, and a three-dimensional self-supporting electrode is prepared by hydrothermal reaction of resorcinol, formaldehyde and iron-containing compounds, simplifying the process and improving the interaction between nanoFe3O4 and the conductive substrate , improve electron/ion transport performance.
Effectively reduce the agglomeration and accumulation of nano-Fe3O4, improve the active site and cyclic stability of electrode materials, buffer the volume changes of lithium ion embedding and detachment, enhance the utilization efficiency and electron mobility of active materials, and improve the lithium ion battery. energy density and rate performance.
Smart Images

Figure CN118919664A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of battery materials, and in particular to a three-dimensional self-supporting electrode and a preparation method thereof, and a lithium ion battery. Background Art
[0002] Lithium-ion batteries have the advantages of high energy density, long cycle life and wide operating voltage range, and are widely used as power sources for various energy storage cabinets, electronic devices and the main power source for electric vehicles. At present, graphite materials are widely used as mainstream lithium-ion battery negative electrode materials due to their advantages such as low resistivity, low price and abundant reserves. However, the theoretical specific capacity of graphite materials is low (372mAh / g), which seriously limits the application of graphite negative electrodes in high energy density devices. Therefore, finding negative electrode materials with higher energy density is one of the main tasks in the development of next-generation lithium-ion batteries. Fe3O4 has attracted widespread attention from researchers because of its high theoretical specific capacity (924mAh / g), abundant reserves and low price. However, due to the special lithium storage method of Fe3O4, the crystal structure of Fe3O4 will change during the lithium ion insertion / extraction process, resulting in irreversible volume expansion, which seriously affects the electrochemical performance of lithium batteries. Therefore, it is necessary to explore a new type of Fe3O4 electrode material. Summary of the invention
[0003] In order to overcome the above-mentioned shortcomings and deficiencies of the prior art, the object of the present invention is to provide a method for preparing a three-dimensional self-supporting electrode, in situ forming carbon-coated nano-Fe3O4 on a three-dimensional self-supporting substrate, the preparation process is simple, and the in situ formed carbon-coated nano-Fe3O4 helps to increase the interaction between the nano-Fe3O4 active material and the conductive substrate, which can further improve the electron / ion transport performance inside the nano-Fe3O4 material and at its interface with the electrolyte.
[0004] Another object of the present invention is to provide a three-dimensional self-supporting electrode prepared by the above preparation method.
[0005] Another object of the present invention is to provide a lithium ion battery based on the above three-dimensional self-supporting electrode.
[0006] The purpose of the present invention is achieved through the following technical solutions:
[0007] The present invention provides a method for preparing a three-dimensional self-supporting electrode, comprising the following steps:
[0008] Dissolving resorcinol and formaldehyde in a mixed solution of ethanol and water, adding ammonia water, and stirring until fully mixed to obtain an organic polymer solution;
[0009] Adding an iron-containing compound to an organic polymer solution and stirring until fully dissolved to obtain a precursor solution; transferring the solution to a reaction kettle, placing a three-dimensional conductive substrate in the reaction kettle for hydrothermal reaction to obtain a three-dimensional self-supporting substrate containing an iron / carbon precursor; the iron-containing compound is at least one of ferric chloride, ferric nitrate nonahydrate, ferric sulfate and ferric citrate;
[0010] The three-dimensional self-supporting substrate containing the iron / carbon precursor is dried and then annealed in an inert atmosphere, and then naturally cooled to room temperature to obtain a three-dimensional self-supporting electrode loaded with in-situ carbon-coated nano-Fe3O4.
[0011] Preferably, the three-dimensional conductive substrate is foamed Ni, foamed Cu or activated carbon cloth.
[0012] Preferably, the mass volume ratio of resorcinol to formaldehyde is (1-5) g: (1-4) ml.
[0013] Preferably, the mass ratio of the iron-containing compound to the resorcinol is (1.5-2.5):0.1.
[0014] Preferably, the reaction conditions of the hydrothermal reaction are: reaction temperature is 160-200° C., and reaction time is 8-12 h.
[0015] Preferably, the annealing treatment is specifically as follows: the annealing temperature is 400-800°C, the annealing time is 1-3h, and the heating rate is 5-10°C / min.
[0016] Preferably, the inert atmosphere is at least one of N2 and Ar.
[0017] Preferably, placing the three-dimensional conductive substrate in the reaction kettle comprises:
[0018] The three-dimensional conductive substrate is placed in the reaction kettle, and the three-dimensional conductive substrate is at an angle of 40 to 50 degrees with the liquid surface of the precursor solution.
[0019] Preferably, the volume ratio of ethanol to water is 1:(1-3).
[0020] Preferably, the three-dimensional conductive substrate is pretreated as follows:
[0021] The three-dimensional conductive substrate is immersed in an acid, and then ultrasonically rinsed with deionized water and ethanol for multiple times and dried to obtain a clean conductive substrate after treatment and activation; more preferably, the acid is hydrochloric acid, sulfuric acid or nitric acid, and the concentration is 2-4M; the immersion time is 10-30min; and the drying temperature is 30-80°C.
[0022] Preferably, the mass volume ratio of resorcinol to ammonia water is: (0.1-0.5) g: (0.3-0.5) ml.
[0023] The present invention also provides a three-dimensional self-supporting electrode, which is prepared by the preparation method of the three-dimensional self-supporting electrode.
[0024] The present invention also provides a lithium ion battery using the three-dimensional self-supporting electrode as a negative electrode.
[0025] Compared with the prior art, the present invention has the following advantages and beneficial effects:
[0026] (1) The preparation method of the three-dimensional self-supporting electrode of the present invention forms carbon-coated nano-Fe3O4 in situ on the three-dimensional self-supporting substrate. The preparation process is simple, and the in-situ formed carbon-coated nano-Fe3O4 helps to increase the interaction between the nano-Fe3O4 active material and the conductive substrate, which can further improve the electron / ion transmission performance inside the nano-Fe3O4 material and at its interface with the electrolyte.
[0027] (2) The preparation method of the three-dimensional self-supporting electrode of the present invention mainly comprises the following steps: dissolving the hydroquinone, formaldehyde and iron-containing compounds in the synthetic raw materials to form a precursor solution, and then in situ synthesizing the carbon-coated nano-Fe3O4 in one step through a hydrothermal reaction. This can effectively reduce the agglomeration and accumulation of the nano-Fe3O4 material, and improve the active sites and cycle stability of the electrode material.
[0028] (3) The preparation method of the three-dimensional self-supporting electrode of the present invention has easy-to-obtain raw materials, simple preparation process, high preparation efficiency, low cost, can be used for large-scale production, and has broad application prospects in the fields of lithium-ion battery electrodes.
[0029] (4) The three-dimensional self-supporting electrode of the present invention and the in-situ carbon-coated nano-Fe3O4 particle structure can effectively buffer the volume change and electrochemical impact of nano-Fe3O4 when lithium ions are embedded and released; and the porous structure on the three-dimensional self-supporting electrode nickel foam substrate can also help to suppress the irreversible volume expansion problem of Fe3O4 during charging and discharging.
[0030] (5) The three-dimensional self-supporting electrode of the present invention can increase the energy density of the whole battery due to its electrode structure without conductive agent and binder. In addition, since the binding force between the active material and the current collector is stronger and more uniform, and there is no dead volume, the utilization efficiency of the active material can be further improved, and the electron mobility is higher.
[0031] (6) The three-dimensional self-supporting electrode of the present invention can increase the contact area between the active material and the electrolyte, which is beneficial to the transmission of ions, shortens the diffusion path of ions, and improves the rate performance and cycle performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 X-ray diffraction patterns of the three-dimensional self-supporting electrode material loaded with in-situ carbon-coated nano-Fe3O4 obtained in Example 2 of the present invention, the Fe3O4 self-supporting electrode material obtained in Comparative Example 1, and the electrode material prepared by carbon-coated Fe3O4 coating obtained in Comparative Example 2.
[0033] Figure 2 This is a SEM scanning electron microscope image of the three-dimensional self-supporting electrode material loaded with in-situ carbon-coated nano-Fe3O4 obtained in Example 2 of the present invention.
[0034] Figure 3 This is a TEM transmission electron microscope image of the three-dimensional self-supporting electrode material loaded with in-situ carbon-coated nano-Fe3O4 obtained in Example 2 of the present invention.
[0035] Figure 4 It is a comparison chart of the rate performance curves of the three-dimensional self-supporting electrode material loaded with in-situ carbon-coated nano-Fe3O4 obtained in Examples 1-3 of the present invention and the Fe3O4 self-supporting electrode material obtained in Comparative Example 1 as negative electrode materials for lithium-ion batteries.
[0036] Figure 5 The three-dimensional self-supporting electrode material loaded with in-situ carbon-coated nano-Fe3O4 obtained in Example 2 of the present invention and the Fe3O4 self-supporting electrode material obtained in Comparative Example 1 were used as negative electrode materials for lithium-ion batteries at 5Ag. -1 Performance comparison chart of high current cycle charge and discharge 1000 times.
[0037] Figure 6 The three-dimensional self-supporting electrode material loaded with in-situ carbon-coated nano-Fe3O4 obtained in Example 2 of the present invention and the electrode material prepared by coating carbon-coated Fe3O4 obtained in Comparative Example 2 were used as negative electrode materials for lithium-ion batteries at 1A g -1 Performance comparison chart of high current cycle charge and discharge 200 times.
[0038] Figure 7 The full battery prepared by using the three-dimensional self-supporting electrode material loaded with in-situ carbon-coated nano-Fe3O4 obtained in Example 2 of the present invention as the negative electrode material of the lithium-ion battery and lithium iron phosphate as the positive electrode material is 0.1Ag -1 Performance comparison chart after 500 cycles at different current densities. DETAILED DESCRIPTION
[0039] The present invention will be further described in detail below in conjunction with the examples, but the embodiments of the present invention are not limited thereto.
[0040] Example 1
[0041] The method for preparing the three-dimensional self-supporting electrode of this embodiment comprises the following steps:
[0042] (1) The Ni foam sheet was cut into a size of 3*5 cm, then soaked in 3M hydrochloric acid for 30 min, taken out and ultrasonically cleaned in deionized water and ethanol for 3 times, and then dried in an oven at 60°C to obtain a clean Ni foam conductive substrate after activation;
[0043] (2) 0.1 g and 0.2 ml of resorcinol and formaldehyde were dissolved in 60 ml of ethanol and water solution with a volume ratio of 1:2, and 0.3 ml of ammonia water was added and stirred for 30 min to mix thoroughly.
[0044] (3) Add 1.5 g of ferric nitrate nonahydrate to step (2) and continue stirring for 30 min. Transfer the solution to a 100 ml reactor and place the Ni foam sheet treated in step (1) into the reactor at a 45° angle. The hydrothermal temperature is 180° C. The reaction time is 12 h. After natural cooling, the Ni foam sheet is dried in an oven at 60° C. to obtain a Ni foam sheet containing an iron-carbon precursor.
[0045] (4) The Ni foam sheet containing the iron-carbon precursor obtained in step (3) is further annealed at 600°C for 2h in a N2 atmosphere at a heating rate of 5°C / min. After naturally cooling to room temperature, a three-dimensional self-supporting electrode material loaded with in-situ carbon-coated nano-Fe3O4 can be obtained.
[0046] Example 2
[0047] The method for preparing the three-dimensional self-supporting electrode of this embodiment comprises the following steps:
[0048] (1) The Ni foam sheet was cut into a size of 3*5 cm, then soaked in 3M hydrochloric acid for 30 min, taken out and ultrasonically cleaned in deionized water and ethanol for 3 times, and then dried in an oven at 60°C to obtain a clean Ni foam conductive substrate after activation;
[0049] (2) 0.1 g and 0.2 ml of resorcinol and formaldehyde were dissolved in 60 ml of ethanol and water solution with a volume ratio of 1:2, and 0.3 ml of ammonia water was added and stirred for 30 min to mix thoroughly.
[0050] (3) Add 2.0 g of ferric nitrate nonahydrate to step (2) and continue stirring for 30 min. Transfer the solution to a 100 ml reactor and place the Ni foam sheet treated in step (1) into the reactor at a 45° angle. The hydrothermal temperature is 180° C. The reaction time is 12 h. After natural cooling, the Ni foam sheet is dried in an oven at 60° C. to obtain a Ni foam sheet containing an iron-carbon precursor.
[0051] (4) The Ni foam sheet containing the iron-carbon precursor obtained in step (3) is further annealed at 600°C for 2h in a N2 atmosphere at a heating rate of 5°C / min. After naturally cooling to room temperature, a three-dimensional self-supporting electrode material loaded with in-situ carbon-coated nano-Fe3O4 can be obtained.
[0052] Example 3
[0053] (1) The Ni foam sheet was cut into a size of 3*5 cm, then soaked in 3M hydrochloric acid for 30 min, taken out and ultrasonically cleaned in deionized water and ethanol for 3 times, and then dried in an oven at 60°C to obtain a clean Ni foam conductive substrate after activation;
[0054] (2) 0.1 g and 0.2 ml of resorcinol and formaldehyde were dissolved in 60 ml of ethanol and water solution with a volume ratio of 1:2, and 0.3 ml of ammonia water was added and stirred for 30 min to mix thoroughly.
[0055] (3) Add 2.5 g of ferric nitrate nonahydrate to step (2) and continue stirring for 30 min. Transfer the solution to a 100 ml reactor and place the Ni foam sheet treated in step (1) into the reactor at a 45° angle. The hydrothermal temperature is 180° C. The reaction time is 12 h. After natural cooling, the Ni foam sheet is dried in an oven at 60° C. to obtain a Ni foam sheet containing an iron-carbon precursor.
[0056] (4) The Ni foam sheet containing the iron-carbon precursor obtained in step (3) is further annealed at 600°C for 2h in a N2 atmosphere at a heating rate of 5°C / min. After naturally cooling to room temperature, a three-dimensional self-supporting electrode material loaded with in-situ carbon-coated nano-Fe3O4 can be obtained.
[0057] Comparative Example 1
[0058] This comparative example is to directly grow nano-Fe3O4 three-dimensional self-supporting electrode material in situ on the treated Ni foam sheet. The specific steps are:
[0059] (1) The Ni foam sheet was cut into a size of 3*5 cm, then soaked in 3M hydrochloric acid for 30 min, taken out and ultrasonically cleaned in deionized water and ethanol for 3 times, and then dried in an oven at 60°C to obtain a clean Ni foam conductive substrate after activation;
[0060] (2) Add 0.3 ml of aqueous ammonia to 60 ml of ethylene glycol solution and stir for 30 min to mix thoroughly.
[0061] (3) Add 2.0 g of ferric nitrate nonahydrate to step (2) and continue stirring for 30 min. Transfer the solution to a 100 ml reactor and place the Ni foam sheet treated in step (1) into the reactor at a 45° angle. The hydrothermal temperature is 180° C. The reaction time is 12 h. After natural cooling, the Ni foam sheet is dried in an oven at 60° C. to obtain a Ni foam sheet containing an iron precursor.
[0062] (4) The Ni foam sheet containing the iron precursor obtained in step (3) is further annealed at 600° C. for 2 h in a N2 atmosphere at a heating rate of 5° C. / min. After naturally cooling to room temperature, a three-dimensional self-supporting electrode material loaded with nano-Fe3O4 can be obtained.
[0063] Comparative Example 2
[0064] In this comparative example, in-situ carbon-coated nano-Fe3O4 is first prepared and then coated on a copper foil. The specific steps are as follows:
[0065] (1) Dissolve 0.1 g and 0.2 ml of resorcinol and formaldehyde in 60 ml of ethanol and water solution with a volume ratio of 1:2, add 0.3 ml of ammonia water, and stir for 30 min to mix thoroughly.
[0066] (2) Add 2.0 g of ferric nitrate nonahydrate to step (2) and continue stirring for 30 min. Transfer the solution to a 100 ml reactor, heat at 180 ° C, and react for 12 h. After cooling naturally, an iron-carbon precursor is obtained. The precipitated material is taken out and washed several times with ethanol and deionized water.
[0067] (3) The iron-carbon precursor powder sample obtained in step (2) is further annealed at 600°C for 2h in a N2 atmosphere at a heating rate of 5°C / min. After naturally cooling to room temperature, a powder electrode material loaded with in-situ carbon-coated nano-Fe3O4 can be obtained.
[0068] (4) The powder electrode material loaded with in-situ carbon-coated nano-Fe3O4 obtained in step (3) is mixed with a conductive agent (acetylene black) and a binder PVDF (polyvinylidene fluoride) in a mass ratio of 8:1:1, and the resulting mixture is ground into a slurry using an NMP (N-methyl-2-pyrrolidone) solvent. The slurry is then uniformly coated on a single-sided copper foil and dried in a vacuum oven at 100°C for 10 hours to obtain an electrode material.
[0069] XRD characterization was performed on the three-dimensional self-supporting electrode loaded with in-situ carbon-coated nano-Fe3O4 obtained in Example 2 of the present invention (Fe3O4@C_self-supporting), the three-dimensional self-supporting electrode material of Fe3O4 obtained in Comparative Example 1 (Fe3O4_self-supporting), and the material of Comparative Example 2 (Fe3O4@C4_coated). Figure 1 It can be seen that the XRD diffraction patterns of the samples of Example 2 and Comparative Examples 1 and 2 all correspond to the Fe3O4 (PDF#77-1545) standard card, indicating that Fe3O4 phases are generated and no other impurity phases are generated.
[0070] Figure 2 This is a SEM scanning electron microscope image of the three-dimensional self-supporting electrode material loaded with in-situ carbon-coated nano-Fe3O4 obtained in Example 2 of the present invention. As can be seen from the figure, the particle size of the Fe3O4 material obtained in Example 1 is nanometer-scale, and all present a nano-spherical morphology, and the surface of the nano-spheres is covered with an amorphous carbon layer to cross-link them.
[0071] Figure 3 This is a TEM transmission electron microscope photograph of the three-dimensional self-supporting electrode material of nano-Fe3O4 coated with in-situ carbon prepared in Example 2 of the present invention. As can be seen from the figure, the prepared Fe3O4 electrode material is in the shape of nano-spheres, and the surface of the Fe3O4 nanoparticles is coated with an amorphous carbon layer. In addition, the interplanar spacing of 0.25nm in the figure belongs to the (311) crystal plane of Fe3O4. The above results all indicate that the three-dimensional self-supporting electrode material of nano-Fe3O4 coated with in-situ carbon is successfully synthesized.
[0072] The in-situ carbon-coated nano-Fe3O4 three-dimensional self-supporting electrode materials prepared in Examples 1-3 and the electrode materials prepared in Comparative Examples 1 and 2 were used as negative electrodes to prepare lithium-ion batteries and the electrochemical performance was analyzed: the obtained electrode materials were cut into pole pieces with a diameter of 0.7×0.7 cm, and metal lithium sheets or commercial LiFePO4 (LFP) were used as positive electrodes in a glove box filled with argon gas, a Kruder 2500 diaphragm was used, and the electrolyte was a 1M LiPF6 solution. The order of negative electrode shell-spring-gasket-lithium sheet-diaphragm-negative electrode-positive electrode shell was placed in sequence, and the battery was sealed with a manual hydraulic sealing machine at a pressure of 50Mpa to assemble into a CR2032 button battery. The electrochemical performance was tested using a Xinwei battery tester.
[0073] The prepared lithium-ion battery was subjected to rate performance test. Figure 4 It can be seen that the rate performance of the in-situ carbon-coated nano-Fe3O4 three-dimensional self-supporting electrode material prepared in Example 2 (Fe3O4@C_2) is better than that of Example 1 (Fe3O4@C_1), Example 3 (Fe3O4@C_3, and Comparative Example 1 (Fe3O4_1), indicating that when the mass ratio of ferric nitrate nonahydrate to hydroquinone is 2.0:0.1, the prepared sample has better charge transfer rate and lithium ion diffusion rate.
[0074] At room temperature, the electrode materials of Example 2 and Comparative Example 1 were subjected to multiple charge and discharge cycle tests at different current densities between 0.01 and 3.0 V. Figure 5 It can be seen that the in-situ carbon-coated nano-Fe3O4 three-dimensional self-supporting electrode material (Fe3O4@C) obtained in Example 2 still retains 87% of its performance after 1000 cycles at a current density of 5A / g, while the Fe3O4 three-dimensional self-supporting electrode material obtained in Comparative Example 1 only retains 3%, which means that the electrode material (Fe3O4) of Comparative Example 1 is almost completely destroyed during the cyclic charge and discharge process at high current density. This also shows that the in-situ carbon-coated nano-Fe3O4 three-dimensional self-supporting electrode prepared in Example 1 can effectively inhibit the irreversible volume expansion of the Fe3O4 active material during high current charge and discharge, so that it has excellent electrochemical stability.
[0075] Depend on Figure 6 It can be seen that the in-situ carbon-coated nano-Fe3O4 three-dimensional self-supporting electrode material obtained in Example 2 (nickel foam) still basically maintains the initial specific capacity performance after 200 cycles at a current density of 1 A / g, while the electrode material (copper foil) prepared by carbon-coated Fe3O4 coating obtained in Comparative Example 2 only has about 31% of the specific capacity remaining, indicating that the porous structure on the three-dimensional self-supporting electrode nickel foam substrate used in Example 2 helps to suppress the irreversible volume expansion of Fe3O4 during charging and discharging, thereby improving the cycle stability of the electrode material.
[0076] In order to better evaluate the commercial application prospects of the in-situ carbon-coated nano-Fe3O4 three-dimensional self-supporting electrode material prepared in Example 2, a lithium-ion full battery was assembled using the three-dimensional self-supporting electrode prepared in Example 2 and commercial LiFePO4 (LFP) as the negative electrode and the positive electrode, respectively. Figure 7 As shown, the lithium-ion full battery was cycled 500 times at a current density of 0.1 A / g, and its battery capacity had almost no attenuation, which proved its excellent electrochemical performance and was conducive to its commercial large-scale application.
[0077] In the above embodiment, ferric nitrate nonahydrate may also be replaced by one of ferric chloride, ferric sulfate and ferric citrate.
[0078] In the above embodiment, the three-dimensional conductive substrate foam Ni may also be replaced by foam Cu or activated carbon cloth.
[0079] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A method for preparing a three-dimensional self-supporting electrode, characterized in that: The following steps are involved: Dissolving resorcinol and formaldehyde in a mixed solution of ethanol and water, adding ammonia water, and stirring until fully mixed to obtain an organic polymer solution; adding an iron-containing compound to an organic polymer solution and stirring until fully dissolved to obtain a precursor solution; Pipetting the liquid into a reaction kettle, placing the three-dimensional conductive substrate in the reaction kettle for hydrothermal reaction, and obtaining a three-dimensional self-supporting substrate containing an iron / carbon precursor; The iron-containing compound is at least one of ferric chloride, ferric nitrate nonahydrate, ferric sulfate and ferric citrate; The three-dimensional self-supporting substrate containing the iron / carbon precursor is dried and then annealed in an inert atmosphere, and then naturally cooled to room temperature to obtain a three-dimensional self-supporting electrode loaded with in-situ carbon-coated nano-Fe3O4.
2. The method for preparing a three-dimensional self-supporting electrode according to claim 1, characterized in that: The three-dimensional conductive substrate is foamed Ni, foamed Cu or activated carbon cloth.
3. The method for preparing a three-dimensional self-supporting electrode according to claim 1, characterized in that: The mass volume ratio of resorcinol to formaldehyde is (1-5) g: (1-4) ml.
4. The method for preparing a three-dimensional self-supporting electrode according to claim 1, characterized in that: The mass ratio of the iron-containing compound to the resorcinol is (1.5-2.5):0.
1.
5. The method for preparing a three-dimensional self-supporting electrode according to claim 1, characterized in that: The reaction conditions of the hydrothermal reaction are: reaction temperature is 160-200° C., and reaction time is 8-12 h.
6. The method for preparing a three-dimensional self-supporting electrode according to claim 1, characterized in that: The annealing treatment is specifically as follows: the annealing temperature is 400-800°C, the annealing time is 1-3h, and the heating rate is 5-10°C / min.
7. The method for preparing a three-dimensional self-supporting electrode according to claim 1, characterized in that: The inert atmosphere is at least one of N2 and Ar.
8. The method for preparing a three-dimensional self-supporting electrode according to claim 1, characterized in that: Placing the three-dimensional conductive substrate in the reaction kettle specifically comprises: The three-dimensional conductive substrate is placed in the reaction kettle, and the three-dimensional conductive substrate is at an angle of 40-50° to the liquid surface of the precursor solution.
9. A three-dimensional self-supporting electrode, characterized in that: The three-dimensional self-supporting electrode is prepared by the preparation method of any one of claims 1 to 8.
10. A lithium ion battery, characterized in that: The three-dimensional self-supporting electrode according to claim 9 is used as the negative electrode.
Citation Information
Patent Citations
Preparation method and application of in-situ ferroferric oxide-carbon core-shell nanoparticles
CN107069031A
Preparing method of using 'one-pot method' to synthesize ferroferric oxide@carbon composite material
CN108270001A
Double-shell-coated ferroferric oxide nano-particles as well as preparation method and application thereof
CN113184915A
Preparation method of nano composite material and lithium ion electrode negative electrode material thereof
CN114551832A
Label handling apparatus
KR1020240037927A