Method for regulating and controlling active region of quantum dot laser based on ultrasonic assistance
By using ultrasonic assisted regulation method in indium arsenide quantum dot lasers, combining high-frequency ultrasonic interaction with indium gallium arsenic thin layer, the As/P interchange effect and uneven quantum dot distribution caused by increased thickness are solved, and the problem of Stable coverage of laser wavelength and room temperature lasing effect.
Patent Information
- Application Number
- CN202410863647.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-29
- Publication Date
- 2024-11-08
AI Technical Summary
In the process of regulating indium arsenide quantum dot lasers, the increase in thickness leads to poor suppression of As/P interchange effect, and the quantum dot size distribution is uneven and the density decreases, affecting the stability of the laser wavelength.
Using ultrasonic-assisted regulation method, by growing indium gallium arsenic thin layer on indium phosphide substrate and applying high-frequency ultrasonic waves during the growth process, the density of thin layers and the activity of gallium atoms are improved, and the energy level interval of quantum dots is adjusted to form Uniform quantum dot distribution enhances the ability to suppress As/P interchange effect.
It effectively suppresses the As/P interchange effect under thickness conditions, avoids the decrease in quantum dot density, ensures that the laser wavelength covers the 1.3-1.7μm communication band, and realizes room temperature laser emission.
Smart Images

Figure CN118920271A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of preparation of quantum dot laser active regions, and in particular relates to a method for regulating the quantum dot laser active region based on ultrasound assistance. Background Art
[0002] Compared with one-dimensional confined quantum well materials, quantum dots have higher state density and stronger carrier confinement, so quantum dot lasers have better temperature stability and smaller frequency chirp effect. Indium arsenide materials have high radiative recombination luminescence efficiency and the luminescence wavelength range can cover 1.0-1.9 microns. As a C-band material for optical communication applications, it has attracted widespread attention. Due to the small lattice mismatch between indium arsenide and indium phosphide, the reduction of internal compressive strain during epitaxial growth makes the luminescence wavelength of indium arsenide quantum dots longer. In order to meet the needs of 1.55-micron optical communications, it is necessary to develop control technology for the active area of quantum dots.
[0003] There are three main existing control technologies. The first is to design a special waveguide structure to achieve continuous laser lasing; the second is to add Ga to indium arsenide quantum dots to adjust the energy level interval and thus adjust the laser wavelength; the third is to insert a GaAs thin layer under the quantum dots to adjust the laser wavelength. The above methods all intervene in the growth process of quantum dots, or dope the quantum dots, or change the growth environment of the quantum dots. This method reduces the photoluminescence intensity of the quantum dot active area material, which is not conducive to the production of lasers with good performance. Secondly, there is an As / P exchange effect in the process of growing indium arsenide quantum dots on indium phosphide substrates, which increases the difficulty of controlling quantum dots.
[0004] In addition, the existing method of inserting a GaAs thin layer is to suppress the As / P exchange effect. However, if the thickness of the thin layer is too thin, it will affect the suppression effect of the As / P exchange effect. If the thickness of the thin layer is too thick, it will not only affect the uniformity of the quantum dot size distribution, but also cause a significant decrease in the quantum dot density, thereby introducing new defects to affect the laser wavelength.
[0005] Based on this, a new control method is urgently needed, which can effectively avoid the introduction of new disadvantages such as the uneven distribution of quantum dot size and a significant decrease in the density of quantum dots while increasing the thickness of the thin layer to enhance the inhibition of the As / P exchange effect. Summary of the invention
[0006] Purpose of the invention: The technical problem to be solved by the present invention is to provide a new type of control method, which can effectively avoid the introduction of new disadvantages such as the uneven distribution of quantum dot size and the substantial decrease in quantum dot density while increasing the thickness of the thin layer to enhance the suppression of the As / P exchange effect, so as to effectively control the laser wavelength.
[0007] Technical solution: The present invention is based on a method for ultrasound-assisted regulation of the active region of a quantum dot laser, comprising the following steps:
[0008] (1) growing an indium phosphide buffer layer, an indium phosphide cladding layer and an indium gallium arsenic phosphide lower waveguide layer on an indium phosphide substrate in sequence;
[0009] (2) growing an InGaAs thin layer with a thickness of 20-60 nm on the InGaAsP lower waveguide layer, and applying high-frequency ultrasonic waves to the InGaAs thin layer;
[0010] (3) epitaxially growing a multi-period indium arsenide quantum dot active layer on the indium gallium arsenide thin layer;
[0011] (4) An InGaAsP upper waveguide layer, an InP cap layer, and an InGaAs contact layer are grown on the InAs quantum dot active layer in sequence to complete the regulation of the active region of the quantum dot laser.
[0012] The present invention adds an indium gallium arsenide thin layer with a thickness of 20-60nm between the indium gallium arsenide phosphide lower waveguide layer and the indium arsenide quantum dots, and before growing the indium arsenide quantum dots, combines high-frequency ultrasound to improve the surface quality of the substrate, and through the interaction between the high-frequency ultrasound and the indium gallium arsenide thin layer, improves the density of the thin indium gallium arsenide thin layer, forms a surface morphology that is conducive to the nucleation of indium arsenide quantum dots, controls the quantum dot size and increases the quantum dot density, makes the quantum dot distribution more uniform, and effectively improves the ability to suppress the arsenic / phosphorus exchange effect under the condition of increasing the thickness, and effectively avoids the introduction of other new defects (non-uniformity of quantum dot size distribution and a significant decrease in the density of the guide quantum dots) caused by the increase in the thickness of the thin layer. At the same time, based on the high-frequency ultrasound, the activity of gallium atoms on the surface of the ultra-thin layer is stimulated, and the energy level interval of the indium arsenide quantum dots is adjusted by gallium atoms, so as to realize the room temperature lasing of the indium arsenide quantum dot laser.
[0013] Furthermore, in step (2) of the control method, the growth temperature of the InGaAs thin layer is 520-560°C, the high-frequency ultrasonic frequency is 60-150kHz, and the ultrasonic power is 1-10W.
[0014] Furthermore, in step (1) of the control method, the growth temperature of the indium phosphide buffer layer is 600-640° C., and the growth thickness is 180-220 nm.
[0015] Furthermore, in step (1) of the control method, the growth temperature of the indium phosphide cladding is 600-640° C., and the growth thickness is 1-1.2 μm.
[0016] Furthermore, in step (1) of the control method, the growth temperature of the InGaAsP lower waveguide layer is 520-560° C., and the growth thickness is 180-220 nm.
[0017] Furthermore, in step (3) of the control method, the period number of the multi-period indium arsenide quantum dot active layer is 1-20, each layer is indium arsenide quantum dots, and the quantum dots are covered with a 20-50 nm thick indium gallium arsenic phosphide barrier layer.
[0018] Furthermore, in step (4) of the control method, the growth temperature of the InGaAsP upper waveguide layer is 520-560° C., and the growth thickness is 180-220 nm.
[0019] Furthermore, in step (4) of the control method, the growth temperature of the indium phosphide capping layer is 620-660° C., and the growth thickness is 1.2-1.4 μm.
[0020] Furthermore, in step (4) of the control method, the growth temperature of the InGaAs contact layer is 520-560° C., and the growth thickness is 80-120 nm.
[0021] Beneficial effect: Compared with the prior art, the significant advantages of the present invention are: the regulation method can be based on a 20-60nm thick InGaAs thin layer, by combining high-frequency ultrasonic reaction, and utilizing the interaction between high-frequency ultrasonic waves and the InGaAs thin layer to form a surface morphology that is conducive to the nucleation of InAs quantum dots, which can not only improve the ability to suppress the arsenic / phosphorus exchange effect, but also increase the activity of surface gallium atoms, utilize gallium atoms to regulate the energy level interval of InAs quantum dots, and realize room temperature lasing of InAs quantum dot lasers; at the same time, it can also effectively avoid the introduction of other new defects, so that the emission wavelength of InAs quantum dot lasers can cover the entire communication band (1.3-1.7μm). BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 It is a schematic structural diagram of the active region of the quantum dot laser of the present invention;
[0023] Figure 2 This is the photoluminescence spectrum of the active region of the quantum dot laser in Example 1 of the present invention. DETAILED DESCRIPTION
[0024] The technical solution of the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments.
[0025] Example 1
[0026] This embodiment 1 is based on a method for ultrasound-assisted regulation of the active region of a quantum dot laser. Figure 1 As shown, the following steps are included:
[0027] (1) An indium phosphide buffer layer is grown on an n-type indium phosphide substrate at a growth temperature of 620° C. and a thickness of 200 nm.
[0028] (2) An indium phosphide cladding layer is epitaxially grown on the indium phosphide buffer layer at a growth temperature of 620°C and a thickness of 1.1 μm.
[0029] (3) A lattice-matched InGaAsP lower waveguide layer is grown on the InP cladding at a growth temperature of 540°C and a thickness of 200 nm.
[0030] (4) A thin InGaAs layer is grown on the InGaAsP lower waveguide layer at a growth temperature of 540°C and a thickness of 40 nm.
[0031] (5) High-frequency ultrasonic waves are applied to the InGaAs thin layer, the frequency of the high-frequency ultrasonic waves is 100 kHz, the ultrasonic welding head is made of ceramic material, the welding head is in a dot matrix shape, and the ultrasonic power is 5 W.
[0032] (6) An InAs quantum dot active layer with 7 layers of epitaxial growth is formed on the InGaAs thin layer, each layer is an InAs quantum dot, the growth temperature is 480°C, and the thickness is 2ML; an InGaAsP barrier layer is formed on the quantum dots, the growth temperature is 480°C, and the thickness is 40nm.
[0033] (7) An InGaAsP upper waveguide layer is deposited on the InAs quantum dot active layer at a growth temperature of 540°C and a thickness of 200 nm.
[0034] (8) depositing an indium phosphide cap layer on the indium gallium arsenic phosphide upper waveguide layer at a growth temperature of 640°C and a thickness of 1.3 μm;
[0035] (9) Depositing an InGaAs contact layer on the InP cap layer, the growth temperature is 540°C, the thickness is 100 nm, and the preparation of the active region of the quantum dot laser is completed. According to the above method, the wavelength of the laser active region can be made to be 1.5 μm, such as Figure 2 shown.
[0036] Example 2
[0037] The method for ultrasound-assisted regulation of the active region of a quantum dot laser in Example 2 includes the following steps:
[0038] (1) An indium phosphide buffer layer is grown on an n-type indium phosphide substrate at a growth temperature of 600° C. and a thickness of 180 nm.
[0039] (2) An indium phosphide cladding layer is epitaxially grown on the indium phosphide buffer layer at a growth temperature of 600°C and a thickness of 1 μm.
[0040] (3) A lattice-matched InGaAsP lower waveguide layer is grown on the InP cladding at a growth temperature of 520°C and a thickness of 180 nm.
[0041] (4) A thin InGaAs layer is grown on the InGaAsP lower waveguide layer at a growth temperature of 520°C and a thickness of 20 nm.
[0042] (5) High-frequency ultrasonic waves are applied to the InGaAs thin layer, the frequency of the high-frequency ultrasonic waves is 60 kHz, the ultrasonic welding head is made of ceramic material, the welding head is in a dot matrix shape, and the ultrasonic power is 10 W.
[0043] (6) An InAs quantum dot active layer with 5 layers of epitaxial growth is formed on the InGaAs thin layer, each layer is an InAs quantum dot, the growth temperature is 480°C, and the thickness is 2ML; an InGaAsP barrier layer is formed on the quantum dots, the growth temperature is 480°C, and the thickness is 20nm.
[0044] (7) An InGaAsP upper waveguide layer is deposited on the InAs quantum dot active layer at a growth temperature of 520°C and a thickness of 180 nm.
[0045] (8) depositing an indium phosphide cap layer on the indium gallium arsenic phosphide upper waveguide layer at a growth temperature of 620°C and a thickness of 1.2 μm;
[0046] (9) An InGaAs contact layer is deposited on the InP cap layer at a growth temperature of 520°C and a thickness of 80 nm, thereby completing the preparation of the active region of the quantum dot laser.
[0047] Example 3
[0048] The method for ultrasound-assisted regulation of the active region of a quantum dot laser in Example 3 includes the following steps:
[0049] (1) An indium phosphide buffer layer is grown on an n-type indium phosphide substrate at a growth temperature of 640° C. and a thickness of 220 nm.
[0050] (2) An indium phosphide cladding layer is epitaxially grown on the indium phosphide buffer layer at a growth temperature of 640°C and a thickness of 1.2 μm.
[0051] (3) A lattice-matched InGaAsP lower waveguide layer is grown on the InP cladding at a growth temperature of 560°C and a thickness of 220 nm.
[0052] (4) A thin InGaAs layer is grown on the InGaAsP lower waveguide layer at a growth temperature of 560°C and a thickness of 60 nm.
[0053] (5) High-frequency ultrasonic waves are applied to the InGaAs thin layer, the frequency of the high-frequency ultrasonic waves is 150 kHz, the ultrasonic welding head is made of ceramic material, the welding head is in a matrix shape, and the ultrasonic power is 1 W.
[0054] (6) An InAs quantum dot active layer with 15 layers of epitaxial growth is formed on the InGaAs thin layer, each layer is an InAs quantum dot, the growth temperature is 480°C, and the thickness is 2ML; an InGaAsP barrier layer is covered on the quantum dots, the growth temperature is 480°C, and the thickness is 50nm.
[0055] (7) An InGaAsP upper waveguide layer is deposited on the InAs quantum dot active layer at a growth temperature of 560°C and a thickness of 220 nm.
[0056] (8) depositing an indium phosphide cap layer on the indium gallium arsenic phosphide upper waveguide layer at a growth temperature of 660°C and a thickness of 1.4 μm;
[0057] (9) An InGaAs contact layer is deposited on the InP cap layer at a growth temperature of 560°C and a thickness of 120 nm, thereby completing the preparation of the active region of the quantum dot laser.
[0058] In addition, based on the above embodiments, the surface morphology of the InGaAs thin layer is changed by adjusting the ultrasonic frequency and power, thereby controlling the quantum dot size and quantum dot density, and thus affecting the laser wavelength. In addition, the laser wavelength can also be controlled by changing the number of quantum dot layers. The combination of the two can make the InAs quantum dot laser emission wavelength cover the entire communication band (1.3-1.7μm).
Claims
1. A method for controlling the active region of a quantum dot laser based on ultrasound assistance. It is characterized in that The steps include: (1) growing an indium phosphide buffer layer, an indium phosphide cladding layer and an indium gallium arsenic phosphide lower waveguide layer on an indium phosphide substrate in sequence; (2) growing an InGaAs thin layer with a thickness of 20-60 nm on the InGaAsP lower waveguide layer, and applying high-frequency ultrasonic waves to the InGaAs thin layer; (3) epitaxially growing a multi-period indium arsenide quantum dot active layer on the indium gallium arsenide thin layer; (4) An InGaAsP upper waveguide layer, an InP cap layer, and an InGaAs contact layer are grown on the InAs quantum dot active layer in sequence to complete the regulation of the active region of the quantum dot laser.
2. According to claim 1, the method for controlling the active region of a quantum dot laser based on ultrasound assistance, It is characterized in that In step (2), the growth temperature of the InGaAs thin layer is 520-560° C., the high-frequency ultrasonic frequency is 60-150 kHz, and the ultrasonic power is 1-10 W.
3. According to the method for controlling the active region of a quantum dot laser based on ultrasound assistance according to claim 1, It is characterized in that In step (1), the growth temperature of the indium phosphide buffer layer is 600-640° C., and the thickness of the growth is 180-220 nm.
4. The method for controlling the active region of a quantum dot laser based on ultrasound assistance according to claim 1, It is characterized in that In step (1), the growth temperature of the indium phosphide cladding is 600-640° C., and the grown thickness is 1-1.2 μm.
5. The method for controlling the active region of a quantum dot laser based on ultrasound assistance according to claim 1, It is characterized in that In step (1), the growth temperature of the InGaAsP lower waveguide layer is 520-560° C., and the grown thickness is 180-220 nm.
6. The method for controlling the active region of a quantum dot laser based on ultrasound assistance according to claim 1, It is characterized in that In step (3), the period number of the multi-period indium arsenide quantum dot active layer is 1-20, each layer is indium arsenide quantum dots, and the quantum dots are covered with a 20-50 nm thick indium gallium arsenic phosphide barrier layer.
7. The method for controlling the active region of a quantum dot laser based on ultrasound assistance according to claim 1, It is characterized in that In step (4), the growth temperature of the InGaAsP upper waveguide layer is 520-560° C., and the grown thickness is 180-220 nm.
8. The method for controlling the active region of a quantum dot laser based on ultrasound assistance according to claim 1, It is characterized in that In step (4), the growth temperature of the indium phosphide cap layer is 620-660° C., and the grown thickness is 1.2-1.4 μm.
9. The method for controlling the active region of a quantum dot laser based on ultrasound assistance according to claim 1, It is characterized in that In step (4), the growth temperature of the InGaAs contact layer is 520-560° C., and the growth thickness is 80-120 nm.