Ultralow interface thermal resistance thin-layer heat-conducting gasket and preparation method thereof
By coating the copper foil with a high viscosity meltable composite material layer and a polyfluoroluminescence isolation film, the problems of high interface thermal resistance and liquid metal leakage corrosion of existing thermal conductivity materials are solved, and efficient thermal conduction and equipment stability are achieved.
Patent Information
- Application Number
- CN202410988195.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-08
AI Technical Summary
The existing thermally conductive materials have high interface thermal resistance during the heat transfer process, resulting in low heat dissipation efficiency, and liquid metal thermally conductive materials are prone to leakage and corrosion, affecting the reliability and service life of the equipment.
Ultra-low interface thermal resistance thin-layer thermal gasket coated with a copper foil surface coated with a layer of meltable composite material and a polyfluoroluminescence isolation film. The composite material is made of phase-change paraffin, butyl rubber, epoxy resin and graphene powder, with High viscosity and low melting point can be tightly adhered to the surface of the copper foil in a molten state, reducing interface thermal resistance and preventing corrosion.
It achieves the effects of high thermal conductivity and low thermal resistance, enhances the heat dissipation performance and stability of the equipment, avoids leakage and corrosion problems of liquid metal heat conduction flakes, and extends the service life of the equipment.
Smart Images

Figure CN118921944A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a thermal interface material, in particular to an ultra-low interface thermal resistance thin-layer thermal conductive pad and a preparation method thereof. Background Art
[0002] With the development of electronic products, automobiles, aerospace and other fields, the power density of equipment is increasing, resulting in a large amount of heat generated inside the equipment. In order to maintain the normal operation of the equipment and extend its life, efficient heat dissipation technology is required. Thermally conductive interface materials can provide effective heat transfer between the heat source and the heat dissipation device to improve the heat dissipation efficiency. Traditional heat dissipation materials have a high interface thermal resistance during the heat transfer process, resulting in low heat transfer efficiency and affecting the overall heat dissipation effect. The thermal conductive silicone grease currently used on the market has limited thermal conductivity, and aging, oxidation, shrinkage and other problems will occur during use, causing the interface thermal conductive material to fail and increase thermal resistance, which leads to a gradual deterioration of the heat dissipation effect of the equipment and reduces the reliability and service life of the equipment. Because liquid metal has fluidity and conductivity, the latest new interface thermal conductive material uses liquid metal as an interface gap filling thermal conductive material, but it will leak when used for interface thermal conductive materials. Because liquid metal is corrosive, it causes short circuits in electronic components and a decrease in interface thermal conductivity. Problems need to be improved, and the market is also in urgent need of developing a thin-layer thermal conductive gasket with ultra-low interface thermal resistance. Summary of the invention
[0003] Features and advantages of the invention are set forth in part in the following description, or may be obvious from the description, or may be learned through practice of the invention.
[0004] In order to overcome the problems of the prior art, the present invention provides an ultra-low interface thermal resistance thin-layer thermal conductive gasket, comprising a copper foil, a meltable composite material layer coated on the upper and lower surfaces of the copper foil, and a polyfluorine isolation film arranged on the outside of the meltable composite material layer; the meltable composite material layer is prepared by mixing phase change paraffin, a mixture of butyl rubber and epoxy resin, and graphene powder.
[0005] Preferably, the mass fractions of the components of the meltable composite material layer are as follows: phase change wax is 25-26%; the mixture of butyl rubber and epoxy resin is 58-60%; and the graphene powder is 13-16%.
[0006] Preferably, the mass ratio of butyl rubber to epoxy resin in the mixture of butyl rubber and epoxy resin is 3:7.
[0007] Preferably, the copper foil is coated with an auxiliary agent layer before being coated with the meltable composite material layer.
[0008] The present invention also provides a method for preparing an ultra-low interface thermal resistance thin-layer thermal conductive gasket, which is used to prepare the ultra-low interface thermal resistance thin-layer thermal conductive gasket, and specifically comprises the following steps:
[0009] Preparation of meltable composite materials: placing phase-change paraffin wax in a water bath and heating it to 70°C to melt it for later use, weighing a preset amount of butyl rubber and epoxy resin and placing them in a stirring cup, placing them on a heating platform, pre-stirring them with a glass rod, mixing the melted phase-change paraffin wax into the mixture of butyl rubber and epoxy resin and stirring them evenly to form a butyl-paraffin mixture; weighing a preset amount of graphene powder and placing it in the butyl-paraffin mixture, placing the entire mixture in a vacuum degassing mixer for vacuum degassing and stirring for 3 minutes to obtain a meltable composite material, taking it out and placing it in a vacuum bag to seal and store it for later use;
[0010] Pretreatment: Apply the additive to the upper and lower surfaces of the copper foil and dry it;
[0011] Compounding: taking a preset amount of meltable composite material, coating it on the upper and lower surfaces of the pretreated copper foil at 70°C;
[0012] Packaging: The polyfluorine isolation film is attached to the upper and lower surfaces of the composite gasket, and then the gasket is vacuum packaged to prevent oxidation.
[0013] Beneficial effects of the present invention: The gasket in the present invention has the advantages of ultra-thinness, high thermal conductivity, and low thermal resistance. As the operating temperature of the chip increases, the meltable composite material layer on both sides of the copper foil of the gasket will be in a molten state. Although the molten state has fluidity, it is different from the fluidity of liquid metal in that the material of the present invention has high viscosity. Even in a molten state, it will not flow at will, but will tightly adhere to the surface of the copper foil. The material of the present invention has strong stability and will not corrode the surface of the chip, thereby ensuring the normal operation and stability of the electronic equipment. At the same time, when the chip is running, heat is generated and the temperature rises. When the meltable composite material layer melts, the heat is also quickly conducted to the wrapped copper foil. Since the high-viscosity and low-melting-point meltable composite material layer has good interface filling performance and good thermal conductivity, the interface thermal resistance between the existing liquid metal thermal conductive sheet and the chip is fully eliminated, making the heat transfer rate between the chip and the radiator faster. In addition, without reducing the excellent thermal conductivity of graphene and copper foil, the high-viscosity meltable composite material coated on the surface of the present application fully fills the gap between the heat sink and the chip interface, reduces the air thermal resistance of the heat transfer interface, and fills the interface gap without leakage due to its fluidity. At the same time, the composite material layer in the present application will not corrode the chip surface, reducing the anti-corrosion treatment of the chip surface, reducing costs, and improving the stability and service life of the equipment. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] The present invention will be described in detail below with reference to the accompanying drawings and in combination with examples, and the advantages and implementation methods of the present invention will become more obvious. The contents shown in the accompanying drawings are only used to explain the present invention and do not constitute any limitation to the present invention in any sense. In the accompanying drawings:
[0015] Figure 1 A schematic diagram of a thin-layer thermal conductive pad with ultra-low interface thermal resistance in a specific embodiment of the present invention;
[0016] In the figure, the corresponding relationship between the component names and the figure numbers is as follows:
[0017] Copper foil-1, meltable composite material layer-2, polyfluorine isolation film-3. DETAILED DESCRIPTION
[0018] The following embodiments of the present invention are described in further detail in conjunction with the accompanying drawings and examples. The following examples are used to illustrate the present invention, but are not intended to limit the scope of the present invention.
[0019] In the description of the present invention, unless otherwise specified, the directions or positional relationships indicated by the terms "upper", "lower", "inside", "outside", etc. are based on the directions or positional relationships shown in the accompanying drawings, and are merely simplified descriptions for the convenience of describing the present invention. They do not indicate or imply that the devices or elements referred to must have a specific direction, be constructed and operated in a specific direction, and therefore should not be understood as limitations on the present invention.
[0020] Example 1
[0021] like Figure 1 As shown, the present invention provides an ultra-low interfacial thermal resistance thin-layer thermal conductive pad, comprising a copper foil 1, a meltable composite material layer 2 coated on the upper and lower surfaces of the copper foil 1, and a polyfluorine isolation film 3 arranged outside the meltable composite material layer 2; the meltable composite material layer 2 is prepared by mixing phase-change paraffin wax, a mixture of butyl rubber and epoxy resin, and graphene powder. The melting point of the phase-change paraffin wax layer is 37°C.
[0022] The polyfluorinated isolation film 3 comprises a PET film and a release slurry coated on the PET film, wherein the release slurry is composed of the following components in preset mass fractions: 55-65% boron nitride nanosheets; 15-20% acrylic acid-PU resin; 10-15% polyfluorinated compound; 5-10% cyclohexanone and ethyl acetate mixed solvent; 0.5-2% organic silicon polymer; 0.5-2% silane coupling agent; 0.1% antioxidant; 0.1% leveling agent; and 0.01% defoaming agent; wherein the polyfluorinated compound is a mixture of 7H-dodecafluoroheptanecarboxylic acid and perfluoroether in a mass ratio of 1:10.
[0023] Furthermore, the mass fractions of the components of the meltable composite material layer 2 are as follows: phase change wax is 25%; the mixture of butyl rubber and epoxy resin is 60%; and the graphene powder is 15%.
[0024] Furthermore, the mass ratio of butyl rubber to epoxy resin in the mixture of butyl rubber and epoxy resin is 3:7.
[0025] Furthermore, the copper foil 1 is coated with an auxiliary agent layer before being coated with the meltable composite material layer 2. The auxiliary agent layer comprises at least one of modified organic siloxane, stearic acid, aluminate, silane coupling agent, organic bentonite, pentaerythritol ester, acrylic leveling agent, and silicon dioxide.
[0026] The present invention also provides a method for preparing a thin-layer thermal conductive pad with ultra-low interface thermal resistance, which specifically comprises the following steps:
[0027] Preparation of meltable composite materials: placing phase-change paraffin wax in a water bath and heating it to 70°C to melt it for later use, weighing a preset amount of butyl rubber and epoxy resin and placing them in a stirring cup, placing them on a heating platform, pre-stirring them with a glass rod, mixing the melted phase-change paraffin wax into the mixture of butyl rubber and epoxy resin and stirring them evenly to form a butyl-paraffin mixture; weighing a preset amount of graphene powder and placing it in the butyl-paraffin mixture, placing the entire mixture in a vacuum degassing mixer for vacuum degassing and stirring for 3 minutes to obtain a meltable composite material, taking it out and placing it in a vacuum bag to seal and store it for later use;
[0028] Pretreatment: coating the additive on the upper and lower surfaces of the copper foil 1 and drying it;
[0029] Compounding: taking a preset amount of meltable composite material, coating it on the upper and lower surfaces of the pretreated copper foil 1 at 70° C.;
[0030] Packaging: The polyfluorine isolation film 3 is attached to the upper and lower surfaces of the composite gasket, and then the gasket is vacuum packaged to prevent oxidation.
[0031] Example 2
[0032] This embodiment also provides an ultra-low interface thermal resistance thin-layer thermal conductive pad, the preparation method and basic structure of which are the same as the technical solution of embodiment 1, except that:
[0033] The mass fractions of the components of the meltable composite material layer 2 are as follows: 26% of phase change wax; 60% of a mixture of butyl rubber and epoxy resin; and 14% of graphene powder.
[0034] Example 3
[0035] This embodiment also provides an ultra-low interface thermal resistance thin-layer thermal conductive pad, the preparation method and basic structure of which are the same as the technical solution of embodiment 1, except that:
[0036] The mass fractions of the components of the meltable composite material layer 2 are as follows: 26% of phase change wax; 59% of the mixture of butyl rubber and epoxy resin; and 15% of graphene powder.
[0037] Example 4
[0038] This embodiment also provides an ultra-low interface thermal resistance thin-layer thermal conductive pad, the preparation method and basic structure of which are the same as the technical solution of embodiment 1, except that:
[0039] The mass fractions of the components of the meltable composite material layer 2 are as follows: phase change wax is 26%, the mixture of butyl rubber and epoxy resin is 58%, and the graphene powder is 16%.
[0040] In actual use, tear off the polyfluorine isolation film 3, align the gasket and place it on top of the chip. Then gently place the cold head on the chip for alignment, then press the cold head and tighten the screws. When the chip is running, heat is generated and the temperature rises. The meltable composite material melts and quickly conducts heat to the wrapped copper foil 1. Since the high-viscosity and low-melting-point meltable composite material has good interface filling performance and good thermal conductivity, it fully eliminates the interface thermal resistance between the liquid metal thermal conductive gasket and the chip in the prior art, making the heat transfer rate between the chip and the radiator faster. Aging test shows that compared with the existing thermal conductive silicone grease, the present invention can be used stably for a long time at 100°C, and there is no need to carry out anti-corrosion treatment on the chip.
[0041] The preferred embodiments of the present invention are described above with reference to the accompanying drawings. A person skilled in the art may implement the present invention in a variety of variations without departing from the scope and essence of the present invention. For example, a feature shown or described as part of one embodiment may be used in another embodiment to obtain another embodiment. The above are only preferred feasible embodiments of the present invention, and do not limit the scope of rights of the present invention. Any equivalent changes made using the contents of the present specification and the accompanying drawings are included in the scope of rights of the present invention.
Claims
1. Ultra-low interface thermal resistance thin-layer thermal conductive pad, characterized in that: The invention comprises a copper foil, a meltable composite material layer coated on the upper and lower surfaces of the copper foil, and a polyfluorine isolation film arranged outside the meltable composite material layer; the meltable composite material layer is prepared by mixing phase-change paraffin wax, a mixture of butyl rubber and epoxy resin, and graphene powder.
2. The ultra-low interface thermal resistance thin-layer thermal conductive pad according to claim 1, characterized in that: The mass fractions of the components of the meltable composite material layer are as follows: phase change paraffin accounts for 25-26%, a mixture of butyl rubber and epoxy resin accounts for 58-60%, and graphene powder accounts for 13-16%.
3. The ultra-low interface thermal resistance thin-layer thermal conductive pad according to claim 1, characterized in that: The mass ratio of butyl rubber to epoxy resin in the mixture of butyl rubber and epoxy resin is 3:
7.
4. The ultra-low interface thermal resistance thin-layer thermal conductive pad according to claim 1, characterized in that: The copper foil is coated with an auxiliary agent layer before being coated with the meltable composite material layer.
5. A method for preparing a thin-layer thermally conductive gasket with ultra-low interface thermal resistance, characterized in that: The method for preparing the ultra-low interface thermal resistance thin-layer thermal conductive gasket according to any one of claims 1 to 3 specifically comprises the following steps: Preparation of meltable composite materials: placing phase-change paraffin wax in a water bath and heating it to 70°C to melt it for later use, weighing a preset amount of butyl rubber and epoxy resin and placing them in a stirring cup, placing them on a heating platform, pre-stirring them with a glass rod, mixing the melted phase-change paraffin wax into the mixture of butyl rubber and epoxy resin and stirring them evenly to form a butyl-paraffin mixture; weighing a preset amount of graphene powder and placing it in the butyl-paraffin mixture, placing the entire mixture in a vacuum degassing mixer for vacuum degassing and stirring for 3 minutes to obtain a meltable composite material, taking it out and placing it in a vacuum bag to seal and store it for later use; Pretreatment: Apply the additive to the upper and lower surfaces of the copper foil and dry it; Compounding: taking a preset amount of meltable composite material, coating it on the upper and lower surfaces of the pretreated copper foil at 70°C; Packaging: The polyfluorine isolation film is attached to the upper and lower surfaces of the composite gasket, and then the gasket is vacuum packaged to prevent oxidation.