EEPROM memory based on ISSG technology and preparation method thereof
By using the ISSG process in EEPROM to form the ONO layer of HTO/SiNx/SiO2, the problems of EEPROM's mid-gate dielectric reliability and ONO layer isolation failure are solved, and more stable thickness and isolation characteristics are achieved, simplifying the process flow.
Patent Information
- Application Number
- CN202411015241.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-08
AI Technical Summary
The problem of EEPROM mid-gate dielectric reliability and ONO layer isolation failure between the floating gate of the storage tube and the control gate of the control gate, especially in the case of reduced characteristic size of the CMOS device and thinner gate dielectric layer thickness, resulting in the occurrence of leakage channels.
Using the EEPROM memory based on the ISSG process, the ISSG SiO2 layer is used as the gate dielectric layer of the core device and input/output device, and the SiNx layer is reoxidized through the ISSG process to form the ONO dielectric layer of the HTO bottom layer, the SiNx middle layer and the ISSG SiO2 top layer. , simplify the process and improve the reliability of the gate medium.
It improves the gate dielectric reliability of the EEPROM memory, ensures the thickness stability and isolation characteristics of the ONO layer, reduces process complexity, avoids thickness fluctuations caused by HF cleaning, and enhances the practical application capabilities of the device.
Smart Images

Figure CN118921986A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of silicon microelectronics, in particular to an EEPROM memory based on ISSG process and a preparation method thereof. Background Art
[0002] Electrically-Erasable Programmable Read Only Memory (EEPROM) is a non-volatile memory widely used in applications that require high data storage security and reliability. The EEPROM process is formed by adding process modules based on the baseline CMOS process, such as the 0.13μm CMOS process. The small-size CMOS baseline process with a feature size below 0.25μm is usually a dual-gate process, forming devices with two operating voltages, namely core devices and input / output devices; the large-size CMOS baseline process with a feature size above 0.25μm is a single-gate process, forming devices with one operating voltage, that is, the circuit does not distinguish between core devices and input / output devices, which can be understood as only input / output devices. In addition, the reading and writing of EEPROM is performed through a high-voltage module, that is, a special high-voltage device (HV device) with thicker gate oxide and higher voltage is used.
[0003] With the reduction of the feature size of CMOS devices and the thinning of the gate dielectric layer, gate dielectric damage has become one of the main failure modes of CMOS integrated circuits in practical applications. In-Situ Steam Generation (ISSG) is a new low-pressure rapid oxidation technology. Due to the strong oxidizing effect of atomic oxygen, the resulting SiO2 layer has fewer defects and interface state density, and the film quality is also higher. In addition, ISSG can x The layer is then oxidized to a SiO2 layer, thereby achieving an upper SiO2 / lower SiN x composite structure.
[0004] The floating gate in EEPROM passes through the ONO layer (SiO2 top layer / SiN x The middle layer / SiO2 bottom layer) is isolated from the storage tube control gate. In the entire process of EEPROM, the SiO2 top layer in the ONO layer is easily affected by the subsequent HF cleaning process before the gate dielectric oxidation, resulting in thickness fluctuations. In severe cases, pinholes may appear and leakage channels may be formed. Summary of the invention
[0005] Aiming at the problems of gate dielectric reliability and ONO layer isolation failure between a storage tube floating gate and a control gate in the prior art, the present invention provides an EEPROM memory based on an ISSG process and a preparation method thereof.
[0006] The present invention is achieved through the following technical solutions:
[0007] An EEPROM memory based on ISSG process, the memory uses ISSG SiO2 layer as the gate dielectric layer of the core device and input / output device, and the top layer of the ONO dielectric layer between the floating gate and the control gate of the storage tube is made of ISSG to SiN x The ONO dielectric layer includes a HTO bottom layer (High Temperature Oxide, high temperature thermal oxide), a SiN x Middle layer and ISSG SiO2 top layer.
[0008] A method for preparing an EEPROM memory based on an ISSG process comprises the following steps:
[0009] Step 1, pre-treating the silicon substrate, and filling five shallow trench isolation (STI) oxides on the upper surface of the silicon substrate, and then respectively injecting storage tube source and drain, low voltage well, medium voltage well, high voltage well and storage tube well between adjacent STI oxides;
[0010] Step 2, growing a SiO2 layer as a gate dielectric layer of a storage tube on the upper surface of a silicon substrate; photolithographically opening a tunneling window above a drain region of the storage tube, and then wet-etching the SiO2 layer in the tunneling window; and oxidizing and growing a SiO2 layer as a tunneling oxide layer at the etching tunneling window;
[0011] Step 3, depositing a polysilicon layer on the tunnel oxide layer, photolithography covers the floating gate region of the storage tube, and etching the polysilicon layer to form a floating gate in the EEPROM unit;
[0012] Step 4: deposit a NO layer on the substrate, the NO layer including the HTO bottom layer and the SiN x In the middle layer, the storage tube area is covered by photolithography, and then the NO layer and the storage tube gate dielectric layer of the core MOS, the NO layer and the storage tube gate dielectric layer of the input / output MOS, and the NO layer and the storage tube gate dielectric layer of the high-voltage MOS are etched away, and the NO layer and the storage tube gate dielectric layer of the storage tube area are retained;
[0013] Step 5, oxidizing and growing the high-voltage gate dielectric layer of the high-voltage MOS, photolithography covers the high-voltage MOS and the storage pipe area, and then etching away the high-voltage gate dielectric layer of the core MOS and the high-voltage gate dielectric layer of the input / output MOS;
[0014] Step 6: Use ISSG process to grow thick gate dielectric layer of input / output MOS. ISSG process also grows SiN layer of NO layer in storage pipe area. x The middle layer is then oxidized to the SiO2 top layer, and the input / output MOS, high-voltage MOS and storage pipe area are covered by photolithography, and then the thick gate dielectric layer of the core MOS is etched away;
[0015] Step 7: Use ISSG process to grow the thin gate dielectric layer of the core MOS. The ISSG process also grows the SiN layer of the NO layer in the storage pipe area. x The middle layer continues to be reoxidized to the SiO2 top layer, and finally the NO layer in the storage tube area is converted into the ONO layer;
[0016] Step 8, depositing a polysilicon layer, photolithography covering the polysilicon layer for etching, and completing the preparation of the gate of the EEPROM;
[0017] Step 9: According to the known process, lightly doped source and drain implantation, sidewall deposition and etching, and source and drain implantation are completed to form a complete device structure.
[0018] Preferably, when the feature size of the EEPROM memory process is above 0.25 μm, the preparation method does not include the photolithography and etching of the thick gate dielectric layer in step 6 and the entirety of step 7, and the STI oxide in step 1 is a field oxide without a low voltage well.
[0019] Preferably, in step 2, the SiO2 layer as the gate dielectric layer of the storage tube is grown by dry oxygen oxidation with O2 or wet oxygen oxidation with a volume ratio of H2:O2 of 1:(1-1.8) as the reaction gas, the reaction temperature is 750°C-900°C, the time is 10min-120min, and the thickness is
[0020] During etching, wet etching is adopted, and the etching solution is a buffered oxide etching solution with a volume ratio of NH4F:HF of 100:1;
[0021] The SiO2 layer as the tunneling oxide layer is grown by dry oxygen oxidation with O2 or wet oxygen oxidation with a volume ratio of H2:O2 of 1:(1-1.8) at a reaction temperature of 750°C-900°C for 5min-30min and a thickness of
[0022] Preferably, in step 3, the polysilicon layer used as the floating gate is prepared by first depositing by LPCVD method, then photolithography and then etching;
[0023] During deposition, the reaction gas is SiH4, the temperature is 575℃~650℃, the pressure is 0.1Torr~5.0Torr, and the thickness is
[0024] During etching, dry etching is adopted, the main gases are HBr, Cl2 and HeO2, the etching selectivity ratio of polysilicon to SiO2 is greater than 200:1, and the etching end point stays on SiO2.
[0025] Preferably, in step 4, the HTO bottom layer and the SiN x The middle layers were deposited using the LPCVD method;
[0026] When the HTO bottom layer is deposited, the reaction gas is SiH2Cl2 and N2O with a volume ratio of 1:(5-10), the reaction temperature is 800℃-900℃, the pressure is 0.1Torr-5.0Torr, the time is 5min-30min, and the thickness is
[0027] S N x During the layer deposition, the reaction gas is SiH2Cl2 and NH3 with a volume ratio of 1: (5-10), the reaction temperature is 700℃-800℃, the pressure is 0.1Torr-5.0Torr, the time is 10min-60min, and the thickness is
[0028] During etching, dry etching is used, and the main etching gases are CF4 and CHF3, SiN x The etching selectivity ratio for SiO2 is 10:1, and the etching endpoint stays on SiO2.
[0029] Preferably, in step 5, the high-voltage gate dielectric layer of the high-voltage MOS is grown by dry oxidation with O2 or wet oxidation with a volume ratio of H2:O2 of 1:(1-1.8) at a reaction temperature of 750°C-950°C, a time of 10min-180min, and a thickness of
[0030] During etching, wet etching is adopted, and the etching solution adopts a buffered oxide etching solution with a volume ratio of NH4F:HF of 100:1.
[0031] Preferably, in step 6, the thick gate dielectric layer is grown SiO2 by ISSG oxidation with a volume ratio of H2:O2 of 1:(3-30) as the reaction gas, the reaction temperature is 900°C-1200°C, the time is 10s-240s, and the thickness is
[0032] While the ISSG process is growing SiO2, the NO layer in the storage pipe area SiN x The middle layer is reoxidized to SiO2 top layer;
[0033] During etching, wet etching is adopted, and the etching solution adopts a buffered oxide etching solution with a volume ratio of NH4F:HF of 100:1.
[0034] Preferably, in step 7, the thin gate dielectric layer is grown SiO2 by ISSG oxidation with a reaction gas H2:O2 volume ratio of 1:(3-30), a reaction temperature of 900°C-1200°C, a time of 5s-120s, and a thickness of
[0035] While growing SiO2 in the ISSG process, the NO layer in the storage pipe area SiN x The middle layer is reoxidized to The SiO2 top layer.
[0036] Preferably, in step 8, the polysilicon layer is deposited by LPCVD, the reaction gas is SiH4, the temperature is 575°C to 650°C, the pressure is 0.1 Torr to 5.0 Torr, and the thickness is
[0037] The polycrystalline gate is etched by dry etching, the main etching gases are HBr, Cl2 and HeO2, the etching selectivity of polysilicon to SiO2 is greater than 200:1, and the etching end point stays on SiO2.
[0038] Compared with the prior art, the present invention has the following beneficial effects:
[0039] The high-reliability EEPROM memory of the present invention uses SiO2 grown by ISSG to replace SiO2 grown by dry or wet oxidation as thick gate dielectric layer and thin gate dielectric layer, which has better gate dielectric reliability. x The reoxidation of the NO layer of the floating gate of the storage tube is converted into an ONO layer, which reduces the deposition of the top SiO2 layer in the ONO layer and simplifies the process. x The layer is not sensitive to HF cleaning process, SiN x The SiO2 achieved by reoxidation has a more stable thickness and better isolation properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 The present invention is a schematic diagram of the structure of an EEPROM memory based on ISSG technology.
[0041] Figure 2 The present invention is a flow chart of a method for preparing an EEPROM memory based on the ISSG process.
[0042] Figure 3 Schematic diagram of a silicon substrate after well implantation according to the present invention.
[0043] Figure 4 It is a schematic diagram of the deposition of the gate dielectric layer of the storage tube of the present invention.
[0044] Figure 5 This is a schematic diagram of the storage tube tunneling window after etching and stripping.
[0045] Figure 6 It is a schematic diagram of the tunneling oxide deposition of the present invention.
[0046] Figure 7 It is a schematic diagram of the floating gate deposition of the present invention.
[0047] Figure 8 This is a schematic diagram of the floating gate after etching and de-resisting of the present invention.
[0048] Fig. 9 The NO layer (SiN x Schematic diagram of the growth of middle layer / HTO bottom layer).
[0049] Fig.10 This is a schematic diagram of the NO layer after etching and stripping of the resist according to the present invention.
[0050] Fig.11 It is a schematic diagram of the growth of the high voltage gate dielectric layer (HV oxide) of the present invention.
[0051] Fig.12 This is a schematic diagram of the high-voltage gate dielectric layer after etching and stripping of the resist according to the present invention.
[0052] Fig.13 The thick gate dielectric layer (Thick oxide) growth diagram of the present invention adopts the ISSG process to grow the thick gate dielectric layer of the input / output MOS. The ISSG process simultaneously grows the SiN layer of the NO layer in the storage pipe area. x The middle layer is then oxidized to form a SiO2 top layer.
[0053] Fig.14 This is a schematic diagram of the thick gate dielectric layer after etching and stripping of the resist according to the present invention.
[0054] Fig.15 The thin gate dielectric layer (Thin oxide) growth diagram of the present invention adopts ISSG process to grow the thin gate dielectric layer of the core MOS. The ISSG process simultaneously grows the SiN oxide of the NO layer in the storage pipe area. x The middle layer continues to be reoxidized to the SiO2 top layer, and finally the NO layer in the storage tube area is converted into the ONO layer.
[0055] Fig.16 This is a schematic diagram of the deposition of a polysilicon layer according to the present invention.
[0056] Fig.17This is a schematic diagram of the polycrystalline gate after etching and stripping of the resist according to the present invention.
[0057] In the figure, 1, silicon substrate; 2, STI oxide; 3, storage tube source and drain; 4, low voltage well; 5, medium voltage well; 6, high voltage well; 7, storage tube well; 8, storage tube gate dielectric layer; 9, tunneling oxide layer; 10, floating gate; 11, HTO bottom layer; 12, SiN x Middle layer; 13, high-voltage gate dielectric layer; 14, thick gate dielectric layer; 15, ISSG SiO2 top layer; 16, thin gate dielectric layer; 17, polycrystalline gate; 18, core lightly doped source and drain; 19, input / output lightly doped source and drain; 20a, MOS device side wall; 20b, storage tube side wall; 21, source and drain; 41, core MOS; 42, input / output MOS; 43, high-voltage MOS; 44, storage tube. DETAILED DESCRIPTION
[0058] The present invention is further described in detail below in conjunction with specific embodiments, which are intended to explain the present invention rather than to limit it.
[0059] The present invention discloses an EEPROM memory based on ISSG process, referring to Figure 1 The memory uses ISSGSiO2 layer as the gate dielectric layer of the core device and input / output device, and the top layer of the ONO dielectric layer between the floating gate and the control gate of the storage tube is realized by ISSG process. The ONO dielectric layer includes HTO bottom layer, SiN x Middle layer and ISSG SiO2 top layer.
[0060] The present invention proposes a method for preparing an EEPROM memory based on an ISSG process, referring to Figure 2 This method realizes thick gate oxide dielectric layer and thin gate oxide dielectric layer of EEPROM based on ISSG process, and at the same time, the ISSG is used to x The re-oxidation of the middle layer converts the NO layer on the floating gate into an ONO layer. ISSG SiO2 has good gate dielectric reliability as a gate dielectric layer. The ONO layer achieved by ISSG re-oxidation has a more stable thickness and better isolation characteristics. The details are as follows:
[0061] Step 1, pre-treat the silicon substrate and fill five STI oxides on the upper surface of the silicon substrate, and then respectively inject storage tube source and drain, low voltage well, medium voltage well, high voltage well and storage tube well between adjacent STI oxides.
[0062] like Figure 3As shown, a silicon substrate 1 is provided, and according to a known process, STI etching, STI oxide 2 filling, STI oxide 2 chemical mechanical planarization (CMP), storage tube source and drain 3 injection, low pressure well 4 injection, medium pressure well 5 injection, high pressure well 6 injection and storage tube well 7 injection are sequentially completed.
[0063] Step 2, growing a SiO2 layer as a gate dielectric layer of the storage tube on the upper surface of the silicon substrate; opening a tunneling window above the drain region of the storage tube, and then wet etching the SiO2 layer in the tunneling window; and oxidizing and growing a SiO2 layer as a tunneling oxide layer at the tunneling window after etching.
[0064] like Figure 4 As shown, a SiO2 layer is grown as a gate dielectric layer 8 of the storage tube;
[0065] The storage tube gate dielectric layer 8 can be grown by dry oxidation with O2 or wet oxidation with a volume ratio of H2:O2 of 1:(1-1.8) at a reaction temperature of 750°C-900°C, a time of 10min-120min, and a thickness of
[0066] like Figure 5 As shown, a tunneling window is opened above the drain region of the storage tube;
[0067] Perform tunneling window lithography (including coating, exposure, and development), cover other areas on the silicon wafer with photoresist, open a tunneling window above the drain area of the storage tube, etch away the oxide layer in the tunneling window, and use wet etching to reduce damage to the Si substrate. The etching solution uses a buffered oxide etchant (BOE) with a volume ratio of NH4F:HF of 100:1. After etching, remove the glue by wet SPM (H2SO4:H2O2 volume ratio of 5:1).
[0068] like Figure 6 As shown, a SiO2 layer as a tunneling oxide layer (Tunneling Oxide) 9 is grown at the tunneling window after etching;
[0069] The tunnel oxide layer is grown by dry oxidation with O2 or wet oxidation with a volume ratio of H2:O2 of 1:(1-1.8) at a reaction temperature of 750°C-900°C for 5 min-30 min and a thickness of
[0070] Step 3, depositing a polysilicon layer on the tunnel oxide layer, photolithography covers the floating gate region of the storage tube, and etching the polysilicon layer to form a floating gate in the EEPROM unit.
[0071] like Figure 7 As shown, a polysilicon layer is deposited as an etching base layer for a floating gate 10;
[0072] The polysilicon layer is deposited by LPCVD (Low Pressure Chemical Vapor Deposition) method, the reaction gas is SiH4, the temperature is 575℃~650℃, the pressure is 0.1Torr~5.0Torr, and the thickness is
[0073] like Figure 8 As shown, the polysilicon layer is etched to form a floating gate 10 of the EEPROM cell;
[0074] The steps of photolithography (including coating, exposure, and development) of the floating gate 10 are as follows: the polysilicon layer of the floating gate region of the storage tube is covered with photoresist, and the polysilicon layer of other regions on the silicon wafer is etched away. Dry etching is used to achieve a higher selectivity. The main etching gases are HBr, Cl2, and HeO2. The etching selectivity of polysilicon to SiO2 is greater than 200:1, and the etching end point stays on SiO2. After etching, degumming is performed by dry and wet processes. The dry degumming process is O2 plasma degumming, and the wet degumming process is SPM degumming.
[0075] Step 4: deposit a NO layer on the substrate, the NO layer including the HTO bottom layer and the SiN x In the middle layer, the storage tube area is covered by photolithography, and then the NO layer and storage tube gate dielectric layer of the core MOS, the NO layer and storage tube gate dielectric layer of the input / output MOS, and the NO layer and storage tube gate dielectric layer of the high-voltage MOS are etched away, and the NO layer and storage tube gate dielectric layer of the storage tube area are retained.
[0076] like Fig. 9 As shown, the HTO bottom layer 11 and SiN in the ONO layer are deposited x Middle level 12;
[0077] The HTO bottom layer 11 in the ONO layer is deposited by LPCVD method, the volume ratio of the reaction gas SiH2Cl2 to N2O is 1:(5-10), the reaction temperature is 800℃-900℃, the pressure is 0.1Torr-5.0Torr, the time is 5min-30min, and the thickness is
[0078] SiN in ONO layer deposited by LPCVD xThe middle layer 12 has a volume ratio of SiH2Cl2 to NH3 of 1:(5-10), a reaction temperature of 700°C-800°C, a pressure of 0.1 Torr-5.0 Torr, a time of 10 min-60 min, and a thickness of
[0079] like Fig.10 As shown, the NO layer and the storage tube gate dielectric layer 8 of the core MOS 41, the NO layer and the storage tube gate dielectric layer 8 of the input / output MOS 42, and the NO layer and the storage tube gate dielectric layer 8 of the high-voltage MOS 43 are etched away;
[0080] Perform NO layer photolithography (including coating, exposure, and development), cover the storage tube 44 area with photoresist, etch away the NO layer and storage tube gate dielectric layer 8 of the core MOS 41, the NO layer and storage tube gate dielectric layer 8 of the input / output MOS 42, and the NO layer and storage tube gate dielectric layer 8 of the high-voltage MOS 43, and use dry etching to achieve a higher selectivity. The main etching gas is CF4 and CHF3, and SiN x The etching selectivity ratio for SiO2 is 10:1, and the etching end point stays on SiO2. After etching, degumming is carried out through dry and wet processes. The dry degumming process is O2 plasma degumming, and the wet degumming process is SPM degumming.
[0081] Step 5, oxidize and grow the high-voltage gate dielectric layer of the high-voltage MOS, cover the high-voltage MOS and the storage pipe area by photolithography, and then etch away the high-voltage gate dielectric layer of the core MOS and the high-voltage gate dielectric layer of the input / output MOS.
[0082] like Fig.11 As shown, SiO2 is grown by dry oxygen oxidation or wet oxygen oxidation as the high voltage gate dielectric layer (HV oxide) 13 of the high voltage MOS 43. The storage tube 44 will not grow the high voltage gate dielectric layer 13 due to the NO layer blocking;
[0083] The high voltage gate dielectric layer 13 is grown by dry oxidation with O2 or wet oxidation with a volume ratio of H2:O2 of 1:(1-1.8) at a reaction temperature of 750°C-950°C for 10min-180min and a thickness of The HF cleaning process before the growth of the high-voltage gate dielectric layer 13 has no effect on the thickness of the NO layer.
[0084] like Fig.12 As shown, the high-voltage gate dielectric layer of the core MOS 41 and the high-voltage gate dielectric layer 13 of the input / output MOS 42 are etched away;
[0085] The high-voltage gate dielectric layer 13 is photolithographically processed (including coating, exposure, and development), and the high-voltage MOS 43 and the storage tube 44 area are covered with photoresist. The high-voltage gate dielectric layer of the core MOS 41 and the high-voltage gate dielectric layer 13 of the input / output MOS 42 are etched away. Wet etching is used to reduce damage to the Si substrate. The etching solution uses a buffered oxide etching solution with a volume ratio of NH4F:HF of 100:1. After etching, the resist is removed by a wet SPM process.
[0086] Step 6: Using ISSG process to grow thick gate dielectric layer of input / output MOS; ISSG process also grows SiN layer of NO layer in storage pipe area x The middle layer is then oxidized to a SiO2 top layer, and the input / output MOS, high-voltage MOS and storage pipe areas are covered by photolithography, and then the thick gate dielectric layer of the core MOS is etched away.
[0087] like Fig.13 As shown, the ISSG process is used to grow SiO2 as the thick gate dielectric layer (thickoxide) 14 of the input / output MOS 42. The ISSG process also grows SiN x A portion of the middle layer 12 close to the upper surface is oxidized to SiO2 to form a SiO2 top layer 15, and the thickness of the high-voltage gate dielectric layer 13 is slightly increased;
[0088] The thick gate dielectric layer 14 is grown by an ISSG oxidation method with a volume ratio of H2:O2 of 1:(3-30) at a reaction temperature of 900°C-1200°C for 10s-240s, and a thickness of
[0089] While the ISSG process is growing SiO2, the NO layer in the storage pipe area SiN x The middle layer is reoxidized to The SiO2 top layer.
[0090] The HF cleaning process before the growth of the thick gate dielectric layer 14 has no effect on the thickness of the NO layer.
[0091] like Fig.14 As shown, the thick gate dielectric layer 14 of the core MOS 41 is etched away;
[0092] The thick gate dielectric layer 14 is photolithographically processed (including coating, exposure, and development), and the input / output MOS 42, high-voltage MOS 43, and storage tube 44 regions are covered with photoresist. The thick gate dielectric layer 14 of the core MOS 41 is etched away. Wet etching is used to reduce damage to the Si substrate. The etching solution is a buffered oxide etching solution with a volume ratio of NH4F:HF of 100:1. After etching, the resist is removed by a wet SPM process.
[0093] Step 7: Use ISSG process to grow the thin gate dielectric layer of the core MOS. The ISSG process also grows the SiN layer of the NO layer in the storage pipe area. x The middle layer continues to be reoxidized to the SiO2 top layer, and finally the NO layer in the storage tube area is converted into the ONO layer.
[0094] like Fig.15 As shown, the ISSG process is used to grow SiO2 as the thin gate dielectric layer (Thinoxide) 16 of the core MOS 41. The ISSG process also grows SiN x A portion of the middle layer 12 near the upper surface continues to be reoxidized to SiO2, eventually forming a SiO2 top layer 15, and the NO layer in the storage tube area is also converted into an ONO layer;
[0095] The thin gate dielectric layer is grown by an ISSG oxidation method with a reaction gas H2:O2 volume ratio of 1:(3-30), a reaction temperature of 900°C-1200°C, a time of 5s-120s, and a thickness of
[0096] While the ISSG process is growing SiO2, the NO layer in the storage pipe area SiN x The middle layer is reoxidized to The SiO2 top layer.
[0097] Step 8, depositing a polysilicon layer on the substrate, and etching the covering polysilicon layer to complete the preparation of the gate of the EEPROM.
[0098] like Fig.16 As shown, a polysilicon layer is deposited as an etching substrate for the core MOS 41, the input / output MOS 42, the high-voltage MOS 43 and the polycrystalline gate 17 of the storage tube 44;
[0099] The polysilicon layer is deposited by LPCVD, the reaction gas is SiH4, the temperature is 575℃~650℃, the pressure is 0.1Torr~5.0Torr, and the thickness is
[0100] like Fig.17 As shown, the polysilicon layer is etched to form a polycrystalline gate 17;
[0101] Perform polycrystalline gate 17 photolithography (including coating, exposure, and development), cover the polycrystalline gate with photoresist for etching, and use dry etching to achieve a higher selectivity. The main etching gases are HBr, Cl2, and HeO2. The etching selectivity of polysilicon to SiO2 is greater than 200:1. The etching end point stays on SiO2. After etching, debonding is performed through dry and wet processes. The dry debonding process is O2 plasma debonding, and the wet debonding process is SPM debonding.
[0102] Step 9: According to the known process, lightly doped source and drain implantation, sidewall deposition and etching, and source and drain implantation are completed to form a complete device structure.
[0103] According to the known process, the core lightly doped source and drain 18 is implanted, the input / output lightly doped source and drain 19 is implanted, the sidewalls (MOS device sidewalls 20a, storage tube sidewalls 20b) are deposited and etched, and the source and drain are implanted 21 to form a complete structure. Figure 1 For EEPROM processes with feature sizes above 0.25 μm, there is no core MOS 41, so it is not necessary to perform the lithography and etching of the thick gate dielectric layer in step 6 ( Fig.14 ) and all of step 7 ( Fig.15 ), and the STI oxide in step 1 is a field oxide and does not contain a low voltage well 4.
[0104] Example 1
[0105] The preparation process of a 0.13μm EEPROM based on ISSG gate dielectric layer is as follows:
[0106] 1) Oxidation growth on original silicon wafer SiO2, LPCVD deposition growth Silicon nitride;
[0107] Active area photolithography, dry etching depth is Shallow trench isolation, stripping after etching;
[0108] STI oxide filling;
[0109] STI oxide chemical mechanical polishing;
[0110] Silicon nitride full stripping;
[0111] Photolithography of the storage tube source and drain, injection of the storage tube source and drain, and stripping after injection;
[0112] Low-voltage P-well lithography, well implantation of core NMOS, including well implantation, anti-punch-through implantation and threshold implantation, and post-implantation stripping;
[0113] Low-voltage N-well lithography, well implantation of core PMOS, including well implantation, anti-punch-through implantation and threshold implantation, and post-implantation debonding;
[0114] Medium voltage P-well lithography, well implantation of input / output NMOS, including well implantation, anti-punch-through implantation and threshold implantation, and post-implantation stripping;
[0115] Medium voltage N-well lithography, well implantation of input / output PMOS, including well implantation, anti-punch-through implantation and threshold implantation, and post-implantation stripping;
[0116] High-voltage P-well lithography, high-voltage NMOS well implantation, including well implantation, anti-punch-through implantation and threshold implantation, and post-implantation debonding;
[0117] High-voltage N-well lithography, high-voltage PMOS well implantation, including well implantation, anti-punch-through implantation and threshold implantation, and post-implantation debonding;
[0118] Photolithography of the storage tube well, injection of the storage tube well, and stripping after injection;
[0119] 2) Dry oxygen oxidation or wet oxygen oxidation growth SiO2 layer, serving as a gate dielectric layer of the storage tube;
[0120] Tunneling window lithography: Use photoresist to cover other areas on the silicon wafer, open a tunneling window above the drain area of the storage tube, wet-etch the oxide layer in the tunneling window, and remove the resist after etching;
[0121] Dry oxygen oxidation or wet oxygen oxidation growth SiO2 layer, serving as a tunneling oxide layer;
[0122] 3) LPCVD deposition A polysilicon layer, serving as a floating gate;
[0123] Floating gate lithography: Use photoresist to cover the polysilicon layer in the floating gate area of the storage tube, dry-etch the polysilicon layer in other areas of the silicon wafer, and remove the photoresist after etching;
[0124] 4) LPCVD deposition HTO layer, as the bottom layer in the ONO layer;
[0125] LPCVD deposition S N x Layer, as the middle layer in the ONO layer;
[0126] Photolithography of the NO layer, covering the storage tube area with photoresist, dry etching the NO layer and storage tube gate dielectric layer of the core MOS, the NO layer and storage tube gate dielectric layer of the input / output MOS, and the NO layer and storage tube gate dielectric layer of the high-voltage MOS, and then removing the resist after etching;
[0127] 5) Dry oxygen oxidation or wet oxygen oxidation growth SiO2, as the high-voltage gate dielectric layer of high-voltage MOS;
[0128] Photolithography of the high-voltage gate dielectric layer, covering the high-voltage MOS and storage tube area with photoresist, wet etching the high-voltage gate dielectric layer of the core MOS and the high-voltage gate dielectric layer of the input / output MOS, and wet stripping the resist after etching;
[0129] 6) The ISSG process grows SiO2 as the thick gate dielectric layer of the input / output MOS, with a thickness of The ISSG process also converts the SiN layer of the NO layer in the storage pipe area into x Part of it is then oxidized to SiO2, i.e., the thickness is SiN x Reoxidation to of SiO2;
[0130] Thick gate dielectric layer photolithography, cover the input / output MOS, high voltage MOS and storage pipe area with photoresist, wet etch the thick gate dielectric layer of the core MOS, and wet strip the resist after etching;
[0131] 7) ISSG process grows SiO2 as the thin gate dielectric layer of the core MOS, with a thickness of The ISSG process also converts the SiN layer of the NO layer in the storage pipe area into x Continue to oxidize to SiO2, that is, the thickness is SiN x Reoxidation to SiO2, which is finally formed in the storage tube area ISSG SiO2 top layer / S N x Middle level / The three-layer structure of the HTO bottom layer;
[0132] 8) LPCVD deposition A polysilicon layer is provided and doped by implantation;
[0133] Polycrystalline grating lithography and etching, and stripping after etching;
[0134] 9) Core N-type lightly doped source and drain photolithography and implantation, and debonding after implantation;
[0135] Core P-type lightly doped source and drain photolithography and implantation, and stripping after implantation;
[0136] Input / output N-type lightly doped source and drain photolithography and implantation, and stripping after implantation;
[0137] Input / output P-type lightly doped source and drain photolithography and implantation, and stripping after implantation;
[0138] CVD deposition Silicon nitride sidewall, silicon nitride sidewall etching;
[0139] N-type source and drain photolithography and implantation, and debonding after implantation;
[0140] P-type source and drain photolithography and implantation, and debonding after implantation;
[0141] Co silicide deposition, Co silicide rapid annealing and cleaning, forming silicide on the exposed active area and the upper surface of the polycrystalline gate;
[0142] Formation of ILD (Inter Layer Dielectrics), including CVD deposition USG layer, CVD deposition Silicon oxide as ILD layer, CMP removed Silicon oxide layer, CVD deposition PETEOS layer, so the equivalent ILD thickness on the active area is
[0143] Ohmic hole lithography and etching, and stripping after etching;
[0144] Hole filling, including sputtering Ti and TiN, CVD deposition Tungsten metal layer, chemical mechanical polishing Metal tungsten layer;
[0145] Formation of metal 1, including sputtering Ti and TiN, sputtering AlCu;
[0146] Metal 1 photolithography and etching, and stripping after etching;
[0147] Formation of IMD1 (Inter Metal Dielectrics 1), including CVD deposition Silicon oxide, CMP wear off Silicon oxide, CVD deposition of silicon oxide;
[0148] Photolithography and etching of through hole 1, and stripping of resist after etching;
[0149] Filling of via 1, including sputtering Ti and TiN, CVD deposition Tungsten metal layer, chemical mechanical polishing Metal tungsten layer;
[0150] Formation of Metal 2, including sputtering Ti and TiN, sputtering AlCu;
[0151] Metal 2 photolithography and etching, and stripping after etching;
[0152] IMD2~IMD5 repeat the material, thickness and process of IMD1, and metal 3~metal 6 repeat the material, thickness and process of metal 2;
[0153] HDP deposition SiO2, CVD deposition SiON as passivation layer;
[0154] The passivation layer is photolithographically processed and etched, and then the resist is removed after etching, and the wafer is tested.
[0155] Example 2
[0156] The process of a 0.5μm EEPROM based on ISSG gate dielectric layer is as follows:
[0157] 1) Oxidation growth on original silicon wafer Oxide layer, CVD deposition growth Silicon nitride;
[0158] Active area lithography, dry etching field area Silicon nitride, resist removal after etching;
[0159] Oxidation to form field oxide isolation;
[0160] Silicon nitride full stripping;
[0161] Photolithography of the storage tube source and drain, injection of the storage tube source and drain, and stripping after injection;
[0162] Medium voltage P-well lithography, well implantation of input / output NMOS, including well implantation, anti-punch-through implantation and threshold implantation, and post-implantation stripping;
[0163] Medium voltage N-well lithography, well implantation of input / output PMOS, including well implantation, anti-punch-through implantation and threshold implantation, and post-implantation stripping;
[0164] High-voltage P-well lithography, high-voltage NMOS well implantation, including well implantation, anti-punch-through implantation and threshold implantation, and post-implantation debonding;
[0165] High-voltage N-well lithography, high-voltage PMOS well implantation, including well implantation, anti-punch-through implantation and threshold implantation, and post-implantation debonding;
[0166] Photolithography of the storage tube well, injection of the storage tube well, and stripping after injection;
[0167] 2) Dry oxygen oxidation or wet oxygen oxidation growth SiO2 layer, serving as a gate dielectric layer of the storage tube;
[0168] Tunneling window lithography: Use photoresist to cover other areas on the silicon wafer, open a tunneling window above the drain area of the storage tube, wet-etch the SiO2 layer in the tunneling window, and remove the resist after etching;
[0169] Dry oxygen oxidation or wet oxygen oxidation growth SiO2 layer, serving as a tunneling oxide layer;
[0170] 3) LPCVD deposition A polysilicon layer, serving as a floating gate;
[0171] Floating gate lithography: Use photoresist to cover the polysilicon layer in the floating gate area of the storage tube, dry-etch the polysilicon layer in other areas of the silicon wafer, and remove the photoresist after etching;
[0172] 4) LPCVD deposition HTO layer, as the bottom layer in the ONO layer;
[0173] LPCVD deposition S N x Layer, as the middle layer in the ONO layer;
[0174] Photolithography of the NO layer, covering the storage tube area with photoresist, dry etching the NO layer and storage tube gate dielectric layer of the input / output MOS, the NO layer and storage tube gate dielectric layer of the high-voltage MOS, and removing the resist after etching;
[0175] 5) Dry oxygen oxidation or wet oxygen oxidation growth SiO2, as the high-voltage gate dielectric layer of high-voltage MOS;
[0176] Photolithography of the high-voltage gate dielectric layer, covering the high-voltage MOS and storage tube area with photoresist, wet etching the high-voltage gate dielectric layer of the input / output MOS, and wet stripping the resist after etching;
[0177] 6) The ISSG process grows SiO2 as the thick gate dielectric layer of the input / output MOS, with a thickness of The ISSG process also converts the SiN layer of the NO layer in the storage pipe area into x The layer is partially oxidized to SiO2, that is, the thickness is SiN x Reoxidation to SiO2, which is finally formed in the storage tube area ISSG SiO2 top layer / S N x Middle level / The three-layer structure of the HTO bottom layer;
[0178] 7) None (Note: the method for preparing an EEPROM memory with a feature size of more than 0.25 μm does not contain the part of step 6 of photolithography and etching of the thick gate dielectric layer, and the whole of step 7);
[0179] 8) LPCVD deposition Polysilicon layer, N-type polycrystalline diffusion doping;
[0180] LPCVD deposition Wlq x layer;
[0181] Polycide polycrystalline lithography and etching;
[0182] 9) Input / output N-type lightly doped source and drain photolithography and implantation, and debonding after implantation;
[0183] Input / output P-type lightly doped source and drain photolithography and implantation, and stripping after implantation;
[0184] LPCVD deposition Silicon oxide sidewall, silicon oxide sidewall etching;
[0185] N-type source and drain photolithography and implantation, and debonding after implantation;
[0186] P-type source and drain photolithography and implantation, and debonding after implantation;
[0187] ILD formation, including CVD deposition USG layer, CVD deposition BPSG layer, dielectric reflow, chemical mechanical polishing BPSG layer, CVD deposition USG layer, so the equivalent ILD thickness on the active area is
[0188] Ohmic hole lithography and etching, and stripping after etching;
[0189] Hole filling, including sputtering Ti and TiN, CVD deposition Tungsten metal layer, chemical mechanical polishing Metal tungsten layer;
[0190] Formation of metal 1, including sputtering Ti and TiN, sputtering AlCu metal layer;
[0191] Metal 1 photolithography and etching, and stripping after etching;
[0192] CVD deposition SiO2, CVD deposition Si3N4 as passivation layer;
[0193] The passivation layer is photolithographically processed and etched, and then the resist is removed after etching, and the wafer is tested.
[0194] The EEPROM memory preparation method based on the ISSG process of the present invention has the following advantages: 1) the SiO2 grown by ISSG replaces the SiO2 grown by dry or wet oxidation as the thick gate dielectric layer and the thin gate dielectric layer, which has better gate dielectric reliability; 2) the SiN in the NO layer xThe layer is not sensitive to the HF cleaning process, which avoids the thickness fluctuation of the SiO2 top layer in the ONO layer caused by multiple HF cleaning in the original process; 3) ISSG is used to clean the SiN x Reoxidation realizes the SiO2 top layer, and the thickness of the SiO2 top layer is precisely controlled by the ISSG process, which has a more stable thickness and better isolation characteristics; 4) The deposition of the SiO2 top layer in the ONO layer is reduced, simplifying the process.
[0195] The above description is only a preferred embodiment of the present invention and is not intended to impose any limitation on the technical solution of the present invention. Those skilled in the art should understand that, without departing from the spirit and principles of the present invention, the technical solution can also be subjected to several simple modifications and substitutions, and these modifications and substitutions are also within the scope of protection covered by the claims.
Claims
1. An EEPROM memory based on ISSG process, characterized in that: The memory uses the ISSG SiO2 layer as the gate dielectric layer of the core device and the input / output device, and the top layer of the ONO dielectric layer between the floating gate and the control gate of the storage tube is made of ISSG to SiN x The ONO dielectric layer includes HTO bottom layer, SiN x Middle layer and ISSG SiO2 top layer.
2. A method for preparing an EEPROM memory based on an ISSG process, characterized in that: The steps include: Step 1, pre-treating the silicon substrate, and filling five STI oxides on the upper surface of the silicon substrate, and then respectively injecting a storage tube source and drain, a low-voltage well, a medium-voltage well, a high-voltage well, and a storage tube well between adjacent STI oxides; Step 2, growing a SiO2 layer as a gate dielectric layer of a storage tube on the upper surface of a silicon substrate; photolithographically opening a tunneling window above a drain region of the storage tube, and then wet-etching the SiO2 layer in the tunneling window; and oxidizing and growing a SiO2 layer as a tunneling oxide layer at the etching tunneling window; Step 3, depositing a polysilicon layer on the tunnel oxide layer, photolithography covers the floating gate region of the storage tube, and etching the polysilicon layer to form a floating gate in the EEPROM unit; Step 4: deposit a NO layer on the substrate, the NO layer including the HTO bottom layer and the SiN x In the middle layer, the storage tube area is covered by photolithography, and then the NO layer and the storage tube gate dielectric layer of the core MOS, the NO layer and the storage tube gate dielectric layer of the input / output MOS, and the NO layer and the storage tube gate dielectric layer of the high-voltage MOS are etched away, and the NO layer and the storage tube gate dielectric layer of the storage tube area are retained; Step 5, oxidizing and growing the high-voltage gate dielectric layer of the high-voltage MOS, photolithography covers the high-voltage MOS and the storage pipe area, and then etching away the high-voltage gate dielectric layer of the core MOS and the high-voltage gate dielectric layer of the input / output MOS; Step 6: Use ISSG process to grow thick gate dielectric layer of input / output MOS. ISSG process also grows SiN layer of NO layer in storage pipe area. x The middle layer is then oxidized to the SiO2 top layer, and the input / output MOS, high-voltage MOS and storage pipe area are covered by photolithography, and then the thick gate dielectric layer of the core MOS is etched away; Step 7: Use ISSG process to grow the thin gate dielectric layer of the core MOS. The ISSG process also forms the SiN layer of the NO layer in the storage pipe area. x The middle layer continues to be reoxidized to the SiO2 top layer, and finally the NO layer in the storage tube area is converted into the ONO layer; Step 8, depositing a polysilicon layer, photolithography covering the polysilicon layer for etching, and completing the preparation of the gate of the EEPROM; Step 9: According to the known process, lightly doped source and drain implantation, sidewall deposition and etching, and source and drain implantation are completed to form a complete device structure.
3. The method for preparing an EEPROM memory based on ISSG process according to claim 2, characterized in that: When the feature size of the EEPROM memory process is above 0.25 μm, the preparation method does not include the photolithography and etching of the thick gate dielectric layer in step 6 and the entirety of step 7, and the STI oxide in step 1 is a field oxide and does not include a low voltage well.
4. The method for preparing an EEPROM memory based on ISSG process according to claim 2, characterized in that: In step 2, the SiO2 layer as the gate dielectric layer of the storage tube is grown by dry oxygen oxidation with O2 or wet oxygen oxidation with a volume ratio of H2:O2 of 1:(1-1.8) at a reaction temperature of 750°C-900°C for 10min-120min and a thickness of During etching, wet etching is adopted, and the etching solution is a buffered oxide etching solution with a volume ratio of NH4F:HF of 100:1; The SiO2 layer as the tunneling oxide layer is grown by dry oxygen oxidation with O2 or wet oxygen oxidation with a volume ratio of H2:O2 of 1:(1-1.8) at a reaction temperature of 750°C-900°C for 5min-30min and a thickness of 5. The method for preparing an EEPROM memory based on ISSG process according to claim 2, characterized in that: In step 3, the polysilicon layer used as the floating gate is prepared by first depositing by LPCVD method, then photolithography and then etching; During deposition, the reaction gas is SiH4, the temperature is 575℃~650℃, the pressure is 0.1Torr~5.0Torr, and the thickness is During etching, dry etching is adopted, the main gases are HBr, Cl2 and HeO2, the etching selectivity ratio of polysilicon to SiO2 is greater than 200:1, and the etching end point stays on SiO2.
6. The method for preparing an EEPROM memory based on ISSG process according to claim 2, characterized in that: In step 4, HTO bottom layer and SiN x The middle layers were deposited using the LPCVD method; When the HTO bottom layer is deposited, the reaction gas is SiH2Cl2 and N2O with a volume ratio of 1:(5-10), the reaction temperature is 800℃-900℃, the pressure is 0.1Torr-5.0Torr, the time is 5min-30min, and the thickness is S N x During the layer deposition, the reaction gas is SiH2Cl2 and NH3 with a volume ratio of 1: (5-10), the reaction temperature is 700℃-800℃, the pressure is 0.1Torr-5.0Torr, the time is 10min-60min, and the thickness is During etching, dry etching is used, and the main etching gases are CF4 and CHF3, SiN x The etching selectivity ratio for SiO2 is 10:1, and the etching endpoint stays on SiO2.
7. The method for preparing an EEPROM memory based on ISSG process according to claim 2, characterized in that: In step 5, the high-voltage gate dielectric layer of the high-voltage MOS is grown by dry oxidation with O2 or wet oxidation with a volume ratio of H2:O2 of 1:(1-1.8) at a reaction temperature of 750°C-950°C, a time of 10min-180min, and a thickness of During etching, wet etching is adopted, and the etching solution adopts a buffered oxide etching solution with a volume ratio of NH4F:HF of 100:
1.
8. The method for preparing an EEPROM memory based on ISSG process according to claim 2, characterized in that: In step 6, the thick gate dielectric layer is grown by an ISSG oxidation method with a volume ratio of H2:O2 of 1:(3-30) as the reaction gas, the reaction temperature is 900°C-1200°C, the time is 10s-240s, and the thickness is While the ISSG process is growing SiO2, the NO layer in the storage pipe area SiN x The middle layer is reoxidized to SiO2 top layer; During etching, wet etching is adopted, and the etching solution adopts a buffered oxide etching solution with a volume ratio of NH4F:HF of 100:
1.
9. The method for preparing an EEPROM memory based on ISSG process according to claim 2, characterized in that: In step 7, the thin gate dielectric layer is grown by an ISSG oxidation method with a reaction gas H2:O2 volume ratio of 1:(3-30), a reaction temperature of 900°C-1200°C, a time of 5s-120s, and a thickness of While the ISSG process is growing SiO2, the NO layer in the storage pipe area SiN x The middle layer is reoxidized to The SiO2 top layer.
10. The method for preparing an EEPROM memory based on ISSG process according to claim 2, characterized in that: In step 8, the polysilicon layer is deposited by LPCVD, the reaction gas is SiH4, the temperature is 575°C to 650°C, the pressure is 0.1 Torr to 5.0 Torr, and the thickness is The polycrystalline gate is etched by dry etching, the main etching gases are HBr, Cl2 and HeO2, the etching selectivity ratio of polysilicon to SiO2 is greater than 200:1, and the etching end point stays on SiO2.