Double-wide-range and high-acid-retention gel state mixed matrix PBI proton exchange membrane as well as preparation method and application thereof

By combining flexible zirconium-glutamic acid or UiO-66 series MOF with polybenzimidazole, a gel-state proton exchange membrane with high efficiency and acid preservation is solved, the performance of the existing proton exchange membrane in low temperature and high humidity environments is solved. and acid loss problem achieve stable and high performance in a wide temperature and humidity range, extending the service life of the fuel cell.

CN118919787AActive Publication Date: 2024-11-08ZHEJIANG UNIV OF TECH

Patent Information

Application Number
CN202411148491.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-08
Estimated Expiration
2044-08-21

AI Technical Summary

Technical Problem

The existing proton exchange membranes have problems with degraded proton conduction performance and acid loss in low temperature and high humidity environments, resulting in unstable fuel cell performance and short service life.

Method used

Using flexible zirconium-glutamic acid or UiO-66 series MOF combined with polybenzimidazole, a gel-state mixed matrix PBI proton exchange membrane is formed by hydrating polyphosphoric acid, achieving excellent performance in a wide temperature and humidity range .

Benefits of technology

Maintaining high proton conduction performance and acid retention ability in the range of -20℃ to 240℃ and 0 to 80% RH, extending the service life of the fuel cell and solving the problems of low-temperature cold start-up difficulties and poor high-temperature performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919787A_ABST
    Figure CN118919787A_ABST
Patent Text Reader

Abstract

The invention discloses a double-wide-range-high-acid-retention gel state mixed matrix PBI proton exchange membrane and a preparation method and application thereof.The gel state proton membrane is composed of a flexible zirconium-glutamic acid (L-Glu-Zr (P)) or UiO-66 series metal organic framework, polybenzimidazole (PBI), phosphoric acid and water, and the preparation method comprises the steps that polyphosphoric acid serves as a solvent, under protection of inert gas, the gel state proton exchange membrane is subjected to heat preservation for 1-2 h, and then the gel state proton exchange membrane is obtained. The preparation method comprises the following steps: carrying out high-temperature polycondensation on an aromatic tetramine monomer and a dicarboxylphenyl monomer to form a PBI polymer solution, adding metal organic framework particles, uniformly dispersing, scraping the mixed solution on a substrate, and carrying out a phase transformation process from the solution to a gel-state film; the proton exchange membrane prepared by the invention shows excellent acid retention capacity, proton transfer characteristic, fuel cell performance and stability in a double-wide-range (the temperature is-20 to 240 DEG C and the humidity is 0 to 80 percent RH) service window, and has a very good application prospect in the field of fuel cells.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of proton exchange membranes that can be used in fuel cells, and in particular to a gel proton exchange membrane based on flexible zirconium-glutamic acid or UiO-66 series MOF-polybenzimidazole (PBI) and a preparation method thereof, and application thereof in dual-wideband fuel cells. Background Art

[0002] A fuel cell is a clean energy conversion device that directly converts the chemical energy of a fuel into electrical energy through an electrochemical reaction. It has the advantages of high energy conversion efficiency, low pollution, and low carbon emissions. From the perspective of energy conservation and environmental protection, fuel cells are one of the most promising power generation technologies. Among them, proton exchange membrane fuel cells (PEMFC) have the advantages of high output power density, fast startup speed, and small size. In the mid-1990s, Wainright et al. made PBI membranes have better proton conductivity by doping with phosphoric acid (PA), pioneering their application in HT-PEMFC. The proton conductivity of PA-PBI membranes strongly depends on the phosphoric acid doping level (ADL) in the membrane. With the increase of ADL, the proton conductivity increases significantly. However, the PA-PBI proton membrane has the problem of phosphoric acid loss, which leads to performance degradation, and its service window is limited to 120-200°C and a humidity-free environment.

[0003] On the one hand, in a high humidity environment, the phosphoric acid in the membrane is easily leaked and lost along with the condensed water vapor in the battery and the water generated from the redox reaction, making frequent starts or low-temperature cold starts difficult. On the other hand, in a low-temperature environment, the water inside the PEM may freeze, which not only blocks the proton transmission channel and causes a significant decrease in proton conduction performance, but also may cause microstructural damage to the membrane material due to ice, thereby affecting its overall physical stability and service life.

[0004] Therefore, in the face of the challenges faced by proton exchange membranes (PEMs) in low temperature and high humidity environments, it is crucial to develop fuel cell proton exchange membranes that have efficient and stable proton conductivity in low temperature environments and strong acid retention properties in high humidity environments.

[0005] Based on this, this work combines the gel membrane preparation process with flexible zirconium-glutamic acid or UiO-66 series MOFs to reveal a gel proton exchange membrane based on efficient acid retention characteristics and its preparation method and application. This proton exchange membrane exhibits excellent performance in a dual-wide range (temperature -20 to 240°C, humidity 0 to 80% RH) service window and has good application prospects in the field of fuel cells. Summary of the invention

[0006] In order to overcome the shortcomings of existing proton exchange membranes, the present invention provides a dual-wide domain-high acid retention gel-state mixed matrix PBI proton exchange membrane and a preparation method and application thereof.

[0007] The technical solution of the present invention is as follows:

[0008] A dual-wide domain-high acid retention gel-state mixed matrix PBI proton exchange membrane composed of polybenzimidazole, zirconium-based MOF, phosphoric acid and water;

[0009] in,

[0010] The structural formula of polybenzimidazole is one or more of the following:

[0011]

[0012] Wherein, n = 40 to 60;

[0013] Polybenzimidazole is a homopolymer or a random copolymer with a weight average molecular weight between 50,000 and 130,000;

[0014] The zirconium-based MOF is selected from a flexible zirconium-glutamic acid MOF (denoted as: L-Glu-Zr(P)) or a UiO-66 series MOF.

[0015] The flexible zirconium-glutamate MOF is synthesized by self-assembly with zirconium as the metal center and L-glutamate as the organic ligand; specifically, the preparation method of the flexible zirconium-glutamate MOF is as follows:

[0016] Dissolve zirconium salt (preferably ZrCl4) in water, then add L-glutamic acid under continuous stirring, transfer the reaction mixture to a reactor, react at 150°C for 2 hours, then cool to room temperature, centrifuge, wash, dry and grind to obtain a flexible zirconium-glutamate MOF (L-Glu-Zr(P), white powder).

[0017] The UiO-66 series MOF is prepared by solvent thermal reaction with zirconium as the metal center and dicarboxylic acid phenyl compound as the organic ligand; specifically, the preparation method of the UiO-66 series MOF is as follows:

[0018] The zirconium salt and the dicarboxylic acid phenyl compound are dissolved in DMF, an organic acid is added as a regulator, and then the reaction mixture is transferred to a reactor, and a solvent thermal reaction is carried out at 120 to 200° C. for 24 to 48 hours, and then cooled to room temperature, centrifuged, washed, dried, and ground to obtain UiO-66 series MOF (powder);

[0019] The zirconium salt is selected from one or both of zirconium tetrachloride (ZrCl4) and zirconium oxychloride (ZrOCl2);

[0020] The dicarboxylic acid phenyl compound is selected from one or both of terephthalic acid and 2-aminoterephthalic acid.

[0021] The organic acid is selected from acetic acid, formic acid or benzoic acid;

[0022] The prepared UiO-66 series MOFs are in the shape of regular octahedrons, with pore sizes ranging from 0.6 to 1.4 nm and particle sizes ranging from 100 to 1000 nm.

[0023] The preparation method of the dual-wide-domain-high-resistance acid gel-state mixed matrix PBI proton exchange membrane of the present invention comprises: using polyphosphoric acid as a solvent for polymerization reaction, adding flexible zirconium-glutamic acid (L-Glu-Zr(P)) or UiO-66 series MOF, and observing the phase transition from solution (sol) to gel-state membrane (gel) through the process of film scraping and polyphosphoric acid hydration to phosphoric acid;

[0024] The prepared membrane structure is already rich in phosphoric acid. Phosphoric acid and water are hydrated from polyphosphoric acid in the polymer solution, and proton transfer can be achieved without additional doping. The prepared membrane material has an acid doping level of 20-80 mol PA / PRU and 200-1000 m 2 / g specific surface area, 92.5% porosity, and pore size between 0.3 and 100 nm.

[0025] Specifically, the preparation method of the dual-wide domain-high acid retention gel-state mixed matrix PBI proton exchange membrane of the present invention is as follows:

[0026] (1) using polyphosphoric acid as a solvent and a polycondensation agent, in an inert gas atmosphere, an aromatic tetraamine monomer and a dicarboxylic acid phenyl compound monomer undergo a polycondensation reaction to obtain a polybenzimidazole polymer solution;

[0027] The aromatic tetraamine monomer is selected from one or more of 3,3'-diaminobenzidine and 1,2,4,5-tetraaminobenzene;

[0028] The dicarboxylic acid phenyl compound monomer is selected from one or more of terephthalic acid, isophthalic acid, 2,5-dihydroxyterephthalic acid, and 4,4'-dicarboxy diphenyl ether;

[0029] Preferably, the molar ratio of the aromatic tetraamine monomer to the dicarboxylic acid phenyl compound monomer is 1:1;

[0030] Preferably, the total mass fraction of the monomers in the polyphosphoric acid solvent is 1 to 15%;

[0031] The temperature of the polycondensation reaction is 170-200°C until the viscosity of the polymer solution reaches a moderate level and the reaction is terminated. The reaction time is 20-72 hours.

[0032] (2) adding zirconium-based MOF to the polybenzimidazole polymer solution obtained in step (1), stirring and blending to make it uniformly dispersed, to obtain a mixed matrix polymer solution;

[0033] The preferred stirring and blending time is 3 to 15 hours;

[0034] Based on the total mass of polybenzimidazole and zirconium-based MOF, the mass fraction of zirconium-based MOF is preferably 1 to 50%;

[0035] (3) scraping the mixed matrix polymer solution obtained in step (2) onto a glass substrate to complete the solution-gel phase transformation through the process of hydrating polyphosphoric acid into phosphoric acid, thereby obtaining the dual-wide-range-high-retention acid gel-state mixed matrix PBI proton exchange membrane;

[0036] The thickness of the scraped film is 20 to 1000 μm;

[0037] The temperature of phase conversion is 0-80°C, the humidity is 40-100%, and the time of phase conversion is 10-30h.

[0038] The dual-wide domain-high acid retention gel-state mixed matrix PBI proton exchange membrane of the present invention can be used in fuel cells.

[0039] Compared with the prior art, the present invention has the following beneficial effects:

[0040] (1) The preparation process of the present invention is mild, simple and feasible, low in cost, and the structural morphology of the material is easy to control, has good dispersibility and uniformity, and is easy to scale up;

[0041] (2) The proton exchange membrane prepared by the present invention not only has an ultra-high acid doping level and excellent proton conduction performance, but also has excellent acid retention capacity in a variety of temperature and humidity environments, avoiding the problems of low proton conductivity and serious acid loss existing in conventional membrane materials, and has a conductivity of -20°C / non-humidified: 0.0148S / cm, a conductivity of 240°C / 0%RH: 0.3422S / cm, an acid retention rate of 40°C / 80%RH (after 80 hours): 68.43%, an acid retention rate of 80°C / 40%RH (after 60 hours): 81.8%, and an acid retention rate of 160°C / 0%RH (after 60 hours): 83.82%;

[0042] (3) The proton exchange membrane prepared by the present invention exhibits operational flexibility and realizes the low temperature and high humidity service range of hydrogen fuel cells (temperature -20 to 240°C, humidity 0 to 80% RH);

[0043] (4) The present invention broadens the types and application scope of membrane materials used in fuel cell technology. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] Figure 1 : Proton conductivity performance diagram of some embodiments and comparative examples.

[0045] Figure 2 : Proton conductivity performance diagram of some embodiments and comparative examples.

[0046] Figure 3 : Proton conduction stability performance diagram of some embodiments and comparative examples (40°C-80%RH).

[0047] Figure 4 : Acid retention performance diagram of some embodiments and comparative examples (40°C-80%RH).

[0048] Figure 5 : Proton conduction stability performance diagram of some embodiments and comparative examples (80℃-40%RH).

[0049] Figure 6 : Acid retention performance diagram of some embodiments and comparative examples (80°C-40%RH).

[0050] Figure 7 : Proton conduction stability performance diagram of some embodiments and comparative examples (160℃-0%RH).

[0051] Figure 8 : Acid retention performance diagram of some embodiments and comparative examples (160°C-0%RH).

[0052] Fig. 9 : Comparative Example 2 fuel cell performance diagram (hydrogen / oxygen, no back pressure, no additional humidification).

[0053] Fig.10 : Example 3 fuel cell performance diagram (hydrogen / oxygen, no back pressure, no additional humidification).

[0054] Fig.11 :Example 3 Fuel cell stability diagram (160℃@0.2A / cm 2 , hydrogen / oxygen, no back pressure, no additional humidification).

[0055] Fig.12 : Cross-sectional morphology of Example 3 (dephosphorylation and freeze-drying).

[0056] Fig.13 : Surface morphology of Example 4 (dephosphorylation and freeze-drying).

[0057] Fig.14 : Cross-sectional morphology of Example 5 (dephosphorylation and freeze-drying).

[0058] Fig.15 : XRD patterns of UiO-66-NH2 and UiO-66 prepared by the present invention.

[0059] Fig.16 : Curves showing the proton conductivity of the mixed matrix proton membranes of the comparative examples and some embodiments of the present invention as a function of temperature (20-220°C).

[0060] Fig.17 : Curves showing proton conductivity changes with temperature for comparative examples and some examples of the present invention (-20 to 20°C). DETAILED DESCRIPTION

[0061] For ease of understanding of the present invention, the present invention will be more fully described in conjunction with the following examples. However, the present invention can be implemented in many different forms, and protection scope is not limited to the embodiments described herein. In addition, for those skilled in the art, without departing from the essence and scope of the present invention, the various modifications or improvements of the material composition and the dosage in these embodiments all belong to the scope of protection claimed in the present invention.

[0062] In the following embodiments,

[0063] The preparation method of L-Glu-Zr(P) is as follows:

[0064] Weigh ZrCl4 (0.200 g, 0.001 mol) and dissolve it in 10 mL of room temperature water. Then, slowly add L-glutamic acid (L-Glu, 0.13 g, 0.001 mol) to the above solution under continuous stirring. Transfer the mixed solution to a 150 mL reactor and place it in a 150 ° C oven to react for 2 hours. After cooling, wash it by multiple ethanol centrifugation. Finally, dry and grind the product obtained by centrifugation to obtain white L-Glu-Zr (P) powder.

[0065] The preparation method of UiO-66-NH2 is as follows:

[0066] Weigh ZrCl4 (0.400g, 0.004mol) and 2-aminoterephthalic acid (BDC-NH2, 0.31g, 0.002mol), add 20mL DMF and 0.6mL acetic acid regulator and mix well. Transfer the mixed solution to a 150mL reactor, place it in a 120℃ oven to react for 24h, and after cooling, wash it with DMF and ethanol several times and centrifuge it. Finally, the product obtained by centrifugation is dried and ground to obtain a light yellow UiO-66-NH2 powder.

[0067] The preparation method of UiO-66 is as follows:

[0068] Weigh ZrCl4 (0.190 g, 0.002 mol) and terephthalic acid (BDC, 0.133 g, 0.001 mol), add 81.7 mL DMF and 2.29 mL acetic acid as a regulator and mix well. Transfer the mixed solution to a 150 mL reactor, place it in a 120 ° C oven to react for 24 hours, and after cooling, wash it with DMF and ethanol several times and centrifuge it. Finally, the product obtained by centrifugation is dried and ground to obtain white UiO-66 powder.

[0069] Comparative Example 1:

[0070] The commercial PBI membrane provided by PBIPerformance was immersed in 85 wt % phosphoric acid solution for 168 hours to complete acid doping and obtain a conventional PA / PBI membrane.

[0071] The conventional PA / PBI membrane obtained in Comparative Example 1 was analyzed and tested:

[0072] Experimental results: Phosphoric acid doping level: 7.73 mol PA / PRU.

[0073] Proton conductivity (without additional humidification): 25℃ conductivity: 0.015S / cm, 80℃ conductivity: 0.051S / cm, 200℃ conductivity: 0.096S / cm, 240℃ conductivity: 0.070S / cm.

[0074] Comparative Example 2:

[0075] (1) Weigh 2.0692 g of 3,3'-diaminobenzidine and 1.6043 g of terephthalic acid respectively, pour them into a three-mouth reaction kettle, and then add a solvent and 180 g of polyphosphoric acid as a polycondensation agent into the reaction kettle. The reaction is carried out under a nitrogen atmosphere, and the oil bath heating method is used, and the temperature is gradually increased to 190°C for 25 hours.

[0076] (2) The polymer solution was poured onto a glass substrate and the film was scraped using a scraping frame to control the thickness of the cast film to be 250 μm.

[0077] (3) The glass plate and the membrane were placed in an environment with room temperature and 60% RH for 12 hours to allow the membrane precursor to undergo phase transformation, thereby obtaining the proton exchange membrane of Comparative Example 2.

[0078] The proton exchange membrane structure of Comparative Example 2 is para-PBI, and the membrane does not contain L-Glu-Zr(P).

[0079] The proton exchange membrane of the control group obtained in Comparative Example 2 was analyzed and tested:

[0080] The membrane performance of the control group proton exchange membrane obtained in this example was tested, and the experimental results were: conductivity at -20°C / non-humidification: 0.0054S / cm, conductivity at 240°C / 0%RH: 0.2624S / cm, conductivity at 40°C / 80%RH (after 80 hours): 0.1131S / cm, conductivity at 80°C / 40%RH (after 60 hours): 0.0788S / cm, conductivity at 160°C / 0%RH (after 60 hours): 0.1604S / cm.

[0081] The control group proton exchange membrane obtained in this example was tested for acid retention capacity, and the experimental results showed that the acid retention rate at 40°C / 80%RH (after 80 hours) was 47.22%, the acid retention rate at 80°C / 40%RH (after 60 hours) was 61.3%, and the acid retention rate at 160°C / 0%RH (after 60 hours) was 57.41%.

[0082] The proton exchange membrane of the control group obtained in this example was used to test the fuel cell performance. The experimental results showed that at 30°C, the peak power density was 146 mW / cm 2 , 200℃, peak power density is 755mW / cm 2 .

[0083] Comparative Example 3:

[0084] (1) Weigh 5.3000 g of 3,3'-diaminobenzidine, 0.5137 g of terephthalic acid, and 3.5956 g of isophthalic acid respectively, pour them into a three-mouth reaction kettle, and then add a solvent and 100 g of polyphosphoric acid as a polycondensation agent into the reaction kettle. The reaction is carried out under a nitrogen atmosphere, and the oil bath heating method is used, and the temperature is gradually increased to 190°C for 20 hours.

[0085] (2) The polymer solution was poured onto a glass substrate and the film was scraped using a scraping frame to control the thickness of the cast film to be 250 μm.

[0086] (3) The glass plate and the membrane were placed in an environment with room temperature and 60% RH for 12 hours to allow the membrane precursor to undergo phase transformation, thereby obtaining the proton exchange membrane of Comparative Example 3.

[0087] The proton exchange membrane structure of Comparative Example 3 is mrp-PBI, and the membrane does not contain L-Glu-Zr(P).

[0088] The proton exchange membrane of the control group obtained in Comparative Example 3 was analyzed and tested:

[0089] The proton exchange membrane of the control group obtained in this example was tested for membrane performance, and the experimental results showed that the conductivity at 240° C. was 0.1566 S / cm.

[0090] Embodiment 1:

[0091] (1) Weigh 2.0692 g of 3,3'-diaminobenzidine and 1.6043 g of terephthalic acid respectively, pour them into a three-mouth reaction kettle, and then add a solvent and 180 g of polyphosphoric acid as a polycondensation agent into the reaction kettle. The reaction is carried out under a nitrogen atmosphere, and the oil bath heating method is used, and the temperature is gradually increased to 190°C for 35 hours.

[0092] (2) 0.1933 g of L-Glu-Zr(P) was added to the polymer solution and stirred for 8 h, wherein the mass concentration of L-Glu-Zr(P) was 5% (relative to the total mass of polybenzimidazole and particles).

[0093] (3) The polymer solution was poured onto a glass substrate and the film was scraped using a scraping frame to control the thickness of the cast film to be 200 μm.

[0094] (4) The membrane was placed in an environment of room temperature and 70% RH for 12 hours to allow the membrane precursor to undergo a phase transformation, thereby obtaining a gel-state proton exchange membrane based on flexible amino acid MOF-polybenzimidazole, para-PBI-(L-Glu-Zr(P))-5%.

[0095] The mixed matrix gel-type high temperature proton exchange membrane para-PBI-(L-Glu-Zr(P))-5% obtained in Example 1 was analyzed and tested:

[0096] The mixed matrix gel-type high-temperature proton exchange membrane obtained in this example was subjected to membrane performance testing, and the experimental results were: conductivity at -20°C / non-humidification: 0.0063S / cm, conductivity at 240°C / 0%RH: 0.2661S / cm, conductivity at 40°C / 80%RH (after 80 hours): 0.2341S / cm, conductivity at 80°C / 40%RH (after 60 hours): 0.12224S / cm, conductivity at 160°C / 0%RH (after 60 hours): 0.1707S / cm.

[0097] The mixed matrix gel-type high temperature proton exchange membrane obtained in this example was tested for acid retention capacity, and the experimental results showed: acid retention rate at 40°C / 80%RH (after 80 hours): 52.11%, acid retention rate at 80°C / 40%RH (after 60 hours): 69.3%, and acid retention rate at 160°C / 0%RH (after 60 hours): 64.04%.

[0098] Embodiment 2:

[0099] (1) Weigh 2.0692 g of 3,3'-diaminobenzidine and 1.6043 g of terephthalic acid respectively, pour them into a three-mouth reaction kettle, and then add a solvent and 180 g of polyphosphoric acid as a polycondensation agent into the reaction kettle. The reaction is carried out under a nitrogen atmosphere, and the oil bath heating method is used, and the temperature is gradually increased to 190°C for 35 hours.

[0100] (2) 0.4082 g of L-Glu-Zr(P) was added to the polymer solution and stirred for 8 h, wherein the mass concentration of L-Glu-Zr(P) was 10% (relative to the total mass of polybenzimidazole and particles).

[0101] (3) The polymer solution was poured onto a glass substrate and the film was scraped using a scraping frame to control the thickness of the cast film to be 250 μm.

[0102] (4) The membrane was placed in an environment of room temperature and 60% RH for 12 hours to allow the membrane precursor to undergo a phase transformation, thereby obtaining a gel-state proton exchange membrane based on flexible amino acid MOF-polybenzimidazole, para-PBI-(L-Glu-Zr(P))-10%.

[0103] The mixed matrix gel-type high temperature proton exchange membrane para-PBI-(L-Glu-Zr(P))-10% obtained in Example 2 was analyzed and tested:

[0104] The mixed matrix gel-type high temperature proton exchange membrane obtained in this example was subjected to membrane performance testing, and the experimental results were: conductivity at -20°C / non-humidification: 0.0099 S / cm, conductivity at 240°C / 0% RH: 0.2745 S / cm, conductivity at 40°C / 80% RH (after 80 hours): 0.2036 S / cm, conductivity at 80°C / 40% RH (after 60 hours): 0.17157 S / cm, conductivity at 160°C / 0% RH (after 60 hours): 0.1897 S / cm.

[0105] The mixed matrix gel-type high temperature proton exchange membrane obtained in this example was tested for acid retention capacity, and the experimental results showed that the acid retention rate at 40°C / 80%RH (after 80 hours) was 57.37%, the acid retention rate at 80°C / 40%RH (after 60 hours) was 82.00%, and the acid retention rate at 160°C / 0%RH (after 60 hours) was 67.14%.

[0106] Embodiment 3:

[0107] (1) Weigh 2.0692 g of 3,3'-diaminobenzidine and 1.6043 g of terephthalic acid respectively, pour them into a three-mouth reaction kettle, and then add a solvent and 180 g of polyphosphoric acid as a polycondensation agent into the reaction kettle. The reaction is carried out under a nitrogen atmosphere, and the oil bath heating method is used, and the temperature is gradually increased to 190°C for 35 hours.

[0108] (2) 0.6482 g of L-Glu-Zr(P) was added to the polymer solution and stirred for 8 h, wherein the mass concentration of L-Glu-Zr(P) was 15% (relative to the total mass of polybenzimidazole and particles).

[0109] (3) The polymer solution was poured onto a glass substrate and the film was scraped using a scraping frame to control the thickness of the cast film to be 250 μm.

[0110] (4) The membrane was placed in an environment of room temperature and 60% RH for 12 hours to allow the membrane precursor to undergo a phase transformation, thereby obtaining a gel proton exchange membrane based on flexible amino acid MOF-polybenzimidazole, para-PBI-(L-Glu-Zr(P))-15%.

[0111] The mixed matrix gel-type high temperature proton exchange membrane para-PBI-(L-Glu-Zr(P))-15% obtained in Example 3 was analyzed and tested:

[0112] The mixed matrix gel-type high-temperature proton exchange membrane obtained in this example was subjected to membrane performance testing, and the experimental results were as follows: conductivity at -20°C / non-humidification: 0.0148 S / cm, conductivity at 240°C / 0% RH: 0.3422 S / cm, conductivity at 40°C / 80% RH (after 80 hours): 0.1536 S / cm, conductivity at 80°C / 40% RH (after 60 hours): 0.1872 S / cm, conductivity at 160°C / 0% RH (after 60 hours): 0.2616 S / cm.

[0113] The mixed matrix gel-type high temperature proton exchange membrane obtained in this example was tested for acid retention capacity, and the experimental results showed: acid retention rate at 40°C / 80%RH (after 80 hours): 68.43%, acid retention rate at 80°C / 40%RH (after 60 hours): 81.8%, and acid retention rate at 160°C / 0%RH (after 60 hours): 83.82%.

[0114] The mixed matrix gel high temperature proton exchange membrane obtained in this example was used to test the fuel cell performance and stability. The experimental results showed that at 30°C, the peak power density was 354 mW / cm 2 , 200℃, peak power density is 1160mW / cm 2 160℃@0.2A / cm 2 The voltage decay rate is 0.29μV / h (575 hours in total).

[0115] Embodiment 4:

[0116] (1) Weigh 2.0692 g of 3,3'-diaminobenzidine and 1.6043 g of terephthalic acid respectively, pour them into a three-mouth reaction kettle, and then add solvent and 180 g of polyphosphoric acid as a condensation agent into the reaction kettle. React under a nitrogen atmosphere, use an oil bath heating method, and program the temperature to 190°C for 35 hours.

[0117] (2) 0.9184 g of L-Glu-Zr(P) was added to the polymer solution and mixed for 8 hours, wherein the mass concentration of L-Glu-Zr(P) was 20% (relative to the total mass of polybenzimidazole and particles).

[0118] (3) The polymer solution was poured onto a glass substrate and the film was scraped using a scraping frame to control the thickness of the cast film to be 250 μm.

[0119] (4) The membrane was placed in an environment of room temperature and 70% RH for 12 hours to allow the membrane precursor to undergo a phase transformation, thereby obtaining a gel-state proton exchange membrane based on flexible amino acid MOF-polybenzimidazole, para-PBI-(L-Glu-Zr(P))-20%.

[0120] The mixed matrix gel-type high temperature proton exchange membrane para-PBI-(L-Glu-Zr(P))-20% obtained in Example 4 was analyzed and tested:

[0121] The mixed matrix gel-type high temperature proton exchange membrane obtained in this example was subjected to membrane performance testing, and the experimental results were: -20°C / non-humidified conductivity: 0.0106S / cm, 240°C / 0%RH conductivity: 0.3061S / cm, 40°C / 80%RH (after 80 hours): 0.19173S / cm, 80°C / 40%RH (after 60 hours): 0.16223S / cm, 160°C / 0%RH (after 60 hours): 0.2086S / cm.

[0122] The mixed matrix gel-type high temperature proton exchange membrane obtained in this example was tested for acid retention capacity, and the experimental results showed: acid retention rate at 40°C / 80%RH (after 80 hours): 60.99%, acid retention rate at 80°C / 40%RH (after 60 hours): 77.6%, and acid retention rate at 160°C / 0%RH (after 60 hours): 73.15%.

[0123] Embodiment 5:

[0124] (1) Weigh 2.0692 g of 3,3'-diaminobenzidine and 1.6043 g of terephthalic acid respectively, pour them into a three-mouth reaction kettle, and then add a solvent and 180 g of polyphosphoric acid as a polycondensation agent into the reaction kettle. The reaction is carried out under a nitrogen atmosphere, and the oil bath heating method is used, and the temperature is gradually increased to 190°C for 35 hours.

[0125] (2) 1.5744 g of L-Glu-Zr(P) was added to the polymer solution and stirred for 8 h, wherein the mass concentration of L-Glu-Zr(P) was 30% (relative to the total mass of polybenzimidazole and particles).

[0126] (3) The polymer solution was poured onto a glass substrate and the film was scraped using a scraping frame to control the thickness of the cast film to be 250 μm.

[0127] (4) The membrane was placed in an environment of room temperature and 60% RH for 12 hours to allow the membrane precursor to undergo a phase transformation, thereby obtaining a gel proton exchange membrane based on flexible amino acid MOF-polybenzimidazole, para-PBI-(L-Glu-Zr(P))-30%.

[0128] The mixed matrix gel-type high temperature proton exchange membrane para-PBI-(L-Glu-Zr(P))-30% obtained in Example 5 was analyzed and tested:

[0129] The mixed matrix gel-type high-temperature proton exchange membrane obtained in this example was subjected to membrane performance testing, and the experimental results were: conductivity at -20°C / non-humidification: 0.0075 S / cm, conductivity at 240°C / 0% RH: 0.2363 S / cm, conductivity at 40°C / 80% RH (after 80 hours): 0.1657 S / cm, conductivity at 80°C / 40% RH (after 60 hours): 0.2296 S / cm, conductivity at 160°C / 0% RH (after 60 hours): 0.15281 S / cm.

[0130] The mixed matrix gel-type high temperature proton exchange membrane obtained in this example was tested for acid retention capacity, and the experimental results showed: acid retention rate at 40°C / 80%RH (after 80 hours): 62.90%, acid retention rate at 80°C / 40%RH (after 60 hours): 59.5%, and acid retention rate at 160°C / 0%RH (after 60 hours): 60.44%.

[0131] Embodiment 6:

[0132] (1) Weigh 4.2399 g of 3,3'-diaminobenzidine, 0.4109 g of terephthalic acid, and 2.8764 g of isophthalic acid respectively, pour them into a three-mouth reaction kettle, and then add a solvent and 80 g of polyphosphoric acid as a condensation agent into the reaction kettle. The reaction is carried out under a nitrogen atmosphere, and the oil bath heating method is used, and the temperature is gradually increased to 190°C for 20 hours.

[0133] (2) 0.5666 g of L-Glu-Zr(P) was added to the polymer solution and stirred and blended for 8 hours, wherein the mass concentration of L-Glu-Zr(P) was 7% (relative to the total mass of polybenzimidazole and particles).

[0134] (3) The polymer solution was poured onto a glass substrate and the film was scraped using a scraping frame to control the thickness of the cast film to be 250 μm.

[0135] (4) The membrane was placed in an environment of room temperature and 60% RH for 12 hours to allow the membrane precursor to undergo a phase transformation, thereby obtaining a gel-state proton exchange membrane mrp-PBI-(L-Glu-Zr(P))-7% based on flexible amino acid MOF-polybenzimidazole.

[0136] The mixed matrix gel-type high temperature proton exchange membrane mrp-PBI-(L-Glu-Zr(P))-7% obtained in Example 6 was analyzed and tested:

[0137] The mixed matrix gel-type high temperature proton exchange membrane obtained in this example was subjected to membrane performance testing, and the experimental results showed that the conductivity at 240° C. was 0.2526 S / cm.

[0138] Embodiment 7:

[0139] (1) Weigh 4.2399 g of 3,3'-diaminobenzidine, 0.4109 g of terephthalic acid and 2.8764 g of isophthalic acid respectively and pour them into a three-mouth reaction kettle, then add a solvent and 80 g of polyphosphoric acid as a polycondensation agent into the reaction kettle. The reaction is carried out under a nitrogen atmosphere, and the oil bath heating method is used, and the temperature is gradually increased to 190°C for 20 hours.

[0140] (2) 1.3283 g of L-Glu-Zr(P) was added to the polymer solution and stirred for 8 h, wherein the mass concentration of L-Glu-Zr(P) was 15% (relative to the total mass of polybenzimidazole and particles).

[0141] (3) The polymer solution was poured onto a glass substrate and the film was scraped using a scraping frame to control the thickness of the cast film to be 250 μm.

[0142] (4) The membrane was placed in an environment of room temperature and 60% RH for 12 hours to allow the membrane precursor to undergo a phase transformation, thereby obtaining a gel-state proton exchange membrane mrp-PBI-(L-Glu-Zr(P))-15% based on flexible amino acid MOF-polybenzimidazole.

[0143] The mixed matrix gel-type high temperature proton exchange membrane mrp-PBI-(L-Glu-Zr(P))-15% obtained in Example 7 was analyzed and tested:

[0144] The mixed matrix gel-type high temperature proton exchange membrane obtained in this example was subjected to membrane performance testing, and the experimental results showed that the conductivity at 240° C. was 0.2270 S / cm.

[0145] Embodiment 8:

[0146] (1) Weigh 4.2399 g of 3,3'-diaminobenzidine, 0.4109 g of terephthalic acid and 2.8764 g of isophthalic acid respectively and pour them into a three-mouth reaction kettle, then add a solvent and 80 g of polyphosphoric acid as a polycondensation agent into the reaction kettle. The reaction is carried out under a nitrogen atmosphere, and the oil bath heating method is used, and the temperature is gradually increased to 190°C for 20 hours.

[0147] (2) 3.2259 g of L-Glu-Zr(P) was added to the polymer solution and stirred for 8 h, wherein the mass concentration of L-Glu-Zr(P) was 30% (relative to the total mass of polybenzimidazole and particles).

[0148] (3) The polymer solution was poured onto a glass substrate and the film was scraped using a scraping frame to control the thickness of the cast film to be 250 μm.

[0149] (4) The membrane was placed in an environment of room temperature and 60% RH for 12 hours to allow the membrane precursor to undergo a phase transformation, thereby obtaining a gel-state proton exchange membrane mrp-PBI-(L-Glu-Zr(P))-30% based on flexible amino acid MOF-polybenzimidazole.

[0150] The mixed matrix gel-type high temperature proton exchange membrane mrp-PBI-(L-Glu-Zr(P))-30% obtained in Example 8 was analyzed and tested:

[0151] The mixed matrix gel-type high temperature proton exchange membrane obtained in this example was subjected to membrane performance testing, and the experimental results showed that the conductivity at 240° C. was 0.1787 S / cm.

[0152] Example 9

[0153] (1) Weigh 3.1358 g of 3,3'-diaminobenzidine and 2.4312 g of terephthalic acid respectively, pour them into a three-mouth reaction kettle, and then add a solvent and 180 g of polyphosphoric acid as a condensation agent into the reaction kettle. The reaction is carried out under a nitrogen atmosphere and heated in an oil bath at 190°C for 25 hours.

[0154] (2) Add 0.4082 g (10 wt%) UiO-66-NH2 powder in small amounts and several times at 180°C, continue heating and stirring for 4 h until the mixture is uniformly mixed, and obtain a casting solution.

[0155] (3) The casting solution obtained in (2) was directly cast on a clean glass plate in an air environment, and the film was scraped using a film applicator to control the film thickness to be 250 μm. The film was placed in an environment of room temperature and 60% RH for sol-gel phase transformation, and after standing for 24 hours, the proton membrane of Example 9 was obtained.

[0156] The gel-state mixed matrix proton membrane obtained in this embodiment was subjected to membrane performance testing, and the experimental results were as follows: proton conductivity at 160°C: 0.319S / cm. The acid doping level was 61.21 molPA / PRU. After being kept at 80°C and 40% RH for 50 hours, the acid doping level was 13.16 molPA / PRU, and the retention rate was 51.97%. After being kept at 160°C and 0% RH for 60 hours, the acid doping level was 16.22 molPA / PRU, and the retention rate was 62.19%. The proton conductivity was retained at 80°C and 40% RH for 60 hours, and 85.55% was retained. After being kept at 160°C and 0% RH for 70 hours, 85.19% was retained.

[0157] Example 10

[0158] (1) Weigh 3.1358 g of 3,3'-diaminobenzidine and 2.4312 g of terephthalic acid respectively, pour them into a three-mouth reaction kettle, and then add a solvent and 180 g of polyphosphoric acid as a polycondensation agent into the reaction kettle. The reaction is carried out under a nitrogen atmosphere, using an oil bath heating method, and the reaction is carried out at 190°C for 27 hours.

[0159] (2) Add 0.6483 g (15 wt%) UiO-66-NH2 powder in small amounts and several times at 180°C, continue heating and stirring for 4 h until the mixture is uniformly mixed, and obtain a casting solution.

[0160] (3) The casting solution obtained in (2) was directly cast on a clean glass plate in an air environment, and the film was scraped using a film applicator to control the film thickness to be 250 μm. The film was placed in an environment of room temperature and 60% RH for sol-gel phase transformation, and after standing for 24 hours, the proton membrane of Example 10 was obtained.

[0161] The preparation method of the metal organic framework material UiO-66-NH2 in this embodiment is as follows: a certain amount of ZrCl4 and 2-aminoterephthalic acid (BDC-NH2) are weighed according to a molar ratio of 1:1, and 20 mL of DMF and 0.6 mL of acetic acid regulator are added and mixed. The mixed solution is transferred to a 150 mL reactor, placed in a 120 ° C oven for reaction for 24 hours, and after cooling, it is washed and centrifuged through multiple DMF and ethanol washings. Finally, the product obtained by centrifugation is dried and ground to obtain a light yellow UiO-66-NH2 powder.

[0162] The gel-state mixed matrix proton membrane obtained in this embodiment was tested for membrane performance, and the experimental results showed that the proton conductivity at 160°C was 0.250S / cm. The acid doping level was 53.26mol PA / PRU. After being kept at 80°C and 40% RH for 50 hours, the acid doping level was 20.47mol PA / PRU, and the retention rate was 59.73%. After being kept at 160°C and 0% RH for 60 hours, the acid doping level was 27.83mol PA / PRU, and the retention rate was 73.14%. The proton conductivity was retained at 80°C and 40% RH for 60 hours, and 87.54% was retained at 160°C and 0% RH for 70 hours.

[0163] Embodiment 11

[0164] (1) Weigh 3.1358 g of 3,3'-diaminobenzidine and 2.4312 g of terephthalic acid respectively, pour them into a three-mouth reaction kettle, and then add a solvent and 180 g of polyphosphoric acid as a polycondensation agent into the reaction kettle. The reaction is carried out under a nitrogen atmosphere, using an oil bath heating method, and the reaction is carried out at 190°C for 28 hours.

[0165] (2) Add 0.9184 g (20 wt%) UiO-66-NH2 powder in small amounts and several times at 180°C, continue heating and stirring for 4 h until the mixture is uniformly mixed, and obtain a casting solution.

[0166] (3) The casting solution obtained in (2) was directly cast on a clean glass plate in an air environment, and the film was scraped using a film applicator to control the film thickness to be 250 μm. The film was placed in an environment of room temperature and 60% RH for sol-gel phase transformation, and after standing for 24 hours, the proton membrane of Example 11 was obtained.

[0167] The preparation method of the metal organic framework material UiO-66-NH2 in this embodiment is as follows: a certain amount of ZrCl4 and 2-aminoterephthalic acid (BDC-NH2) are weighed according to a molar ratio of 1:1, and 20 mL of DMF and 0.6 mL of acetic acid regulator are added and mixed. The mixed solution is transferred to a 150 mL reactor, placed in a 120 ° C oven for reaction for 24 hours, and after cooling, it is washed and centrifuged through multiple DMF and ethanol washings. Finally, the product obtained by centrifugation is dried and ground to obtain a light yellow UiO-66-NH2 powder.

[0168] The gel-state mixed matrix proton membrane obtained in this embodiment was tested for membrane performance, and the experimental results showed that the proton conductivity at 160°C was 0.231S / cm. The acid doping level was 46.64 mol PA / PRU. After being kept at 80°C and 40% RH for 50 hours, the acid doping level was 21.28 mol PA / PRU, and the retention rate was 59.79%. After being kept at 160°C and 0% RH for 60 hours, the acid doping level was 28.85 mol PA / PRU, and the retention rate was 71.16%. The proton conductivity was retained at 80°C and 40% RH for 60 hours, and 81.22% was retained after being kept at 160°C and 0% RH for 70 hours.

[0169] Example 12

[0170] (1) Weigh 3.1358 g of 3,3'-diaminobenzidine and 2.4312 g of terephthalic acid respectively, pour them into a three-mouth reaction kettle, and then add a solvent and 180 g of polyphosphoric acid as a polycondensation agent into the reaction kettle. The reaction is carried out under a nitrogen atmosphere, using an oil bath heating method, and the reaction is carried out at 190°C for 28 hours.

[0171] (2) At 180° C., 0.4082 g (10 wt %) of UiO-66 powder was added in small amounts and several times, and heating and stirring were continued for 4 h until the mixture was uniformly mixed to obtain a casting solution.

[0172] (3) The casting solution obtained in (2) was directly cast on a clean glass plate in an air environment, and the film was scraped using a film applicator to control the film thickness to be 250 μm. The film was placed in an environment of room temperature and 60% RH for sol-gel phase transformation, and after standing for 24 hours, the proton membrane of Example 12 was obtained.

[0173] The gel-state mixed matrix proton membrane obtained in this example was tested for membrane performance, and the experimental results showed that the proton conductivity at 160° C. was 0.262 S / cm.

[0174] This work combines the gel membrane preparation process with flexible zirconium-glutamic acid (L-Glu-Zr(P)) or UiO-66 series MOF to develop a gel proton exchange membrane with high acid retention properties and its preparation method and application. This proton exchange membrane exhibits excellent performance in a wide range of use (temperature -20 to 240°C, humidity 0 to 80% RH).

[0175] In fuel cells, due to the water vapor environment generated by condensation, flexible L-Glu-Zr(P) can spontaneously absorb these water molecules that easily cause phosphoric acid loss, thereby extending the service life of the proton exchange membrane. L-Glu-Zr(P) itself has extremely high proton conductivity, which makes the PBI proton exchange membrane doped with L-Glu-Zr(P) significantly improved in proton conductivity, thereby effectively alleviating the difficulty of cold start of fuel cells at low temperatures and the poor performance of fuel cells at high temperatures.

[0176] In addition, the UiO-66 series MOFs, with their excellent thermal and chemical stability, enable the mixed matrix proton membrane doped with UiO-66 to maintain excellent performance over a wide temperature range of -20°C to 220°C. The porous structure of UiO-66 and its alkaline functional groups effectively limit the loss of phosphoric acid and significantly improve the acid retention capacity under low temperature and high humidity environments. Due to the effective retention of phosphoric acid and the microporous mass transfer effect of UiO-66, the proton membrane exhibits excellent proton conductivity at both high and low temperatures. The porous lamellar structure inside the membrane increases the transport path of protons and facilitates the rapid migration of protons within the membrane. This membrane not only maintains stable performance over a wide temperature range, but also maintains high proton conductivity and excellent acid retention capacity at different water contents. At the same time, the retention capacity of phosphoric acid is further enhanced through specific intermolecular interactions or structural design.

Claims

1. A double-wide domain-high acid retention gel-state mixed matrix PBI proton exchange membrane, characterized in that: It is composed of polybenzimidazole, zirconium-based MOF, phosphoric acid and water; in, The structural formula of polybenzimidazole is one or more of the following: Wherein, n = 40 to 60; Polybenzimidazole is a homopolymer or a random copolymer with a weight average molecular weight between 50,000 and 130,000; The zirconium-based MOF is selected from flexible zirconium-glutamate MOF or UiO-66 series MOF.

2. The double-wide domain-high acid retention gel-state mixed matrix PBI proton exchange membrane according to claim 1, characterized in that: Flexible zirconium-glutamate MOF is synthesized by self-assembly with zirconium as the metal center and L-glutamate as the organic ligand; UiO-66 series MOF is prepared by solvothermal reaction with zirconium as the metal center and dicarboxylic acid phenyl compounds as organic ligands.

3. The method for preparing the double-wide domain-high acid retention gel-state mixed matrix PBI proton exchange membrane according to claim 1, characterized in that: The preparation method is as follows: (1) using polyphosphoric acid as a solvent and a polycondensation agent, in an inert gas atmosphere, an aromatic tetraamine monomer and a dicarboxylic acid phenyl compound monomer undergo a polycondensation reaction to obtain a polybenzimidazole polymer solution; The aromatic tetraamine monomer is selected from one or more of 3,3'-diaminobenzidine and 1,2,4,5-tetraaminobenzene; The dicarboxylic acid phenyl compound monomer is selected from one or more of terephthalic acid, isophthalic acid, 2,5-dihydroxyterephthalic acid, and 4,4'-dicarboxy diphenyl ether; (2) adding zirconium-based MOF to the polybenzimidazole polymer solution obtained in step (1), stirring and blending to make it uniformly dispersed, to obtain a mixed matrix polymer solution; (3) Scrape the mixed matrix polymer solution obtained in step (2) onto a glass substrate to complete the solution-gel phase transformation through the process of hydrating polyphosphoric acid into phosphoric acid, thereby obtaining the dual-wide-domain-high-retention acid gel-state mixed matrix PBI proton exchange membrane.

4. The preparation method according to claim 3, characterized in that: In step (1), the molar ratio of the aromatic tetraamine monomer to the dicarboxylic acid phenyl compound monomer is 1:

1.

5. The preparation method according to claim 3, characterized in that: In step (1), the total mass fraction of the monomers in the polyphosphoric acid solvent is 1 to 15%.

6. The preparation method according to claim 3, characterized in that: In step (1), the temperature of the polycondensation reaction is 170 to 200° C., and the reaction time is 20 to 72 hours.

7. The preparation method according to claim 3, characterized in that: In step (2), based on the total mass of polybenzimidazole and zirconium-based MOF, the mass fraction of zirconium-based MOF is 1 to 50%.

8. The preparation method according to claim 3, characterized in that: In step (3), the thickness of the scraped film is between 20 and 1000 μm.

9. The preparation method according to claim 3, characterized in that: In step (3), the temperature of the phase inversion is 0 to 80° C., the humidity is 40 to 100%, and the time of the phase inversion is 10 to 30 hours.

10. Use of the dual-wide domain-high acid retention gel mixed matrix PBI proton exchange membrane as claimed in claim 1 in a fuel cell.

Citation Information

Patent Citations

  • Polybenzimidazole gel type high-temperature proton exchange membrane with functional / branched structure and preparation method of polybenzimidazole gel type high-temperature proton exchange membrane

    CN115275290A

  • Polymer hybrid proton exchange membrane modified by-PO3H2 / - NH2 acid-base pair functionalized metal organic framework

    CN117209825A

  • Proton exchange membrane for use in proton exchange membrane fuel cells

    WO2010022963A2

Cited By

  • Phosphoric acid doped polybenzimidazole high-temperature proton exchange membrane and preparation method thereof

    CN119890375A