Preparation method of high-first-effect high-magnification lithium ion battery silicon-carbon negative electrode material

By employing steps such as acid washing of nanoscale silicon powder and coating with organic carbon sources, a silicon-carbon anode material with high initial efficiency and high rate of operation was prepared. This solved the problems of volume expansion and poor conductivity of silicon materials during charging and discharging, thereby improving the energy density and cycle stability of lithium-ion batteries.

CN118919703AInactive Publication Date: 2024-11-08SHENZHEN GUANGFENG NEW ENERGY TECH INNOVATION CENT CO LTD

Patent Information

Application Number
CN202411394742.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-08
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The theoretical capacity of graphite, the existing lithium-ion battery anode material, limits the improvement of energy density. The huge volume expansion and poor electronic conductivity of silicon materials during charging and discharging lead to electrode failure and capacity decay. Therefore, it is necessary to develop silicon-carbon anode materials with high initial efficiency and high rate of return.

Method used

A silicon-carbon anode material with high initial efficiency and high rate capability was prepared by acid washing, organic modification, organic carbon source coating, inorganic lithium source and doped element precursor composite treatment of nanoscale silicon powder, including acid washing, magnetic stirring, centrifugal washing, isothermal reaction and high temperature calcination.

Benefits of technology

This study achieved high initial charge-discharge efficiency and high rate performance of silicon-carbon anode materials, improved the cycle stability and conductivity of the battery, and reduced structural damage caused by volume expansion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919703A_ABST
    Figure CN118919703A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method of a high-first-effect high-magnification lithium ion battery silicon-carbon negative electrode material, which comprises the following steps: S1, weighing a certain mass of nano-micron silicon powder, adding the nano-micron silicon powder into acid for pickling, and stirring at room temperature for 5 minutes to obtain a product 1; s2, mixing the product 1 and an organic modifier according to a certain proportion, magnetically stirring the mixture at normal temperature, and centrifugally washing for multiple times after stirring to obtain a product 2; s3, respectively dissolving the product 2, an organic carbon source, an inorganic lithium source, a doped element precursor and the like in a solvent, mixing, and stirring at a certain temperature for a period of time to obtain a product 3; s4, adding the product 3 into an organic solvent, performing constant-temperature reaction for a period of time, performing suction filtration and washing, drying, and performing high-temperature calcination to obtain a final product; by adopting the steps, carbon coating, metal / nonmetal doping, pre-lithiation and the like of the nano-micron silicon powder are realized, and the silicon-carbon negative electrode material with high initial efficiency and high magnification is obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a method for preparing a silicon-carbon negative electrode material for a lithium ion battery with high initial efficiency and high rate. Background Art

[0002] Lithium-ion batteries have the advantages of high energy density, long cycle life, and good safety. They have been widely used in portable electronic products, electric vehicles, and energy storage. With the advancement of science and technology, the demand for high-energy-density lithium-ion batteries has become increasingly urgent. At present, the commercial lithium battery negative electrode material is graphite, with a theoretical capacity of 372mAh / g, which limits the improvement of lithium battery energy density. Silicon, as a negative electrode material, has an ultra-high theoretical capacity (4200 mAh / g) and a suitable lithium insertion and extraction platform, and has good safety. It is the most promising next-generation lithium battery negative electrode alternative material. However, the huge volume expansion (300%) of silicon materials during the charging and discharging process and the semiconductor properties with poor electronic conductivity restrict its large-scale application in the field of electrochemical energy storage. The huge volume expansion of silicon during the charging and discharging process causes the destruction of the particle structure, resulting in electrode failure, and the SEI film is broken and repeatedly generated, resulting in continuous consumption of electrolyte and capacity decay. Reducing the silicon particle size to nanoscale can effectively shorten the lithium ion transmission distance, and can release the volume expansion stress. Composite with materials such as carbon can further improve the cycle stability and conductivity of silicon negative electrodes. The key to preparing a stable silicon-carbon negative electrode is the uniform compounding of silicon and carbon and the strong bonding between them. In-situ carbon growth on the silicon surface can achieve a complete and uniform coating on the silicon surface, so that silicon is evenly dispersed in the carbon material, which can increase the contact area between silicon and carbon compared to physical mixing. Surface carbon can provide binding sites for heteroatom doping, and metal / non-metal doping can further enhance the conductivity of the composite material. In order to better utilize the advantages of the high specific capacity of the silicon negative electrode, it is extremely important to develop a suitable method to reduce the irreversible capacity loss of the silicon negative electrode in the first cycle.

[0003] Therefore, there is an urgent need to provide a method for preparing a high-initial-efficiency and high-rate lithium-ion battery silicon-carbon negative electrode material to solve the above problems. Summary of the invention

[0004] The purpose of the present invention is to overcome the shortcomings and defects of the prior art and provide a method for preparing a silicon-carbon negative electrode material for a lithium-ion battery with high initial efficiency and high rate, thereby realizing carbon coating, metal / non-metal doping, and pre-lithiation of nano-micron silicon powder, and obtaining a silicon-carbon negative electrode material with high initial efficiency and high rate.

[0005] The objective of the present invention is achieved through the following technical solutions: A method for preparing a high-initial-efficiency and high-rate lithium-ion battery silicon-carbon negative electrode material comprises the following steps: S1: Weigh a certain mass of nano-micron silicon powder, add it to acid for pickling, and stir it at room temperature for 5 minutes to obtain product 1; S2: mixing product 1 and an organic modifier in a certain proportion, magnetically stirring the mixture at room temperature, and centrifugally washing the mixture for multiple times after stirring to obtain product 2; S3: dissolving the product 2, the organic carbon source, the inorganic lithium source and the doping element precursor in a solvent respectively, mixing and stirring at a certain temperature for a period of time to obtain the product 3; S4: adding the product 3 to an organic solvent, reacting at a constant temperature for a period of time, filtering and washing, drying, and calcining at a high temperature to obtain the final product.

[0006] Optionally, the nano-micron silicon particle size D50 in the S1 is 0.5μm~1μm, and the purity is greater than 99.9%. The pickling agent in the S1 is any one or more combinations of hydrogen peroxide, sulfuric acid, and hydrochloric acid. The concentration of the pickling agent is 5%~7%, and the solid-liquid ratio of the nano-micron silicon powder to the pickling agent is 1:20~1:100.

[0007] Optionally, the organic modifier in S2 is one or a combination of diethylene glycol phthalate, hexadecyltrimethylammonium bromide, and the product 1 is mixed with the organic modifier and dissolved in deionized water, wherein the ratio of the product 1, the organic modifier and the deionized water is 0.5 g: 2 mL: 100 mL, and magnetic stirring is performed for 1-6 h.

[0008] Optionally, the organic carbon source in S3 is a combination of any two or more of urea, polyacrylic acid, formaldehyde, glucose, tannic acid, carboxymethyl cellulose, glutaraldehyde polyvinyl alcohol, and dopamine; the inorganic lithium source is any one or more of lithium hydroxide, lithium carbonate, and lithium bicarbonate; the doping element precursor is any one or more of zinc nitrate hexahydrate, cobalt chloride hexahydrate, and ethylenediamine; the mass ratio of the product 2, the organic carbon source, the inorganic lithium source, and the doping element precursor in S3 is 6:2:1:1~7:2:0.5:0.5; and the reaction temperature in S3 is 30-100°C.

[0009] Optionally, the solvent in S3 is any one or more combinations of formaldehyde, acetaldehyde, formic acid, and polyvinyl pyrrolidone, and the calcination temperature in S4 is 700-900°C.

[0010] Compared with the prior art, the present invention has the following beneficial effects: In the present invention, a certain mass of nano-micron silicon powder is weighed, added to acid for pickling to improve the chemical properties of the silicon powder, and stirred at room temperature for 5 minutes; a certain amount of modifier is added, magnetic stirring is performed at room temperature, and centrifugal washing is performed for multiple times; the organic carbon source, inorganic lithium source, doping element precursor, etc. are dissolved in the solvent respectively, so that the nano-micron silicon can be coated with the organic carbon source, inorganic lithium source and doping element precursor; the product is added to an organic solvent, reacted at a constant temperature for a period of time, filtered and washed, and then dried and calcined to obtain the final product; carbon coating, metal / non-metal doping, pre-lithiation, etc. of nano-micron silicon powder are achieved, and a silicon-carbon negative electrode material with high first efficiency and high rate is obtained. BRIEF DESCRIPTION OF THE DRAWINGS

[0011] Figure 1 It is a process flow chart of the present invention.

[0012] Figure 2 This is a blue electric cycle test diagram comparing Examples 1 and 3 of the present invention at different current densities.

[0013] Figure 3 This is a test chart comparing the blue electric rate under different current densities in Example 2 of the present invention. DETAILED DESCRIPTION

[0014] The present invention is further described in detail below in conjunction with embodiments and drawings, but the embodiments of the present invention are not limited thereto.

[0015] The technical solution of the present invention proposes a method for preparing a silicon-carbon negative electrode material for a lithium-ion battery with high initial efficiency and high rate.

[0016] Reference Figures 1 to 3 , in this embodiment, includes: S1: Weigh a certain mass of nano-micron silicon powder, add it to acid for pickling, and stir it at room temperature for 5 minutes to obtain product 1; S2: mixing product 1 and an organic modifier in a certain proportion, magnetically stirring the mixture at room temperature, and centrifugally washing the mixture for multiple times after stirring to obtain product 2; S3: dissolving the product 2, the organic carbon source, the inorganic lithium source and the doping element precursor in a solvent respectively, mixing and stirring at a certain temperature for a period of time to obtain the product 3; S4: adding the product 3 to an organic solvent, reacting at a constant temperature for a period of time, filtering and washing, drying, and calcining at a high temperature to obtain the final product.

[0017] Optionally, in this embodiment, a certain mass of nano-micron silicon powder is weighed and added to acid for pickling. Pickling the nano-micron silicon powder can improve the purity of the silicon powder and remove impurities in the silicon powder. At the same time, pickling can change the physical and chemical properties of the surface of the silicon powder, and to a certain extent alleviate the strain caused by the volume expansion of the silicon powder during the charging and discharging process, thereby maintaining the stability of the electrode. After the pickling is completed, stirring at room temperature for five minutes to obtain product 1; mixing product 1 with an organic modifier in a certain proportion, magnetically stirring the mixture at room temperature, so that the organic modifier modifies product 1, and stirring and centrifuging to obtain product 2; product 2, an organic carbon source, The inorganic lithium source and the doping element precursor are dissolved in the solvent respectively, so that the nano-micron silicon can be coated by the organic carbon source, the inorganic lithium source and the doping element precursor to obtain product 3, and then the product 3 is added to the organic solvent, filtered and washed after isothermal reaction, and dried and calcined to obtain the final product, that is, the doped and coated silicon-carbon composite material. The composite structure material can expand the volume of silicon during the charge and discharge cycle, thereby improving the conductivity of the material. In-situ pre-lithiation can obtain a higher first charge and discharge efficiency. Through the above steps, carbon coating, metal / non-metal doping, pre-lithiation, etc. of nano-micron silicon powder are realized, and a silicon-carbon negative electrode material with high first efficiency and high rate is obtained. Example 1

[0018] Weigh a certain mass of nano-micron silicon powder, add 5% hydrogen peroxide for pickling, the solid-liquid ratio of silicon powder to hydrogen peroxide is 1:20, and stir at room temperature for 5 minutes to obtain product 1. Then add a certain amount of diethylene glycol diacrylate phthalate to product 1, wherein the ratio of pickled silicon powder to diethylene glycol diacrylate phthalate is 0.5g of pickled silicon powder dissolved in 2ml of diethylene glycol diacrylate phthalate, mix and stir magnetically at room temperature, centrifuge and wash 3 times to obtain product 2. Then, product 2, urea, polyacrylic acid, lithium hydroxide, and zinc nitrate hexahydrate are dissolved in formaldehyde, mixed and stirred at 30°C for 1 hour, filtered and washed, and then the sample is carbonized at 750°C to obtain the target negative electrode material. The silicon-carbon negative electrode material prepared in Example 1 was directly used as the negative electrode material of lithium-ion batteries, with metal lithium sheets as the counter electrode, Celgard2325 as the separator, and 1 mol / L LiPF6 (the solvent was a mixture of ethylene carbonate and dimethyl carbonate in a volume ratio of 1:1) as the electrolyte, and assembled into CR2032 button batteries in an argon-protected glove box. The voltage charge and discharge range in the blue power test was 0.01~3 V. Figure 2 After 300 cycles of lithium-ion battery at a current density of 0.2 A / g, it showed a specific capacity of 1358.6 mA h / g. The silicon-carbon negative electrode showed outstanding capacity advantage and cycle stability. Example 2

[0019] Weigh 5g of nano-micron silicon powder and place it in 5% hydrochloric acid for pickling. The solid-liquid ratio of the silicon powder and hydrochloric acid is 1:30. After stirring at room temperature for 10 minutes, product 1 is obtained. Subsequently, a certain amount of hexadecyltrimethylammonium bromide is added to product 1, wherein the ratio of pickled silicon powder to hexadecyltrimethylammonium bromide is 0.5g of pickled silicon powder dissolved in 2ml of hexadecyltrimethylammonium bromide, mixed and magnetically stirred at room temperature, and centrifuged and washed 3 times to obtain product 2. Subsequently, product 2, tannic acid, carboxymethyl cellulose, lithium carbonate, and cobalt chloride hexahydrate are dissolved in acetaldehyde, mixed and stirred at 30°C for 1 hour, filtered and washed, and then the sample is carbonized at 800°C to obtain the target silicon-carbon negative electrode material. The final negative electrode material was assembled into a half-button battery for charge and discharge performance testing. The charge and discharge current density of the lithium-ion battery in the test program was 0.1 A / g, 0.2 A / g, 0.5A / g, 1.0 A / g, 2.0 A / g, 5.0 A / g, 0.1 A / g. The number of charge and discharge cycles at the same current density was 10. Figure 3 The specific capacities of lithium-ion batteries at the above current densities are 1702.2 mA h / g, 1376.3 mAh / g, 1120.4 mA h / g, 1028.7 mA h / g, 920.4 mA h / g, 849.1 mA h / g, and 1638.9 mA h / g, respectively. It can be found that when the current density is restored to the initial current density of 0.5 A / g, the reversible specific capacity of the negative electrode material can still reach 96% of the first discharge specific capacity. It can be seen that the silicon-carbon negative electrode has obtained excellent rate performance when tested at different current densities. Example 3

[0020] Weigh a certain mass of nano-micron silicon powder, add it to 5% sulfuric acid for pickling, the solid-liquid ratio of silicon powder to sulfuric acid is 1:50, and stir at room temperature for 5 minutes to obtain product 1. Then add a certain amount of diethylene glycol diacrylate of phthalate and hexadecyl trimethyl ammonium bromide mixed solution to product 1, dissolve 0.5g of pickled silicon powder in 2ml of diethylene glycol diacrylate of phthalate and hexadecyl trimethyl ammonium bromide mixed solution, and then stir magnetically at room temperature, centrifuge and wash 3 times to obtain product 2. Then, product 2, carboxymethyl cellulose, glutaraldehyde polyvinyl alcohol, zinc nitrate hexahydrate, ethylenediamine, lithium bicarbonate, etc. are dissolved in formic acid, mixed and stirred at 30°C for 1 hour, filtered and washed, and then the sample is carbonized at 900°C and kept warm for 2 hours to obtain the target negative electrode material. The final negative electrode material is assembled into a semi-button battery for charge and discharge performance testing. The voltage charge and discharge range in the blue electricity test is 0.01~3 V. Reference Figure 2After 300 cycles at a current density of 0.5 A / g, the potassium ion battery exhibited a specific capacity of 1066.5 mA h / g, and the silicon-carbon negative electrode showed outstanding capacity advantages and cycle stability. Example 4

[0021] Weigh a certain mass of nano-micron silicon powder, add 5% hydrogen peroxide and 5% hydrochloric acid for pickling, the solid-liquid ratio of the silicon powder and the acid is 1:100, and stir for 5 minutes at room temperature to obtain product 1. Then add a certain amount of diethylene glycol diacrylate of phthalate and hexadecyl trimethyl ammonium bromide mixed solution to product 1, dissolve 0.5g of pickled silicon powder in 2ml of diethylene glycol diacrylate of phthalate and hexadecyl trimethyl ammonium bromide mixed solution, and then stir magnetically at room temperature, centrifuge and wash 3 times to obtain product 2. Then, product 2, glucose, tannic acid, dopamine, carboxymethyl cellulose, glutaraldehyde polyvinyl alcohol, zinc nitrate hexahydrate, cobalt chloride hexahydrate, lithium hydroxide, etc. are dissolved in polyvinyl pyrrolidone, mixed and stirred at 30°C for 2 hours, filtered and washed, and then the sample is carbonized at 700°C and kept warm for 2 hours to obtain the target negative electrode material. The final negative electrode material was assembled into a half-button battery for charge and discharge performance testing. Comparing the two cases with and without lithium hydroxide, the first charge and discharge efficiency was 86% and 74% respectively. The results showed that the pre-lithiation silicon-carbon negative electrode exhibited high first efficiency performance.

Claims

1. A method for preparing a high initial efficiency and high rate lithium ion battery silicon-carbon negative electrode material, characterized in that: The following steps are involved: S1: Weigh a certain mass of nano-micron silicon powder, add it to acid for pickling, and stir it at room temperature for 5 minutes to obtain product 1; S2: mixing product 1 and an organic modifier in a certain proportion, magnetically stirring the mixture at room temperature, and centrifugally washing the mixture for multiple times after stirring to obtain product 2; S3: dissolving the product 2, the organic carbon source, the inorganic lithium source and the doping element precursor in a solvent respectively, mixing and stirring at a certain temperature for a period of time to obtain the product 3; S4: adding the product 3 to an organic solvent, reacting at a constant temperature for a period of time, filtering and washing, drying, and calcining at a high temperature to obtain the final product.

2. The method for preparing a high initial efficiency and high rate lithium ion battery silicon-carbon negative electrode material according to claim 1, characterized in that: The nano-micron silicon particle size D50 in the S1 is 0.5μm~1μm, and the purity is greater than 99.9%. The pickling agent in the S1 is any one or more combinations of hydrogen peroxide, sulfuric acid, and hydrochloric acid. The concentration of the pickling agent is 5%~7%, and the solid-liquid ratio of the nano-micron silicon powder to the pickling agent is 1:20~1:

100.

3. The method for preparing a high initial efficiency and high rate lithium ion battery silicon-carbon negative electrode material according to claim 2, characterized in that: The organic modifier in S2 is one or a combination of diethylene glycol phthalate and hexadecyltrimethylammonium bromide. The product 1 is mixed with the organic modifier and dissolved in deionized water. The ratio of the product 1, the organic modifier and the deionized water is 0.5 g: 2 mL: 100 mL, and the mixture is stirred magnetically for 1-6 h.

4. The method for preparing a high initial efficiency and high rate lithium ion battery silicon-carbon negative electrode material according to claim 3, characterized in that: The organic carbon source in S3 is any combination of two or more of urea, polyacrylic acid, formaldehyde, glucose, tannic acid, carboxymethyl cellulose, glutaraldehyde polyvinyl alcohol, and dopamine; the inorganic lithium source is any one or more of lithium hydroxide, lithium carbonate, and lithium bicarbonate; the doping element precursor is any one or more of zinc nitrate hexahydrate, cobalt chloride hexahydrate, and ethylenediamine; the mass ratio of the product 2, the organic carbon source, the inorganic lithium source, and the doping element precursor in S3 is 6:2:1:1~7:2:0.5:0.5; and the reaction temperature in S3 is 30-100°C.

5. The method for preparing a high initial efficiency and high rate lithium ion battery silicon-carbon negative electrode material according to claim 2, characterized in that: The solvent in S3 is any one or more combinations of formaldehyde, acetaldehyde, formic acid, and polyvinyl pyrrolidone, and the calcination temperature in S4 is 700-900°C.

Citation Information

Patent Citations

  • Silver-particle-doped silicon carbon negative electrode material preparation method

    CN108336311A

  • Organic-inorganic composite silicon-based negative electrode material, and preparation method and application thereof

    CN112289987A

  • Silicon-carbon negative electrode material and preparation method thereof

    CN114388807A

  • Lithium-pre-embedded silicon-carbon negative electrode material and preparation method and application thereof

    CN116487549A

  • Silicon-oxygen composite negative electrode, preparation method thereof and all-solid-state battery

    CN116705994A

Cited By

  • Preparation method and application of low-expansion silicon-carbon negative electrode material

    CN119528146A

  • Silicon-carbon negative electrode material containing lithium super-ionic conductor gradient interface and in-situ construction preparation method and application of silicon-carbon negative electrode material

    CN122638443A