Polyetherimide coated ceramic particle coating diaphragm and preparation method thereof

By covering polyetherimide and nano aluminum trioxide on the surface of ceramic particles, the problems of uneven distribution and agglomeration of ceramic particles are solved, significantly improving the electrochemical performance and capacity retention rate of lithium-ion batteries, and achieving a more uniform Coating effect and higher battery performance.

CN118920015AActive Publication Date: 2024-11-08GUIZHOU MEILING POWER SUPPLY CO LTD

Patent Information

Application Number
CN202411183868.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-08
Estimated Expiration
2044-08-27

AI Technical Summary

Technical Problem

During the preparation process, traditional ceramic separators are prone to uneven distribution and agglomeration of ceramic particles, which affects the coating effect and battery performance, resulting in uneven current density, poor rate performance and cycle performance of lithium-ion batteries.

Method used

The nano aluminum trioxide particles are coated with polyetherimide, and the protective layer is formed on the surface of the ceramic particles to reduce agglomeration, improve the uniformity of the particles and the coating effect, and is modified by hydroxyl groups and silane coupling agent. Enhance the binding force and dielectric constant of the particles.

Benefits of technology

It significantly improves the electrochemical performance of ceramic separators, increases the wetting performance and dielectric constant of the separators, improves the electrochemical window and capacity retention rate of lithium-ion batteries, and ensures efficient battery performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118920015A_ABST
    Figure CN118920015A_ABST
Patent Text Reader

Abstract

The invention discloses a polyetherimide coated ceramic particle coating diaphragm in the technical field of lithium ion battery materials, which is characterized in that S1, 4, 4 '-diaminodiphenyl ether and bisphenol A type diether dianhydride are respectively dissolved in N, N-dimethylacetamide to obtain an ODA solution and a BPADA solution; the preparation method comprises the following steps: dissolving 4-hydroxyphthalic anhydride in N, N-dimethylacetamide to obtain a 4-HP solution; s2, dropwise adding the BPADA solution into the ODA solution, and dropwise adding the 4-HP solution into the ODA solution to obtain a polyetherimide solution; s3, respectively adding aluminum nitrate and ammonium bicarbonate into water and an ethanol solvent to obtain an aluminum nitrate solution and an ammonium bicarbonate solution; adding polyethylene glycol into the ammonium bicarbonate solution, dropwise adding aluminum nitrate into the ammonium bicarbonate solution, and washing and drying the precipitate to obtain nano Al2O3 particles; s4, preparing the nano aluminum oxide coated with the polyetherimide; and S5, preparing the coating diaphragm. The lithium ion battery (LCO / / HC) assembled by adopting the diaphragm still has 64% of capacity retention ratio at 100C multiplying power, and still has 91% of capacity retention ratio after 1000 cycles.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of lithium ion battery materials, and in particular to a polyetherimide-coated ceramic particle-coated diaphragm and a preparation method thereof. Background Art

[0002] Lithium-ion battery separator is one of the key components of lithium-ion batteries. The separator can maintain the relative position of the battery during use, prevent the positive and negative electrodes from directly contacting and short-circuiting, and provide a channel for the smooth migration of lithium ions during the charging and discharging process. The chemical stability, thermal stability, mechanical strength, porosity, etc. of lithium-ion battery separators have an important impact on the performance, safety and life of lithium-ion batteries.

[0003] Ceramic diaphragm is a type of diaphragm that is improved on the basis of traditional lithium-ion battery diaphragm. It is achieved by coating a layer of ceramic material (such as alumina, boehmite, etc.) on the surface of the diaphragm group (such as polyethylene, polypropylene, etc.). This structure makes the ceramic diaphragm have better thermal stability and higher mechanical strength, and improves the performance and safety of lithium-ion batteries. The traditional ceramic diaphragm preparation process is: ceramic powder preparation, slurry preparation, coating, and drying. The main factor affecting the performance of ceramic diaphragms is the uneven ceramic particle slurry. This is due to the interaction between the electrostatic force and other interactions between the ceramic particles, which makes the particles with smaller particle sizes agglomerate together and form many irregular agglomerates, resulting in the ceramic particle slurry being coated on the base film, affecting the coating effect.

[0004] During the preparation process of ceramic diaphragms, ceramic particles are prone to uneven distribution and agglomeration, which affects the coating thickness and leads to diaphragm defects. There are also problems such as weak bonding between the binder and the base film, and ceramic particles falling off during long-term cycle use. These problems will lead to uneven current density inside lithium-ion batteries, poor rate performance and cycle performance. Summary of the invention

[0005] The present invention aims to provide a polyetherimide-coated ceramic particle coated diaphragm and a preparation method thereof, which can be more easily and evenly coated on a base film, increase the wetting performance and dielectric constant of the diaphragm, and significantly improve the electrochemical performance of the battery.

[0006] In order to achieve the above object, the present invention provides the following technical solutions:

[0007] A method for preparing a polyetherimide-coated ceramic particle-coated diaphragm comprises the following steps:

[0008] S1. Under an inert gas atmosphere, 4,4'-diaminodiphenyl ether (ODA) and bisphenol A diether dianhydride (BPADA) are dissolved in N,N-dimethylacetamide (DMAc) to obtain an ODA solution and a BPADA solution respectively; 4-hydroxyphthalic anhydride (4-HP) is dissolved in N,N-dimethylacetamide (DMAc) to obtain a 4-HP solution;

[0009] S2, BPADA solution is added dropwise to ODA solution, inert gas is introduced for stirring, and then 4-HP solution is added dropwise to ODA solution to obtain polyetherimide solution;

[0010] S3, adding aluminum nitrate and ammonium bicarbonate to a solvent consisting of water and ethanol to obtain an aluminum nitrate solution and an ammonium bicarbonate solution; adding polyethylene glycol to the ammonium bicarbonate solution, and then adding aluminum nitrate dropwise to the ammonium bicarbonate solution, and after continuous stirring, washing, drying, grinding, calcining, and then sieving to obtain nano-Al2O3 particles;

[0011] S4, adding toluene to obtain a suspension, adding KH570 silane coupling agent to the suspension for full reaction, washing and drying the precipitate obtained by the reaction, and placing it in a container filled with ethanol, introducing an inert gas into the container, and adding a polyetherimide solution to the container; dissolving triethylamine and acetic anhydride in N, N-dimethylacetamide to obtain a triethylamine solution and an acetic anhydride solution, respectively, adding the triethylamine solution and the acetic anhydride solution to the container for stirring and reacting, washing and drying the product obtained by the reaction to obtain a polyetherimide-coated nano-alumina material;

[0012] S5. Evenly mix polyetherimide-coated nano-aluminum oxide particles, sodium hydroxymethyl cellulose and styrene-butadiene rubber, add a mixed solvent of deionized water and ethanol, and stir until the mixture is evenly mixed to obtain a slurry; coat the obtained slurry on the front side of a commercial polyethylene diaphragm, then dry it, and coat the back side in the same way to obtain a polyetherimide-coated nano-aluminum oxide coated diaphragm.

[0013] Working principle and beneficial effects of the present invention:

[0014] The end-capping of the hydroxyl groups in S1 is an inventive point. The hydroxyl groups replace the heterogeneous groups when the polymer ends are capped, which promotes the subsequent coating of nanoparticles; S2 uses polyethylene glycol PEG6000 with a molecular weight of 6000. The surface activity reduces the agglomeration of nano inorganic ceramic particles during nucleation, and obtains Al2O3 particles with an average particle size of 30nm; S4 uses KH570 silane coupling agent on the surface of ceramic particles, which helps the surface of ceramic particles to form surface functional groups combined with the above-mentioned second step. Please inquire about the role of silane coupling agent modification for details. In the second step, only {C 37 H24 O6N2} polyetherimide molecular solution, generally the generated polyetherimide is {C 37 H 24 O6N2} molecules, that is, the chemical composition of the addition polymer is the same as the initial monomer, that is, {C 37 H 24 O6N2}n polymer products. The formation of polymers is a continuous intensification reaction. The secondary end-capping mechanism here is that the polymer is {C 37 H 24 The hydroxyl groups of O6N2} react with the amino groups on the surface of nano-aluminum oxide to form chemical bonds, making {C 37 H 24 O6N2} is tightly connected with nano-aluminum oxide during the addition polymerization reaction to form a dense protective layer.

[0015] Polyetherimide is a type of polyimide with ether bonds in its molecular chain structure. It is widely used in aerospace, electronic instrumentation and other fields due to its high temperature resistance and low dielectric loss. Coating polyetherimide on the surface of inorganic nano-ceramic particles can reduce the agglomeration between inorganic ceramic particles. The specific principle can refer to carbon-coated nano-lithium iron phosphate, which makes it easier to evenly coat the particles on the base film and increases the air permeability of the diaphragm. The improvement in wetting performance comes from the large number of functional groups remaining on the surface of the coated particles.

[0016] The present application uses polyetherimide to coat nano-aluminum trioxide particles. Polyetherimide forms a protective transition layer on the surface of inorganic nanoparticles, which increases the strength and dielectric constant of the ceramic diaphragm. Polyetherimide is cross-linked and hydroxylated, which increases the breakdown strength and hydrophilicity of the diaphragm and the wettability of the electrolyte. Polymer coating of inorganic nanoparticles reduces the agglomeration of nanoparticles and makes the nanoparticles more evenly dispersed.

[0017] The polyetherimide-coated ceramic particles coated diaphragm in the present application have uniform coating thickness, with a thickness range of less than 5% at five points, a liquid absorption rate of 480%, no shrinkage after baking at 140°C for 6 hours, an electrochemical window of 5V, and an ionic conductivity of 2.05mS / cm. The lithium-ion battery (LCO / / HC) assembled with the diaphragm still has a capacity retention rate of 64% at a rate of 100C, and a capacity retention rate of 91% after 1000 cycles.

[0018] Optimally, the BPADA solution is added dropwise to the ODA solution at a rate of 1-2 ml / min.

[0019] Optimally, the solvent in S3 is composed of water:ethanol in a volume ratio of 1:1.

[0020] Optimally, the molecular weight of the polyethylene glycol is 6,000.

[0021] Preferably, S3 grinds the obtained powder and puts it into a microwave heating furnace for calcination at 1200°C for 2 hours. After cooling, it is ball-milled and sieved to obtain Al2O3 particles with an average particle size of 30 nm.

[0022] Preferably, KH570 silane coupling agent is added dropwise to the suspension at a rate of 1.5 ml / min, and ultrasonication is continued for 1 h until the dispersion is uniform, and the suspension is reacted at 120° C. for 12 h.

[0023] Optimally, the volume ratio of ionized water to ethanol in the S5 mixed solvent is 1:1.

[0024] Optimally, S3 is washed with ethanol; the precipitate in S4 is washed with toluene, and the product obtained by the reaction is washed with ethanol.

[0025] Optimally, S5 dries the solvent at 60°C. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 is the rate performance diagram of the diaphragm;

[0027] Figure 2 The cycle performance diagram is shown in Figure 2. DETAILED DESCRIPTION

[0028] The following is further described in detail through specific implementation methods:

[0029] Example 1: Al2O3 particles + diaphragm

[0030] 2.5 g of aluminum oxide particles were mixed with sodium carboxymethyl cellulose (CMC) and styrene-butadiene rubber (SBR) in a mass ratio of 94:3:3, 25 ml of a mixed solvent of deionized water and ethanol in a volume ratio of 1:1 was added, and the mixture was stirred for 4 hours until the mixture was uniformly mixed; the resulting slurry was coated on the front side of a commercial polyethylene (PE) diaphragm, the solvent was then dried at 60°C, and the reverse side was coated in the same manner to obtain the diaphragm of Example 1.

[0031] Example 2: A nano-aluminum oxide particle diaphragm was prepared by the same method.

[0032] 20.02g aluminum nitrate (Al(NO3)3) and 60.07g ammonium bicarbonate (NH4HCO3) were added to 200ml of a solvent consisting of water and ethanol in a volume ratio of 1:1, and dissolved by ultrasonication for 1h;

[0033] Add 4.24 g of polyethylene glycol (PEG6000, surfactant) with a molecular weight of 6000 to the NH4HCO3 solution and stir for 1 hour to fully dissolve. Add Al(NO3)3 solution to the NH4HCO3 solution at a rate of 1.5 mL / min. After ultrasonic treatment for 15 minutes, continue stirring for 30 minutes. Then filter and separate the precipitate, wash it with a mixed solvent of water and ethanol for 3-5 times, and dry it in a vacuum drying oven at 80°C for 2 hours. Grind the obtained powder and calcine it in a microwave heating furnace, and keep it warm at 1200°C for 2 hours. After cooling, ball mill the sample and sieve it to obtain Al2O3 particles with an average particle size of 30 nm;

[0034] 2.5 g of Al2O3 particles were mixed evenly with sodium carboxymethyl cellulose (CMC) and styrene-butadiene rubber (SBR) in a mass ratio of 94:3:3, and 25 ml of a mixed solvent of deionized water and ethanol in a volume ratio of 1:1 was added, and stirred for 4 hours until the mixture was evenly mixed; the resulting slurry was coated on the front side of a commercial polyethylene (PE) diaphragm, and then the solvent was dried at 60°C, and the back side was coated in the same way to obtain a nano-aluminum oxide particle diaphragm.

[0035] Example 3: A method for preparing a polyetherimide-coated ceramic particle-coated diaphragm, comprising the following steps:

[0036] S1. Under an inert gas atmosphere (argon, helium), 4.42 g of 4,4'-diaminodiphenyl ether (ODA) and 10.39 g of bisphenol A diether dianhydride (BPADA) were dissolved in 100 ml of N, N-dimethylacetamide (DMAc) and ultrasonicated for 1 h; 0.34 g of 4-hydroxyphthalic anhydride (4-HP) was dissolved in 5 ml of N, N-dimethylacetamide (DMAc) and ultrasonicated for 1 h;

[0037] S2. At room temperature, add the dispersed ODA solution into a 500 ml three-necked flask, introduce inert gas and stir for 1 hour; drop the dispersed BPADA solution into the flask at a rate of 1 ml / min, and continue stirring for 8 hours after the addition is completed (this process generates a polyetherimide solution); then drop the 4-HP solution into the flask (this process caps the hydroxyl groups of the generated polyetherimide and increases the affinity of the polyetherimide with the nanoparticles).

[0038] S3, add 20.02g aluminum nitrate (Al(NO3)3) and 60.07g ammonium bicarbonate (NH4HCO3) into 200ml of a solvent consisting of water and ethanol in a volume ratio of 1:1, and dissolve by ultrasonication for 1h;

[0039] Add 4.24g of polyethylene glycol (PEG6000, surfactant) with a molecular weight of 6000 to the NH4HCO3 solution and stir for 1h to fully dissolve. Add Al(NO3)3 solution to the NH4HCO3 solution at a rate of 1.5mL / min, ultrasonicate for 15min, and continue stirring for 30min. Then filter and separate the precipitate, wash it with a mixed solvent of water and ethanol for 3-5 times, and dry it in a vacuum drying oven at 80℃ for 2h. Grind the obtained powder and calcine it in a microwave heating furnace, and keep it warm at 1200℃ for 2h. After cooling, ball mill the sample and sieve it to obtain Al2O3 particles with an average particle size of 30nm.

[0040] S4, put 10g nano Al2O3 particles in a 1000ml flask, add 650ml toluene, and ultrasonically disperse for 1h to form a suspension; add 11ml KH570 silane coupling agent, slowly drop it at a dropping speed of 1.5ml / min, and continue ultrasonically for 1h until it is evenly dispersed; react the suspension at 120℃ for 12h (surface amination); then wash the precipitate with toluene 3-5 times, and after drying, place the particles in 150ml ethanol in a three-necked flask with argon gas again, and ultrasonically disperse for 1h; add the polyetherimide solution prepared above, dissolve 6.67g triethylamine and 6.74g acetic anhydride in 20ml N, N-dimethylacetamide (DMAc) respectively, ultrasonically for 1h, add the triethylamine solution and acetic anhydride solution to the three-necked flask, and stir for 24h before the reaction ends; wash the product with ethanol 3-5 times, and dry it at 80℃ to obtain a polyetherimide-coated nano-alumina material;

[0041] S5. Mix 2.5 g of polyetherimide-coated nano-aluminum oxide particles with sodium carboxymethyl cellulose (CMC) and styrene-butadiene rubber (SBR) in a mass ratio of 94:3:3, add 25 ml of a mixed solvent of deionized water: ethanol in a volume ratio of 1:1, and stir for 4 hours until the mixture is uniform; apply the resulting slurry on the front side of a commercial polyethylene (PE) diaphragm, then dry the solvent at 60°C, and apply the same method on the back side to obtain a polyetherimide-coated nano-aluminum oxide coated diaphragm.

[0042] Example 4: PE original diaphragm.

[0043] The diaphragm-assembled lithium-ion batteries prepared in Examples 1 to 4 were subjected to rate performance and cycle tests. Figure 1 and Figure 2 As shown, from Figure 1 and Figure 2 It can be seen that the polyetherimide-coated nano-aluminum oxide-coated diaphragm prepared in Example 3 is superior to Example 1, Example 2 and Example 4 in terms of rate performance and number of cycles.

[0044] The polyetherimide-coated ceramic particles coated diaphragm in the present application have uniform coating thickness, with a thickness range of less than 5% at five points, a liquid absorption rate of 480%, no shrinkage after baking at 140°C for 6 hours, an electrochemical window of 5V, and an ionic conductivity of 2.05mS / cm. The lithium-ion battery (LCO / / HC) assembled with the diaphragm still has a capacity retention rate of 64% at a rate of 100C, and a capacity retention rate of 91% after 1000 cycles.

Claims

1. A method for preparing a polyetherimide-coated ceramic particle-coated diaphragm, Features: The following steps are included: S1. Under an inert gas atmosphere, 4,4'-diaminodiphenyl ether (ODA) and bisphenol A diether dianhydride (BPADA) are dissolved in N,N-dimethylacetamide (DMAc) to obtain an ODA solution and a BPADA solution respectively; 4-hydroxyphthalic anhydride (4-HP) is dissolved in N,N-dimethylacetamide (DMAc) to obtain a 4-HP solution; S2, BPADA solution is added dropwise to ODA solution, inert gas is introduced for stirring, and then 4-HP solution is added dropwise to ODA solution to obtain polyetherimide solution; S3, adding aluminum nitrate and ammonium bicarbonate to a solvent composed of water and ethanol to obtain an aluminum nitrate solution and an ammonium bicarbonate solution; adding polyethylene glycol to the ammonium bicarbonate solution, and then adding aluminum nitrate dropwise to the ammonium bicarbonate solution, and after continuous stirring, washing, drying, grinding, calcining, and then sieving to obtain nano-Al 2 O 3 Particles; S4, Nano-Al 2 O 3 Toluene is added to the particles to obtain a suspension, a KH570 silane coupling agent is added dropwise to the suspension to fully react, a precipitate obtained by the reaction is washed and dried, and then placed in a container filled with ethanol, an inert gas is introduced into the container, and a polyetherimide solution is added to the container; triethylamine and acetic anhydride are respectively dissolved in N,N-dimethylacetamide to obtain a triethylamine solution and an acetic anhydride solution, the triethylamine solution and the acetic anhydride solution are added to the container for stirring reaction, and the product obtained by the reaction is washed and dried to obtain a polyetherimide-coated nano-aluminum oxide material; S5. Evenly mix polyetherimide-coated nano-aluminum oxide particles, sodium hydroxymethyl cellulose and styrene-butadiene rubber, add a mixed solvent of deionized water and ethanol, and stir until the mixture is evenly mixed to obtain a slurry; coat the obtained slurry on the front side of a commercial polyethylene diaphragm, then dry it, and coat the back side in the same way to obtain a polyetherimide-coated nano-aluminum oxide coated diaphragm.

2. The method for preparing the etherimide-coated ceramic particles coated diaphragm according to claim 1, Features: The BPADA solution was added dropwise to the ODA solution at a rate of 1-2 ml / min.

3. The method for preparing the etherimide-coated ceramic particles coated diaphragm according to claim 2, Features: S3 is a solvent composed of water and ethanol in a volume ratio of 1:

1.

4. The method for preparing the etherimide-coated ceramic particles coated diaphragm according to claim 3, Features: The molecular weight of polyethylene glycol is 6000.

5. The method for preparing the etherimide-coated ceramic particles coated diaphragm according to claim 4, Features: S3 grinds the obtained powder and puts it into a microwave heating furnace for calcination at 1200°C for 2 hours. After cooling, it is ball-milled and sieved to obtain Al2O3 with an average particle size of 30 nm. 2 O 3 Particles.

6. The method for preparing the etherimide-coated ceramic particles coated diaphragm according to claim 5, Features: KH570 silane coupling agent was added dropwise to the suspension at a rate of 1.5 ml / min, and ultrasonic treatment was continued for 1 h until the dispersion was uniform. The suspension was reacted at 120° C. for 12 h.

7. The method for preparing the etherimide-coated ceramic particles coated diaphragm according to claim 6, Features: The volume ratio of ionized water and ethanol in the S5 mixed solvent is 1:

1.

8. The method for preparing the etherimide-coated ceramic particles coated diaphragm according to claim 7, Features: S3 was washed with ethanol; the precipitate in S4 was washed with toluene, and the product obtained by the reaction was washed with ethanol.

9. The method for preparing the etherimide-coated ceramic particles coated diaphragm according to claim 8, Features: S5: Dry the solvent at 60°C. 10 . The diaphragm prepared according to the method for preparing a diaphragm coated with etherimide-coated ceramic particles according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Coaxial aluminum oxide coated polyimide nanofiber membrane and preparation method thereof

    CN111455476A

  • Novel polyimide microsphere slurry and coated diaphragm thereof

    CN114883746A

Cited By

  • Early-strength high-fluidity geopolymer grouting material and preparation method thereof