Chiral photoelectric functional material with wide band gap and preparation method thereof

Through spin coating and heat treatment technology of chiral organic ammonium halide salts and metal halides, chiral photoelectric functional materials with band gap greater than 4.0 eV were prepared, solving the problems of narrow band gap and weak chirality of existing materials when working in the deep ultraviolet band. , improves the response capability to near-ultraviolet and visible light.

CN118922037APending Publication Date: 2024-11-08WUHAN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410962835.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing chiral optoelectronic functional materials have narrow band gaps and weak chiral optical properties when operating in the deep ultraviolet band, and cannot effectively respond to near-ultraviolet and visible light, resulting in limited device performance.

Method used

The precursor solution of chiral organic ammonium halide salt and metal halide in organic solvents was spin-coated and heat-treated to prepare chiral photoelectric functional materials with band gap greater than 4.0 eV. The band gap was calculated by the Tauc method and spin-coated and optimize molar ratios and conditions during heat treatment to improve the absorption asymmetry factor of the material.

Benefits of technology

The wide band gap and strong chiral optical properties of the material are achieved, the anti-interference ability to near-ultraviolet and visible light is improved, and the response ability of optoelectronic devices to deep ultraviolet light is expanded.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118922037A_ABST
    Figure CN118922037A_ABST
Patent Text Reader

Abstract

The invention discloses a chiral photoelectric functional material with a wide band gap and a preparation method of the chiral photoelectric functional material. The band gap width, calculated through a Tauc method, of the material is larger than 4.0 eV, and the absorption asymmetry factor, measured at the wavelength of 220-280 nm, of the material is larger than 10 <-2 >; the preparation method comprises the following steps: dissolving chiral organic halogenated ammonium salt and metal halide in an organic solvent to obtain a precursor solution; and carrying out spin coating on the precursor solution and then carrying out heat treatment to obtain the chiral photoelectric functional material with the wide band gap. The chiral photoelectric functional material is simple in structure, has the band gap width larger than 4.0 eV and the absorption asymmetry factor larger than 10 <-2 >, and compared with a traditional material, the chiral photoelectric functional material is better in anti-interference performance on near ultraviolet light and visible light, higher in chiral optical property and better in application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of chiral perovskite materials, and in particular to a chiral photoelectric functional material with a wide bandgap and a preparation method thereof. Background Art

[0002] With the development of optoelectronic technology and materials science, the research and development of new functional materials has occupied an important position in modern science and technology. The chiral optical properties of chiral optoelectronic functional materials make them widely used in devices such as optical rotation filters, circularly polarized light detectors and chiral optical sensors.

[0003] However, most of the chiral optoelectronic functional materials currently exhibit narrow band gaps (E g <3.5 eV) and weak chiral optical properties (light absorption asymmetry factor of 10 -3 The strong interference of near-ultraviolet and visible light makes the device unable to work in the deep ultraviolet band. In order to expand the response of optoelectronic devices to deep ultraviolet light, it is urgent to develop devices with wide band gap (E g >4.0 eV) chiral optoelectronic functional materials. Summary of the invention

[0004] In order to solve the problems existing in the prior art, the present invention provides a chiral optoelectronic functional material with a wide band gap, wherein the band gap width calculated by the Tauc method is greater than 4.0 eV, and the absorption asymmetry factor measured at a wavelength of 220-280 nm is greater than 10 -2 .

[0005] The present invention also provides a method for preparing the chiral optoelectronic functional material having a wide band gap, comprising: dissolving a chiral organic ammonium halide salt and a metal halide in an organic solvent to obtain a precursor solution; The precursor solution is spin-coated and then heat-treated to obtain a chiral optoelectronic functional material with a wide band gap.

[0006] Furthermore, the molar ratio of the chiral organic ammonium halide salt to the metal halide in the precursor solution is 1-2:1.

[0007] Furthermore, the organic solvent includes at least one of N,N-dimethylformamide, dimethyl sulfoxide, and isopropanol.

[0008] Furthermore, the spin coating is continued for 30-60 s at a rotation speed of 2000-5000 rpm.

[0009] Furthermore, the heat treatment is continued at 80-120° C. for 5-10 min.

[0010] Furthermore, the metal element in the metal halide is at least one of lead, cobalt, cesium and copper; The halogen element in the metal halide is at least one of chlorine, bromine and iodine.

[0011] In the present invention, it should be noted that spin coating is to drop the precursor solution on the transparent substrate and use a spin coater to spin coat the transparent substrate. The transparent substrate may be fluorine-doped SnO 2 One of glass (FTO glass), indium tin oxide glass (ITO glass), quartz glass, etc. The transparent substrate is also washed and treated with ultraviolet ozone (UVO) before use. The washing includes cleaning with detergent, deionized water, ethanol and isopropanol under ultrasonic action respectively, and the UVO treatment uses a UVO cleaning machine for 20-60 minutes.

[0012] Furthermore, the preparation method of the chiral organic ammonium halide salt comprises: The chiral organic amine and the aqueous solution of hydrohalic acid are mixed for reaction, and after the reaction, impurities are removed to obtain the chiral organic ammonium halide salt.

[0013] Preferably, after the chiral organic amine and the hydrohalic acid aqueous solution are mixed, a proper amount of ethanol is added. The ethanol is used as a reaction solvent to ensure that the reactants react fully, and the amount thereof does not need to be strictly limited.

[0014] Further, the organic chiral amine includes at least one of (R)-1-(1-naphthyl)ethylamine, (S)-1-(1-naphthyl)ethylamine, (R)-α-methylbenzylamine, (S)-α-methylbenzylamine, (R)-β-methylphenethylamine, (S)-β-methylphenethylamine, (R)-1-phenylpropylamine, (S)-1-phenylpropylamine, (R)-1-(2-naphthyl)ethylamine, (R)-1-(2-bromophenyl)-ethylamine, (S)-1-(2-bromophenyl)-ethylamine, (R)-1-(3-bromophenyl)-ethylamine, (S)-1-(3-bromophenyl)-ethylamine, (R)-1-(4-bromophenyl)-ethylamine, and (S)-1-(4-bromophenyl)-ethylamine; The volume ratio of the organic chiral amine to the hydrohalic acid aqueous solution is 1:1-2.

[0015] Preferably, the chiral organic amine is (R)-1-(1-naphthyl)ethylamine (R-NEA) or (S)-1-(1-naphthyl)ethylamine (S-NEA), and the hydrohalic acid aqueous solution is hydrochloric acid and hydrobromic acid aqueous solution. Accordingly, the chiral organic halide ammonium salt is preferably (R / S)-1-(1-naphthyl)ethylammonium chloride or (R / S)-1-(1-naphthyl)ethylammonium bromide.

[0016] Compared with the prior art, the present invention has the following beneficial effects: The chiral photoelectric functional material of the present invention has a simple structure, a band gap width greater than 4.0 eV and a -2 The absorption asymmetry factor is better than traditional materials in terms of anti-interference to near-ultraviolet and visible light, stronger chiral optical properties, and better application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0018] Figure 1 The optical band gap diagram of the chiral optoelectronic functional material prepared in Example 2 calculated according to the Tauc method is shown; Figure 2 The optical band gap diagram of the chiral optoelectronic functional material prepared in Example 4 calculated according to the Tauc method is shown; Figure 3 A diagram showing the circularly polarized light absorption asymmetry factor of the chiral optoelectronic functional material prepared in Example 2 is shown; Figure 4 The circularly polarized light absorption asymmetry factor diagram of the chiral optoelectronic functional material prepared in Example 4 is shown. DETAILED DESCRIPTION

[0019] The endpoints and any values ​​of the ranges disclosed in the present invention are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be regarded as specifically disclosed in the present invention.

[0020] The following will be combined with the specific embodiments of the present invention and the drawings of the specification to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0021] Example 1 A method for preparing a chiral optoelectronic functional material with a wide bandgap comprises the following steps: (1) Chiral organic amine S-NEA, 37% hydrochloric acid, and an appropriate amount of ethanol were mixed, with the volume ratio of S-NEA to hydrochloric acid being 3:5; nitrogen was pumped in and continuously passed through the mixture to maintain a vacuum environment, and the mixture was stirred in an ice-water bath for 2 h. The resulting solution was then evaporated at 80°C to remove ethanol and water, thereby obtaining (S)-1-(1-naphthyl)ethylammonium chloride (S-NEACl); (2) S-NEACl, PbCl 2 Dissolve in N,N-dimethylformamide at a molar ratio of 2:1 to obtain a precursor solution, wherein the concentration of S-NEACl in the precursor solution is 0.5 mol L -1 ; (3) The ITO glass was immersed in detergent, deionized water, isopropanol and ethanol respectively and ultrasonically cleaned for 15 min, and then dried with nitrogen. The cleaned ITO glass was then treated with ultraviolet ozone (UVO) for 30 min to obtain pretreated ITO glass; (4) 60 μL of the precursor solution was applied to the pretreated ITO glass surface; then the solution was transferred to a spin coater for spin coating and spun at 3500 rpm for 50 s to form a thin film, which was then annealed on a 100°C heating table for 10 min to induce crystallization, thereby obtaining a chiral optoelectronic functional material with a wide band gap.

[0022] Example 2 A method for preparing a chiral optoelectronic functional material with a wide bandgap comprises the following steps: (1) Chiral organic amine R-NEA, 37% hydrochloric acid, and an appropriate amount of ethanol were mixed, with the volume ratio of R-NEA to hydrochloric acid being 3:5; nitrogen was pumped in and continuously passed through the mixture to maintain a vacuum environment, and the mixture was stirred in an ice-water bath for 2 h. The resulting solution was then evaporated at 80°C to remove ethanol and water, thereby obtaining (R)-1-(1-naphthyl)ethylammonium chloride (R-NEACl); (2) R-NEACl, PbCl 2 Dissolve in N,N-dimethylformamide at a molar ratio of 2:1 to obtain a precursor solution, wherein the concentration of R-NEACl in the precursor solution is 0.5 mol L -1 ; (3) The ITO glass was immersed in detergent, deionized water, isopropanol and ethanol respectively and ultrasonically cleaned for 15 min, and then dried with nitrogen. The cleaned ITO glass was then treated with ultraviolet ozone (UVO) for 30 min to obtain pretreated ITO glass; (4) 60 μL of the precursor solution was applied to the pretreated ITO / glass surface; then the surface was transferred to a spin coater for spin coating and spun at 3500 rpm for 50 s to form a thin film, which was then annealed on a 100°C heating table for 10 min to induce crystallization, thereby obtaining a chiral optoelectronic functional material with a wide band gap.

[0023] Example 3 A method for preparing a chiral optoelectronic functional material with a wide bandgap comprises the following steps: (1) Chiral organic amine S-NEA, 48% hydrobromic acid aqueous solution, and an appropriate amount of ethanol were mixed, with the volume ratio of S-NEA to hydrobromic acid aqueous solution being 3:5; nitrogen was pumped and continuously passed through to maintain a vacuum environment, and the mixture was stirred in an ice-water bath for 2 h. The resulting solution was then evaporated at 80°C to remove ethanol and water, thereby obtaining (S)-1-(1-naphthyl)ethylammonium bromide (S-NEABr); (2) S-NEABr, CoBr 2 Dissolve in N,N-dimethylformamide at a molar ratio of 1:1 to obtain a precursor solution, wherein the concentration of S-NEABr in the precursor solution is 1 mol L -1 ; (3) The ITO glass was immersed in detergent, deionized water, isopropanol and ethanol respectively and ultrasonically cleaned for 15 min, and then dried with nitrogen. The cleaned ITO glass was then treated with ultraviolet ozone (UVO) for 30 min to obtain pretreated ITO glass; (4) 60 μL of the precursor solution was applied to the pretreated ITO / glass surface; then the surface was transferred to a spin coater for spin coating and spun at 5000 rpm for 60 s to form a thin film, which was then annealed on a 120°C heating table for 8 min to induce crystallization, thereby obtaining a chiral optoelectronic functional material with a wide band gap.

[0024] Example 4 A method for preparing a chiral optoelectronic functional material with a wide bandgap comprises the following steps: (1) Chiral organic amine R-NEA, 48% hydrobromic acid aqueous solution, and an appropriate amount of ethanol were mixed, with the volume ratio of R-NEA to hydrobromic acid aqueous solution being 3:5; nitrogen was pumped and continuously passed through the vacuum environment to maintain the vacuum environment, and the reaction was stirred in an ice-water bath for 2 h. The resulting solution was then evaporated at 80°C to remove ethanol and water, thereby obtaining (R)-1-(1-naphthyl)ethylammonium bromide (R-NEABr); (2) R-NEABr, CoBr 2 Dissolved in N,N-dimethylformamide at a molar ratio of 1:1 to obtain a precursor solution, wherein the concentration of R-NEABr in the precursor solution is 1 mol L -1 ; (3) The ITO glass was immersed in detergent, deionized water, isopropanol and ethanol respectively and ultrasonically cleaned for 15 min, and then dried with nitrogen. The cleaned ITO glass was then treated with ultraviolet ozone (UVO) for 30 min to obtain pretreated ITO glass; (4) 60 μL of the precursor solution was applied to the pretreated ITO / glass surface; then the surface was transferred to a spin coater for spin coating and spun at 5000 rpm for 60 s to form a thin film, which was then annealed on a 120°C heating table for 8 min to induce crystallization, thereby obtaining a chiral optoelectronic functional material with a wide band gap.

[0025] like Figure 1 and Figure 2 As shown, the optical band gaps of the chiral optoelectronic functional materials prepared in Example 2 and Example 4 calculated according to the Tauc method are 4.09 eV and 4.11 eV, respectively, which are far greater than the band gap widths of most chiral optoelectronic functional materials currently available (less than 3.5 eV). This shows that the present invention optimizes the ligand selection by a relatively simple method and successfully prepares chiral metal halide optoelectronic materials with a band gap greater than 4.0 eV. Such a wide band gap may be related to the inorganic components in the crystal, because the orbits of the conduction band and valence band of the chiral metal halide are both composed of hybridization between metal and halogen, which further determines the band structure of the material. In addition, for halide anions, their p orbitals participate in hybridization, and compared with the I 5p energy, Cl 3p and Br 4p have lower energy, so when Cl or Br is used as a halogen anion, the material will exhibit a wider band gap.

[0026] The circular polarization spectrometer was used to test the circular polarization light absorption asymmetry factor of the chiral optoelectronic functional materials prepared in Example 2 and Example 4. Figure 3 and Figure 4 It can be seen that at a wavelength of 220-280 nm, the circularly polarized light absorption asymmetry factors of the chiral optoelectronic functional materials prepared in Example 2 and Example 4 are 0.012 and 0.03, respectively. However, the light absorption asymmetry factors of the chiral optoelectronic materials reported so far are between 10 -3 These results also show that the materials prepared by the present invention have strong chiral optical properties.

[0027] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A chiral optoelectronic functional material with a wide bandgap, characterized in that: The band gap width of the material calculated by the Tauc method is greater than 4.0 eV, and the absorption asymmetry factor measured at a wavelength of 220-280 nm is greater than 10 -2 .

2. A method for preparing a chiral optoelectronic functional material with a wide band gap as claimed in claim 1, characterized in that: include, dissolving a chiral organic ammonium halide salt and a metal halide in an organic solvent to obtain a precursor solution; The precursor solution is spin-coated and then heat-treated to obtain a chiral optoelectronic functional material with a wide band gap.

3. The preparation method according to claim 2, characterized in that: The molar ratio of the chiral organic ammonium halide salt to the metal halide in the precursor solution is 1-2:

1.

4. The preparation method according to claim 2, characterized in that: The organic solvent includes at least one of N,N-dimethylformamide, dimethyl sulfoxide and isopropanol.

5. The preparation method according to claim 2, characterized in that: The spin coating was continued for 30-60 s at a rotation speed of 2000-5000 rpm.

6. The preparation method according to claim 2, characterized in that: The heat treatment lasts for 5-10 min at 80-120°C.

7. The preparation method according to claim 2, characterized in that: The metal element in the metal halide is at least one of lead, cobalt, cesium and copper; The halogen element in the metal halide is at least one of chlorine, bromine and iodine.

8. The preparation method according to any one of claims 2 to 7, characterized in that: The preparation method of the chiral organic ammonium halide salt comprises: The chiral organic amine and the hydrohalic acid aqueous solution are mixed and reacted, and then impurities are removed to obtain the chiral organic ammonium halide salt.

9. The preparation method according to claim 8, characterized in that: The organic chiral amine includes at least one of (R)-1-(1-naphthyl)ethylamine, (S)-1-(1-naphthyl)ethylamine, (R)-α-methylbenzylamine, (S)-α-methylbenzylamine, (R)-β-methylphenethylamine, (S)-β-methylphenethylamine, (R)-1-phenylpropylamine, (S)-1-phenylpropylamine, (R)-1-(2-naphthyl)ethylamine, (R)-1-(2-bromophenyl)-ethylamine, (S)-1-(2-bromophenyl)-ethylamine, (R)-1-(3-bromophenyl)-ethylamine, (S)-1-(3-bromophenyl)-ethylamine, (R)-1-(4-bromophenyl)-ethylamine, and (S)-1-(4-bromophenyl)-ethylamine; The volume ratio of the organic chiral amine to the hydrohalic acid aqueous solution is 1:1-2.