Preparation and application of nickel vanadate / carbon nanotube composite nanosphere

Synthesis of nickel vanadate/carbon nanotube composite nanospheres by one-step hydrothermal method, the poor conductivity and volume expansion problems of nickel vanadate materials were solved, and the preparation of nanospheres with high dispersion and uniform particle size was achieved, which improved the lithium-ion battery. Electrochemical properties and cyclic stability.

CN118919706AActive Publication Date: 2024-11-08CHONGQING RES INST OF CHANGCHUN UNIV OF TECH
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411172473.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-08
Estimated Expiration
2044-08-26

AI Technical Summary

Technical Problem

As the negative electrode material of lithium-ion batteries, nickel vanadate has problems such as poor conductivity, huge volume expansion, fragility in powder and low specific surface area, which affects its electrochemical performance and cyclic stability.

Method used

A one-step hydrothermal method was used to synthesize nickel vanadate/carbon nanotube composite nanospheres. By adding NiCl2·6H2O and nickel-plated carbon nanotubes to the ammonium metavanadate solution, adding anhydrous ethanol slowly, and heating at 160-200℃ 6 ~10 hours, centrifugation and drying were performed to produce highly dispersed and uniform particle size Ni3V2O8/CNT composite nanospheres. The CNT wound structure provides a conductive pathway, and ultra-small Ni3V2O8 nanoparticles are embedded on the CNT.

Benefits of technology

The electrochemical performance and cyclic stability of Ni3V2O8/CNT composite nanospheres are improved, the electron transmission rate and lithium ion transmission distance are enhanced, and the specific capacity and rate performance of the material are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919706A_ABST
    Figure CN118919706A_ABST
Patent Text Reader

Abstract

The invention discloses preparation and application of nickel vanadate / carbon nanotube composite nanospheres, NiCl2. 6H2O and nickel-plated carbon nanotubes are added into an ammonium metavanadate solution, absolute ethyl alcohol is slowly added, and heating is performed for 6-10 h at the temperature of 160-200 DEG C; and centrifugally separating, and drying the precipitate. The Ni3V2O8 / CNT composite nanosphere with high dispersion and uniform particle size is synthesized by adopting a one-step hydrothermal method for the first time. The unique CNT winding main body structure can provide a conductive path for transmission of electrons. The ultra-small Ni3V2O8 nanoparticles are uniformly embedded on the CNT, so that the transmission distance of lithium ions is greatly reduced while electron transmission is accelerated, and the electrochemical performance of the Ni3V2O8 / CNT composite nanosphere is improved. The Ni3V2O8 / CNT lithium ion battery negative electrode material prepared by the method disclosed by the invention has good cycling stability and rate capability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of nanocomposite materials and their application, and specifically relates to the preparation of nickel vanadate / carbon nanotube (Ni3V2O8 / CNT) composite nanospheres and their application in lithium ion batteries. Background Art

[0002] Industrial graphite has been widely used as anode for lithium-ion batteries, but its specific capacity is relatively low (372 mA h g -1 ), which limits its further application in lithium-ion batteries. Therefore, exploring new high-energy, high-power density lithium-ion battery negative electrode materials and improving their electrochemical performance is one of the important research directions of lithium-ion batteries.

[0003] Transition metal vanadate materials have multiple valence states of vanadium, which makes this type of electrode material have a higher electrode specific capacity and is also conducive to the application of batteries in a wider potential range. Therefore, metal vanadates are considered to be anode materials with great development potential for lithium-ion batteries. Among them, nickel vanadate electrode materials have the advantages of high specific capacity, excellent rate performance, and environmental friendliness. At the same time, the price of nickel is only one-third of that of cobalt, and the cost is low. Therefore, it is a new type of negative electrode material for lithium-ion batteries with great application prospects [LU Y, NAI JW, LOU X W. Formation of NiCo2V2O8 yolk-doubleshell spheres with enhanced lithium storage properties. Angewandte ChemieInternational Edition, 2018, 57(11): 2899-2903; YANG GZ, LI SY, WU MM, etal. Zinc pyrovanadate nanosheets of atomic thickness: excellent Li-storageproperties and investigation of their electr℃hemical mechanism. Journal ofMaterials Chemistry A, 2016, 4(28): 10974-10985.]. However, nickel vanadate also has some shortcomings in practical applications as a negative electrode material for lithium-ion batteries. The metal vanadate material has poor electrical conductivity, huge volume expansion during the charge and discharge process, and is easily pulverized, causing the active material to fall off the current collector, which significantly affects the cycle stability. In addition, the specific surface area of ​​the metal vanadate material currently prepared is not high, which affects its electrochemical performance. In order to solve the above inherent shortcomings of nickel vanadate and improve the electrochemical performance of nickel vanadate as a negative electrode material for lithium-ion batteries, in recent years, researchers have focused on the micro-nano, surface coating, and composite of nickel vanadate electrode materials. In addition to suppressing the volume effect during the charge and discharge process and improving the cycle stability of the electrode material, the special nanostructure, such as hollow spheres, porous and ultrafine particles, especially ultrafine nanoparticles, have extraordinary performance due to their ultra-small particle size.Among many carbon-based materials, carbon nanotubes, as one-dimensional nanomaterials, are light in weight, have perfectly connected hexagonal structures of tube walls, and have many exceptional mechanical, electrical and chemical properties [WANG C, FANG D, WANG HE, et al. Uniform nickel vanadate (Ni3V2O8) nanowirearrays organized by ultrathin nanosheets with enhanced lithium storageproperties. Scientific Reports, 2016, 6: 20826- 20834; SAMBANDAM B,SOUNDHARRAJAN V, SONG J, et al. Ni3V2O8 nanoparticles as an excellent anodematerial for high-energy lithium-ion batteries. Journal of ElectroanalyticalChemistry, 2018, 810: 34-40; SOUNDHARRAJAN V, SAMBANDAM B, SONG J, et al.Bitter gourd-shaped Ni3V2O8 anode developed by a one-pot metal-organicframework-combustion technique for advanced Li-ion batteries. CeramicsInternational, 2017, 43(16): 13224-13232.]. How to combine carbon nanotubes with ultrafine nickel vanadate nanoparticles and find a simple and controllable method to alleviate the agglomeration and pulverization of electrode materials caused by volume expansion / contraction is of great significance to improving the cycle stability of nickel vanadate electrode materials. Summary of the invention

[0004] The purpose of the present invention is to provide a preparation method of nickel vanadate / carbon nanotube composite nanospheres Ni3V2O8 / CNT and application thereof in lithium ion batteries. The nickel vanadate / carbon nanotube composite nanospheres prepared by the method have the characteristics of good dispersibility, large specific capacity, good cycle performance, long service life, etc.

[0005] A nickel vanadate / carbon nanotube composite nanosphere is prepared by the following method, which comprises:

[0006] 1) Add 300-500 mg of ammonium metavanadate powder to 30-50 mL of deionized water, heat to 60-80°C, stir, dissolve, and cool to room temperature;

[0007] 2) Weigh 30-60 mg NiCl2·6H2O and 500-800 mg nickel-plated carbon nanotubes, add them to the ammonium metavanadate solution obtained in step 1), stir for 10-20 min, then slowly add 50-70 mL of anhydrous ethanol to the solution, stir and mix evenly;

[0008] 3) The mixed solution obtained in step 2) is heated at a temperature of 160-200° C. for 6-10 hours; centrifuged, precipitated and dried to obtain Ni3V2O8 / CNT composite nanospheres.

[0009] Step 3) The drying is carried out in an oven at 50 to 70°C for 10 to 20 hours;

[0010] The centrifugation in step 3) is 5000-6000 rpm for 5-7 min.

[0011] 300 mg of the ammonium metavanadate described in step 1), 30 mL of deionized water;

[0012] Step 2) 30 mg of NiCl2·6H2O, 500 mg of nickel-plated carbon nanotubes, and 50 mL of anhydrous ethanol;

[0013] Step 3) The temperature is 170°C and heated for 10 hours.

[0014] 500 mg of the ammonium metavanadate described in step 1), 50 mL of deionized water;

[0015] Step 2) 60 mg of NiCl2·6H2O, 800 mg of nickel-plated carbon nanotubes, and 70 mL of anhydrous ethanol;

[0016] Step 3) Heat at 180°C for 6 hours.

[0017] 400 mg of the ammonium metavanadate described in step 1), 40 mL of deionized water;

[0018] Step 2) NiCl2·6H2O 50 mg, nickel-plated carbon nanotubes 600 mg, anhydrous ethanol 60 mL;

[0019] Step 3) The temperature is 190°C and heated for 6 hours.

[0020] The invention provides a preparation method and application of nickel vanadate / carbon nanotube composite nanospheres. NiCl2·6H2O and nickel-plated carbon nanotubes are added to an ammonium metavanadate solution, and then anhydrous ethanol is slowly added. The mixture is heated at a temperature of 160 to 200°C for 6 to 10 hours. The mixture is centrifuged and the precipitate is dried to obtain the prepared nanospheres. A one-step hydrothermal method is used for the first time to synthesize highly dispersed Ni3V2O8 / CNT composite nanospheres with uniform particle size. The unique CNT winding main structure can provide a conductive path for the transmission of electrons. Ultra-small Ni3V2O8 nanoparticles are uniformly embedded in CNTs, which accelerates the transmission of electrons and greatly reduces the transmission distance of lithium ions, thereby improving the electrochemical performance of the Ni3V2O8 / CNT composite nanospheres. The Ni3V2O8 / CNT lithium ion battery negative electrode material prepared by the method of the invention has good cycle stability and rate performance.

[0021] The present invention has the following advantages:

[0022] 1) The synthesis method of the present invention is simple, and for the first time, a one-step hydrothermal method is used to synthesize highly dispersed Ni3V2O8 / CNT composite nanospheres with uniform particle size.

[0023] 2) The CNT-wrapped main structure can provide a conductive pathway for the transmission of electrons and accelerate the kinetics of electrochemical reactions.

[0024] 3) Ultra-small Ni3V2O8 nanoparticles are evenly embedded on CNTs, which not only increases the electron transmission rate, but also greatly reduces the transmission distance of lithium ions, thus improving the electrochemical performance of Ni3V2O8 / CNT composite nanospheres.

[0025] 4) The Ni3V2O8 / CNT composite nanomaterial prepared by the method of the present invention has a high capacity and good cycle stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 This is a transmission electron microscope image of the nickel-plated CNT prepared in Example 1 of the present invention;

[0027] Figure 2 This is a scanning electron microscope image of the Ni3V2O8 / CNT composite nanospheres prepared in Example 1 of the present invention;

[0028] Figure 3 This is a transmission electron microscope image of a single Ni3V2O8 / CNT composite nanosphere prepared in Example 1 of the present invention;

[0029] Figure 4 This is a surface scanning image of the Ni3V2O8 / CNT composite nanospheres prepared in Example 1 of the present invention;

[0030] Figure 5The charge and discharge cycle curves of the Ni3V2O8 / CNT composite nanomaterial prepared in Example 1 of the present invention at different current densities. DETAILED DESCRIPTION

[0031] Example 1

[0032] A nickel vanadate / carbon nanotube composite nanosphere Ni3V2O8 / CNT

[0033] 300 mg of ammonium metavanadate powder was added to 30 mL of deionized water and the mixture was placed at 60 ℃ Heat and stir in an oil bath for 5 min. After the solid powder is completely dissolved, cool to room temperature for later use. Weigh 30 mg NiCl2·6H2O and 500 mg nickel-plated carbon nanotubes (3A, product number: A60059, CAS: 308068-56-6) and add them to the above solution. After stirring at room temperature for 10 min, slowly add 50 mL of anhydrous ethanol to the above solution and stir to mix evenly. Then, transfer the mixed solution to an autoclave at 170 ℃ Heating for 10 h. Then centrifugation (speed: 5000 rpm, time: 7 min), drying (temperature: 50 ℃ , time: 20 h), Ni3V2O8 / CNT composite nanospheres were obtained.

[0034] Example 2

[0035] A nickel vanadate / carbon nanotube composite nanosphere Ni3V2O8 / CNT

[0036] 500 mg of ammonium metavanadate powder was added to 50 mL of deionized water and the mixture was placed at 75 ℃ Heat and stir in an oil bath for 5 min. After the solid powder is completely dissolved, cool to room temperature for later use. Weigh 60 mg NiCl2·6H2O and 800 mg nickel-plated carbon nanotubes and add them to the above solution. After stirring at room temperature for 20 min, slowly add 70 mL of anhydrous ethanol to the above solution and stir to mix evenly. Then, transfer the mixed solution to an autoclave at 180 ℃ Heating for 6 h. Then centrifugation (speed: 6000 rpm, time: 6 min), drying (temperature: 70 ℃ , time: 10 h), Ni3V2O8 / CNT composite nanospheres were obtained.

[0037] Example 3

[0038] A nickel vanadate / carbon nanotube composite nanosphere Ni3V2O8 / CNT

[0039] 400 mg of ammonium metavanadate powder was added to 40 mL of deionized water and the mixture was placed at 80 ℃ Heat and stir in an oil bath for 6 min. After the solid powder is completely dissolved, cool to room temperature for later use. Weigh 40 mg NiCl2·6H2O and 600 mg nickel-plated carbon nanotubes and add them to the above solution. After stirring at room temperature for 15 min, slowly add 60 mL of anhydrous ethanol to the above solution and stir to mix evenly. Then, transfer the mixed solution to an autoclave at 190 ℃ Heating for 6 h. Then centrifugation (speed: 7000 rpm, time: 5 min), drying (temperature: 50 ℃ , time: 12 h), Ni3V2O8 / CNT composite nanospheres were obtained.

[0040] Experimental example

[0041] The nickel vanadate / carbon nanotube composite nanosphere NNi3V2O8 / CNT composite nanomaterial prepared in Example 1 is used in lithium-ion batteries.

[0042] Take three materials, namely Ni3V2O8 / CNT composite nanospheres, conductive agent (SuperP) and adhesive (PVDF), and then weigh them according to m1:m2:m3=8:1:1, add appropriate amount of N-methylpyrrolidone solution, mix and stir evenly, apply it on the cut copper foil, and place it horizontally at 120 ℃ In the vacuum oven, the drying time is set to 12 h, and then a button battery slicer is used to punch it into round electrodes for standby use.

[0043] The assembly of button cells is carried out in a glove box filled with high-purity Ar, and O2 < 0.1 ppm and H2O < 0.1 ppm are controlled. First, the negative electrode shell is placed on a horizontal table, the negative electrode plate is placed in the center of the electrode shell, the electrolyte is added to the center of the plate, and then the diaphragm is placed to cover the plate. The diaphragm needs to be wetted by the electrolyte, and the lithium sheet, gasket and shrapnel are placed on the diaphragm. After the positive electrode shell is covered, the sheet is pressed and transferred outside the glove box.

[0044] Experiments show that the prepared Ni3V2O8 / CNT composite nanomaterial has high capacity and good cycle stability. Figure 5 As shown, at 1 A g -1 , 10A g -1 and 20 A g -1 The capacity of the battery after 500 charge and discharge cycles is 880.4 mA h g -1 , 490.9 mA hg -1 and 316.1 mA hg -1 .

Claims

1. A nickel vanadate / carbon nanotube composite nanosphere is prepared by the following method, which comprises: 1) Add 300-500 mg of ammonium metavanadate powder to 30-50 mL of deionized water, heat to 60-80°C, stir, dissolve, and cool to room temperature; 2) Weigh 30-60 mg NiCl2·6H2O and 500-800 mg nickel-plated carbon nanotubes, add them to the ammonium metavanadate solution obtained in step 1), stir for 10-20 min, then slowly add 50-70 mL of anhydrous ethanol to the solution, stir and mix evenly; 3) The mixed solution obtained in step 2) is heated at a temperature of 160-200° C. for 6-10 hours; centrifuged, precipitated and dried to obtain Ni3V2O8 / CNT composite nanospheres.

2. The nickel vanadate / carbon nanotube composite nanosphere according to claim 1, characterized in that: The drying in step 3) is carried out in an oven at 50 to 70°C for 10 to 20 hours.

3. The nickel vanadate / carbon nanotube composite nanosphere according to claim 2, characterized in that: The centrifugation in step 3) is 5000-6000 rpm for 5-7 min.

4. The nickel vanadate / carbon nanotube composite nanosphere according to claim 1, 2 or 3, characterized in that: 300 mg of the ammonium metavanadate described in step 1), 30 mL of deionized water; Step 2) 30 mg of NiCl2·6H2O, 500 mg of nickel-plated carbon nanotubes, and 50 mL of anhydrous ethanol; Step 3) The temperature is 170°C and heated for 10 hours.

5. The nickel vanadate / carbon nanotube composite nanosphere according to claim 1, 2 or 3, characterized in that: 500 mg of the ammonium metavanadate described in step 1), 50 mL of deionized water; Step 2) 60 mg of NiCl2·6H2O, 800 mg of nickel-plated carbon nanotubes, and 70 mL of anhydrous ethanol; Step 3) Heat at 180°C for 6 hours.

6. The nickel vanadate / carbon nanotube composite nanosphere according to claim 1, 2 or 3, characterized in that: 400 mg of the ammonium metavanadate described in step 1), 40 mL of deionized water; Step 2) NiCl2·6H2O 50 mg, nickel-plated carbon nanotubes 600 mg, anhydrous ethanol 60 mL; Step 3) The temperature is 190°C and heated for 6 hours.

Citation Information

Patent Citations

  • Positive pole of lithium ionic cell

    CN101420022A

  • Preparation method of carbon-coated vanadate composite fiber for lithium-ion battery anode material

    CN102280625A

  • High strength polymer comprising carbon nanotube

    CN107108954A

  • An ultra-small vanadium carbide embedded carbon nanotube material, a preparing method thereof and an application thereof in a water cracking hydrogen production aspect

    CN108837838A

  • Carbon nanotube / nickel cobaltate lithium ion battery negative electrode material and preparation method thereof

    CN110858640A