Preparation method of pi-type p-HMS / n-InSb medium-temperature thermal electric device
By using MnSi and InSb materials, combined with V and Mo barrier layers, and using SPS sintering technology to prepare medium-temperature thermoelectric devices, the problem of high cost and toxicity of existing thermoelectric devices is solved, and efficient thermoelectric conversion performance and green non-toxicity are achieved. mid-temperature thermoelectric device applications.
Patent Information
- Application Number
- CN202410997055.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-08
AI Technical Summary
The existing medium and high temperature thermoelectric devices are costly and toxic, making it difficult to meet large-scale production applications, especially in the field of medium and high temperature waste heat recovery, and lack of green, non-toxic and stable thermoelectric materials.
MnSi (high manganese silicon, HMS) and InSb are used as materials for π-type thermoelectric devices, V and Mo are used as barrier layers, and p-HMS and n-InSb are prepared by SPS sintering technology, and medium temperature is formed by welding. Thermoelectric devices, optimize the interface structure to improve performance.
It realizes efficient thermoelectric conversion efficiency and output power at medium temperature. The maximum conversion efficiency of the device reaches 3.75%, the maximum output power is 106.9mW, and the material is green and non-toxic, suitable for large-scale production.
Smart Images

Figure CN118922049A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of new energy thermoelectric functional materials, and in particular to a method for preparing a π-type p-HMS / n-InSb medium-temperature thermoelectric device. Background Art
[0002] Thermoelectric semiconductor materials can realize the mutual conversion of heat energy and electrical energy, and have broad application prospects in the fields of industrial waste heat, automobile waste heat, decentralized micro-heat source power generation and thermoelectric refrigeration in life and production. The quality of thermoelectric performance can be measured by the dimensionless thermoelectric figure of merit zT = S 2 σT / κ tot Measure, where S, σ, κ tot , T represent the Seebeck coefficient, electrical conductivity, total thermal conductivity and absolute temperature of the material respectively.
[0003] In recent years, the global demand for energy has been increasing, and the research on thermoelectric devices has also developed rapidly, which has led to a series of improvements in the performance of thermoelectric devices. Qu et al. from Harbin Institute of Technology developed a Bi-ion battery with a thermoelectric conversion efficiency of 7.1% at a temperature difference of 230K. 2 Te 3 Based on thermoelectric devices, it is obvious that the conversion efficiency is higher than that of Bi 2 Te 3 The value of GeTe / PbTe based devices (4% to 7%) is higher. PbTe based thermoelectric materials provide continuous, stable and reliable electrical energy for deep space probes, using isotope decay heat as the heat source to achieve a thermoelectric conversion efficiency of 5% to 6%. When the hot end temperature is 773K and the temperature difference ΔT is 473K, the thermoelectric conversion efficiency of GeTe / PbTe thermoelectric devices can reach about 11.3%, and after 50 cycles of aging experiments, the device performance can still remain stable. The 8 pairs of Half-Heusler single-stage thermoelectric devices developed by Xing et al. from the Shanghai Institute of Silicates have a maximum conversion efficiency of 9.6% when ΔT is 680K, and a power density of 3.1Wcm -2 .
[0004] To date, the thermoelectric materials commonly used in applications are mainly bismuth telluride, lead telluride and other chalcogenides due to their high efficiency. However, their widespread application is limited by the toxic and / or rare element content (Pb, Te, etc.), high raw material cost, poor mechanical properties and high vapor pressure in the efficiency peak temperature range. Nowadays, many other materials are studied as candidates for thermoelectric applications, among which metal silicides have become one of the most interesting alternatives. They have good thermoelectric properties and are low in raw material cost, non-toxic, lightweight, good mechanical and chemical stability and high oxidation resistance. MnSi γHigh manganese silicon (HMS) represented by (1.67<γ<1.77) has the characteristics of high melting point, low diffusion coefficient of silicon in HMS matrix, large Seebeck coefficient and low resistivity. Therefore, they are considered to be promising p-leg candidates for thermoelectric devices operating in the medium and high temperature range. Chen et al. doped Al and Ge elements into Si, and the carriers were improved, and zT reached 0.57 at 823K. Muthiah et al. studied Al-doped MnSi 1.73 The zT reaches 0.82.
[0005] Based on a large number of previous studies on thermoelectric materials, the types of p-type thermoelectric materials in the medium temperature range are more abundant than those of n-type thermoelectric materials, and p-type thermoelectric materials generally have better performance than n-type thermoelectric materials. So far, n-type thermoelectric materials with excellent thermoelectric performance in the medium temperature range are mainly CoSb 3 Based on the raw materials, the raw materials are mainly Te-based compounds and Pb-based compounds. The large-scale use of rare elements and Pb brings challenges of high cost and environmental pollution, and at the same time limits the large-scale production of thermoelectric materials. Based on this, the environmentally friendly III-V compound InSb is considered to be a potential N-type thermoelectric material. R. Bower et al. prepared polycrystalline InSb by zone melting, and the zT value was about 0.4 at 772K. Yamaguchi et al. used chemical vapor deposition to grow n-type Te-doped InSb single crystals, and the maximum zT value was 0.6 at 673K.
[0006] Thermoelectric generators (TEGs) can achieve direct conversion of thermal energy and electrical energy. As a clean energy conversion technology with compact structure, high reliability and no noise, thermoelectric generators can be used in aerospace, industrial waste heat recovery, flexible wearable self-powered devices and other fields. In recent years, the development of TEGs has made certain progress. At present, the thermoelectric devices that can be commercially applied are mainly Bi 2 Te 3 Based on thermoelectric devices, they cannot better meet the temperature reached by waste heat recovery, so the research and development and preparation of medium and high temperature devices are inevitable. The materials contained in the medium and high temperature thermoelectric devices currently studied are generally expensive and toxic, and are not suitable for large-scale production applications. Therefore, using green, non-toxic, and stable medium-temperature thermoelectric materials HMS and InSb as the p and n thermoelectric arms of thermoelectric devices, studying the selection of barrier layer materials when used as medium-temperature thermoelectric devices, as well as the welding and output performance testing of the devices has become an issue of important production practical significance. Summary of the invention
[0007] The purpose of the present invention is to provide a method for preparing a π-type p-HMS / n-InSb medium-temperature thermoelectric device, which comprises the following steps: using Mn powder and Si powder as thermoelectric materials, using V as a barrier layer raw material, sequentially loading them into a graphite mold and sintering them through SPS to make a p-HMS thermoelectric single arm; then using InSb as a thermoelectric material, using Mo as a barrier layer, sequentially loading them into a graphite mold and sintering them through SPS to make an n-InSb thermoelectric single arm; and finally assembling them; and obtaining the temperature at T by simulation. h =450℃, ΔT=420K, the device has a maximum conversion efficiency of 3.75%, and the maximum output power of the device is 106.9mW. h When the temperature is 450°C and the temperature difference ΔT is 420K, the open circuit voltage is 120.4mV, the internal resistance is 82.5mΩ, and the maximum output power and maximum conversion efficiency of the device are 43.9mW and 1.56% respectively, thereby solving the problems existing in the above-mentioned prior art.
[0008] To achieve the above object, the present invention provides the following solutions:
[0009] One of the technical solutions of the present invention is to provide a π-type p-HMS / n-InSb medium-temperature thermoelectric device, wherein the π-type p-HMS / n-InSb medium-temperature thermoelectric device is composed of a p-type HMS thermoelectric single arm and an n-type InSb thermoelectric single arm welded together;
[0010] The p-type HMS thermoelectric single arm uses Mn powder and Si powder as thermoelectric materials, and V as a barrier layer raw material;
[0011] The n-type InSb thermoelectric single arm uses InSb as the thermoelectric material and Mo as the barrier layer.
[0012] Furthermore, the molar ratio of the Mn powder to the Si powder is 1:1.68-1.80.
[0013] The second technical solution of the present invention is to provide a method for preparing the above-mentioned π-type p-HMS / n-InSb medium-temperature thermoelectric device, the steps comprising:
[0014] The Mn powder and the Si powder are mixed, ball-milled and dried to obtain the HMS-based precursor powder;
[0015] The HMS-based precursor powder is used as the thermoelectric material, and the V powder is used as the barrier layer raw material. After assembling according to the barrier layer-thermoelectric material-barrier layer structure, the p-type HMS thermoelectric single arm is obtained by sintering.
[0016] In particles and Sb particles are used as reaction raw materials, and InSb powder is obtained through calcination, quenching and grinding;
[0017] The InSb powder is used as the thermoelectric material, the Mo powder is used as the barrier layer, and the structure of barrier layer-thermoelectric material-barrier layer is assembled, and then sintered to obtain an n-type InSb thermoelectric single arm;
[0018] The p-type HMS thermoelectric single arm and the n-type InSb thermoelectric single arm are welded on a substrate to form a pn pair, thereby obtaining the π-type p-HMS / n-InSb medium-temperature thermoelectric device.
[0019] Furthermore, the ball milling is wet ball milling, the ball-to-material ratio is 20:1, the rotation speed is 350 rpm, the time is 1 to 4 hours, and the solvent is n-hexane.
[0020] Furthermore, the drying temperature is 55° C. and the drying time is 12 hours.
[0021] Furthermore, the p-type HMS thermoelectric single arm is sintered by spark plasma sintering (SPS sintering) under vacuum conditions.
[0022] Preferably, the vacuum condition is 1.0×10 -4 ~1.0×10 -3 Pa; the spark plasma sintering pressure is 40 to 80 MPa, the temperature is 950 to 1100°C, the heating rate is 50°C / min, and the time is 5 to 20 min.
[0023] In the process of SPS sintering to obtain a p-type HMS thermoelectric single arm, the SPS sintering procedure is divided into four stages, preferably a heating stage of 30 to 1000°C, a secondary heating stage of 1000 to 1050°C, sintering at 1050°C, and cooling from 1050 to 30°C, wherein the cooling is natural cooling.
[0024] Furthermore, the calcination is carried out under vacuum conditions not exceeding 4×10 -3 Pa, and then heated to 800 °C at a heating rate of 60 K / h and kept at that temperature for 6 h.
[0025] Furthermore, the n-type InSb thermoelectric single arm is obtained by sintering by SPS under vacuum conditions.
[0026] Preferably, the vacuum condition is 1.0×10 -4 ~1.0×10 -3 The SPS sintering pressure is 40-80MPa, the temperature is 450°C, the heating rate is 50°C / min, and the holding time is 10min.
[0027] Furthermore, the substrate is a ceramic substrate.
[0028] The third technical solution of the present invention is to provide an application of the above-mentioned π-type p-HMS / n-InSb medium-temperature thermoelectric device in medium-temperature waste heat recovery.
[0029] The present invention discloses the following technical effects:
[0030] The present invention uses V as the barrier layer material of the p-type HMS thermoelectric single arm, and generates V after one-step SPS sintering. 3 Si phase hinders the further diffusion of elements at the interface. When Mo is used as the barrier layer material of n-type InSb thermoelectric single arm, no element reaction occurs at the interface after one-step SPS sintering, and the stratification is obvious.
[0031] After aging treatment for 1 to 7 days, the resistivity of HMS and InSb increased from 7.82 μΩcm to 2 and 17.93 μΩcm 2 It becomes 9.47μΩcm 2 and 21.05μΩcm 2 The change is small. In addition, the thermal expansion coefficient of V and Mo is 11.3×10 -6 K -1 , 5.58×10 - 6 K -1 Compared with HMS (12.53×10 -6 K -1 ) and InSb(5.9×10 -6 K -1 )’s thermal expansion coefficients match each other, which is beneficial to interface contact.
[0032] The output performance of a single-arm p-HMS and n-InSb thermoelectric device with a size of 3.0 mm × 3.0 mm × 10.0 mm was simulated, and the results showed that the output performance of a single-arm p-HMS and n-InSb thermoelectric device with a size of 3.0 mm × 3.0 mm × 10.0 mm was h When =450℃, ΔT=420K, the output voltage and maximum output power of HMS single arm are 44.2mV and 47.9mW respectively, and the output voltage and maximum output power of InSb single arm are 56.7mV and 78.8mW respectively.
[0033] Mini-PEM was used to test a single pair of devices at T h =450℃, ΔT=420K, the open circuit voltage is 120.4mV, the internal resistance is 82.5mΩ, the maximum output power and maximum conversion efficiency of the device are 43.9mW and 1.56% respectively, and when the temperature difference is 420K, its power density is 0.33W / cm 2 .
[0034] Different from the current mainstream commercial Bi 2 Te 3Based thermoelectric devices, the π-type p-HMS / n-InSb-based thermoelectric devices prepared by the present invention adopt silicon-based compounds and antimonide thermoelectric materials: on the one hand, HMS and InSb have stable thermal and chemical properties in a medium temperature (500-800K) environment, which can better meet the purpose of medium temperature waste heat recovery; on the other hand, the elements involved in both HMS and InSb materials are green, non-toxic, cheap and abundant, and are more suitable for large-scale production applications.
[0035] The present invention first prepares a predetermined ratio of Mn-Si mixed powder and InSb powder, uses SPS vacuum high temperature sintering environment to obtain HMS and InSb thermoelectric materials, tests and analyzes their thermoelectric properties, and tests and analyzes the thermal expansion coefficient and work function of HMS and InSb, then selects V and Mo as barrier layer materials, uses one-step SPS sintering to prepare thermoelectric materials / barrier layer materials, and obtains thermoelectric devices by forming pn pairs. Using V and Mo as barrier layer materials reduces the diffusion of elements at the interface, so that the interface is well bonded and 7.82μΩcm is obtained respectively. 2 and 17.93 μΩcm 2 The smaller contact resistivity is far lower than the device standard value. h =450℃, ΔT=420K, the device has a maximum conversion efficiency of 3.75%, and the maximum output power of the device is 106.9mW. h When the temperature is 450℃ and the temperature difference ΔT is 420K, the open circuit voltage is 120.4mV, the internal resistance is 82.5mΩ, and the maximum output power and maximum conversion efficiency of the device are 43.9mW and 1.56% respectively.
[0036] The preparation method of the invention is simple, low in cost, green and non-toxic, and has good stability. The invention is a medium-temperature thermoelectric device that can better meet the temperature reached by waste heat recovery. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0038] Figure 1 The process flow chart of preparing π-type p-HMS / n-InSb medium-temperature thermoelectric device of the present invention;
[0039] Figure 2Graphs of thermal expansion coefficients of thermoelectric material HMS and Ni, Fe, Co, V, Cr and Mo in p-HMS, wherein (a) is a graph of thermal expansion coefficients of thermoelectric material HMS in p-HMS at different temperatures, and (b) is a graph of thermal expansion coefficients of Ni, Fe, Co, V, Cr and Mo;
[0040] Figure 3 The thermal expansion coefficient diagram and UPS photoelectron spectrum of the thermoelectric material InSb in n-InSb, where (a) is the thermal expansion coefficient diagram and (b) is the UPS photoelectron spectrum;
[0041] Figure 4 UPS photoelectron spectrum of thermoelectric material HMS in p-HMS;
[0042] Figure 5 Comparison diagram of interface contact resistivity of different thermoelectric single-arm materials, XRD spectrum of V / HMS sample, SEM image of V / HMS interface junction and EDS surface scan of V / HMS interface junction, where (a) is a comparison diagram of interface contact resistivity of different thermoelectric single-arm materials, (b) is the XRD spectrum of V / HMS sample, (c) is the SEM image of V / HMS interface junction, (d) to (g) are EDS surface scans of V / HMS interface junction;
[0043] Figure 6 The SEM characterization images and elemental surface scans of the V / HMS interface after aging treatment of p-HMS for 1, 2, 4, and 7 days, where (a) is 1 day, (b) is 2 days, (c) is 4 days, and (d) is 7 days;
[0044] Figure 7 The curve of the contact resistivity of the V / HMS interface of p-HMS changing with the aging time;
[0045] Figure 8 The XRD pattern of the Mo / InSb interface of n-InSb, the SEM characterization pattern and the elemental surface scan pattern of the Mo / InSb interface, wherein (a) is the XRD pattern of the Mo / InSb interface of n-InSb, (b) is the SEM characterization pattern of the Mo / InSb interface, and (c) to (f) are elemental surface scan patterns of the Mo / InSb interface;
[0046] Fig. 9 The SEM characterization images and elemental surface scans of the Mo / InSb interface after aging treatment of n-InSb for 1, 2, 4, and 7 days, where (a) is 1 day, (b) is 2 days, (c) is 4 days, and (d) is 7 days;
[0047] Fig.10The Mo / InSb interface contact resistivity of n-InSb varies with aging time;
[0048] Fig.11 The graph of the thermoelectric conversion efficiency of the π-type p-HMS / n-InSb medium-temperature thermoelectric device as a function of height and the ratio of the p and n cross-sectional areas (a), the simulated temperature field distribution (b), the maximum conversion efficiency and maximum output power of the device (c), and the power density as a function of temperature (d);
[0049] Fig.12 The curves of voltage, output power, conversion efficiency with current, and maximum conversion efficiency, maximum output power, power density, and device internal resistance with temperature difference of the π-type p-HMS / n-InSb medium-temperature thermoelectric device, where (a) is the curve of device voltage with current, (b) is the curve of device output power with current, (c) is the curve of device conversion efficiency with current, (d) is the curve of maximum conversion efficiency and maximum output power with temperature difference, (e) is the curve of power density with temperature difference, and (f) is the curve of device internal resistance with temperature difference;
[0050] Fig.13 For n-type Mg 2 Performance curves of segmented thermoelectric devices with Si and p-type high manganese silicide (HMS) as high temperature segments and n-type and p-type Bi-Te as low temperature segments, where (a) is the output power variation curve of two pairs of segmented thermoelectric devices with load current under different temperature differences, and (b) is the maximum conversion efficiency variation of two pairs of segmented thermoelectric devices with temperature;
[0051] Fig.14 p-HMS / n-InSb medium-temperature thermoelectric devices and commercial Bi 2 Te 3 The devices are assembled in series and parallel to obtain p-HMS / n-InSb / commercial Bi 2 Te 3 Performance curves of the double-layer thermoelectric device, where (a) is the maximum output power and (b) is the maximum conversion efficiency versus temperature. DETAILED DESCRIPTION
[0052] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0053] It should be understood that the terms described in the present invention are only for describing a particular embodiment and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0054] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0055] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.
[0056] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0057] Unless otherwise specified, the reagents and materials used in the specific embodiments of the present invention are all commercially available products.
[0058] Example 1
[0059] The preparation steps of π-type p-HMS / n-InSb medium-temperature thermoelectric device are as follows:
[0060] S1. Place Mn and Si in a clean cemented carbide ball mill at a molar ratio of 1:1.79, with a ball-to-material ratio of 20:1. Inject 50 mL of n-hexane solvent into the ball mill, seal it, and put it into a ball mill. Mill it at a speed of 350 rpm for 2 hours. After ball milling, place the ball mill containing the mixture in a vacuum drying oven and dry it for 12 hours at a temperature of 65°C. After drying, take out the ball mill after the temperature drops to room temperature to obtain HMS-based precursor powder.
[0061] S2, using HMS-based precursor powder as thermoelectric material and V powder as barrier layer raw material, they are loaded into the mold in the order of barrier layer-thermoelectric material-barrier layer, and the vacuum degree is maintained at 1.0×10 -3Pa, axial pressure of 60MPa, SPS heating program (heating rate of 50℃ / min) is 10min to 1000℃, then 1min to 1050℃, and then sintered at 1050℃ for 8min to form a cylindrical block with a diameter of 15mm, i.e., p-type HMS thermoelectric single-arm material.
[0062] S3, In particles and Sb particles were placed in a clean quartz tube at a molar ratio of 1:1, and then the vacuum in the quartz tube was evacuated to 4×10 -3 Pa, and then seal the quartz tube, place the sealed quartz tube vertically in a high-temperature box furnace, slowly heat it to 800°C at a heating rate of 60K / h, keep it at this temperature for 6 hours to fully react, and finally quench it in ice water, grind the ingot into powder using an agate mortar to obtain InSb powder;
[0063] S4, InSb powder is used as thermoelectric material and Mo powder is used as barrier layer. They are loaded into the mold in the order of barrier layer-thermoelectric material-barrier layer. The vacuum degree is maintained at 1.0×10 -3 Under the conditions of 2000 ℃, axial pressure of 50 MPa, sintering temperature of 450℃ (heating rate of 50℃ / min), and holding time of 10 min, a cylindrical block with a diameter of 15 mm was sintered by SPS, i.e., n-type InSb thermoelectric single-arm material.
[0064] S5. The p-type HMS thermoelectric single arm material and the n-type InSb thermoelectric single arm material are polished to the same height using a polishing machine. Since the barrier layer material has poor wettability and direct welding is not firm, a layer of copper is electroplated on the upper and lower surfaces for transition. Finally, the copper-plated samples are cut using diamond wire according to the required size to obtain the p-type HMS thermoelectric single arm (p-HMS) and the n-type InSb thermoelectric single arm (n-InSb).
[0065] S6, applying a layer of tin-silver-copper solder paste on the upper and lower surfaces of the p-type HMS thermoelectric single arm and the n-type InSb thermoelectric single arm, and then forming a pn pair with the p-type HMS thermoelectric single arm and the n-type InSb thermoelectric single arm, fixing them on a ceramic substrate, and then placing them in a vacuum drying oven at 120° C. for 1 hour to remove organic components in the solder paste;
[0066] S7. Place the dried pn pair in a graphite mold and weld them by SPS. The welding process is as follows: pressure 5.0 MPa, temperature 470 °C, time 10 min, and heating rate 15 °C / min. Finally, use solder to weld two wires on the lower ceramic substrate to obtain a single pair of π-type p-HMS / n-InSb medium-temperature thermoelectric devices.
[0067] Comparative Example 1
[0068] By n-type Mg 2 During the manufacturing process of the medium-temperature thermoelectric device composed of (Si, Sn) and p-type HMS, the raw materials are first placed in a mold for SPS sintering to prepare Mg 2 (Si, Sn) and HMS thermoelectric materials, and then use magnetron sputtering technology to deposit a barrier layer composed of Ti / Au on the upper and lower surfaces of the thermoelectric material, and then weld it with the metal electrode. 2 The segmented thermoelectric devices with Si and p-type high manganese silicide HMS as the high temperature segment and n-type and p-type Bi-Te as the low temperature segment are also prepared by SPS sintering to prepare the corresponding thermoelectric materials. Then, the thermoelectric arms are welded to the Cu electrodes with Ag-Cu-Sn-Zn alloy. The welding process is carried out in an environment with a gas flow of 95% Ar and 5% hydrogen (2L / min) to prevent oxidation and contamination of the joint interface during high temperature.
[0069] Test example
[0070] The thermoelectric properties of the π-type p-HMS / n-InSb medium-temperature thermoelectric device prepared in Example 1 were tested, including thermal expansion coefficient test, UPS test, XRD test, SEM test, EDS test, Mini-PEM test, electrical property test and thermal property test.
[0071] The aging treatment method is as follows: in order to observe the changes in the interface microstructure of the thermoelectric device under service, the prepared single-arm element is vacuum-sealed with a quartz tube and placed in a high-temperature box furnace for constant temperature aging tests for different times. Since the use temperature of the prepared thermoelectric device is below 450°C, the aging temperature is set to 450°C for 1, 2, 4, and 7 days, respectively, to observe the changes in the interface microstructure and the changes in the interface contact resistance after aging at different times.
[0072] Figure 1 The process flow chart of the present invention for preparing π-type p-HMS / n-InSb medium-temperature thermoelectric devices.
[0073] Figure 2 Figure 2 is a graph of thermal expansion coefficients of thermoelectric material HMS and Ni, Fe, Co, V, Cr and Mo in p-HMS, where (a) is a graph of thermal expansion coefficients of thermoelectric material HMS in p-HMS at different temperatures, and (b) is a graph of thermal expansion coefficients of Ni, Fe, Co, V, Cr and Mo. Figure 2 It can be seen that in (a), within the temperature range of 50 to 450 °C, the average thermal expansion coefficient of HMS is 12.53 × 10 -6 K -1 ; (b) The thermal expansion coefficient of V (11.3×10 -6 K -1) is closer to the thermal expansion coefficient value of HMS.
[0074] Figure 3 The thermal expansion coefficient diagram and UPS photoelectron spectrum of the thermoelectric material InSb in n-InSb, where (a) is the thermal expansion coefficient diagram and (b) is the UPS photoelectron spectrum. Figure 3 It can be seen that in (a), within the temperature range of 50 to 450°C, the linear expansion coefficient of InSb is 5.90×10 -6 K -1 The work function of InSb was tested and analyzed using an X-ray photoelectron spectrometer (XPS ESCALAB 250Xi). Since the electron energy of the ultraviolet light source is 21.2 eV, according to the formula Φ = hv-(E F -E Cutoff ) to calculate the work function of the test material, where E Cutoff is the inelastic electron cutoff edge, E F is the Fermi level; (b) the inelastic electron cutoff edge energy E of InSb Cutoff is 0.55eV, and the Fermi level E F It is 16.9eV, so after calculation, it can be obtained that the work function of InSb is 4.85eV.
[0075] Figure 4 is the UPS photoelectron spectrum of the thermoelectric material HMS in p-HMS, Figure 4 It can be seen that the Fermi level of HMS is at 16.4 eV, and the inelastic electron cutoff energy is -0.08 eV. According to the formula Φ = hv-(E F -E Cutoff ) calculated the work function of HMS to be 4.72 eV.
[0076] Figure 5 Comparison diagram of interface contact resistivity of different thermoelectric single-arm materials, XRD spectrum of V / HMS sample, SEM image of V / HMS interface junction and EDS surface scan of V / HMS interface junction, among which, (a) is the comparison diagram of interface contact resistivity of different thermoelectric single-arm materials, (b) is the XRD spectrum of V / HMS sample, (c) is the SEM image of V / HMS interface junction, (d) to (g) are EDS surface scans of V / HMS interface junction. Figure 5 V / HMS is the interface of the p-type HMS thermoelectric single-arm material in the present invention) Figure 5 It can be seen that the contact resistivity at the Cr / HMS interface in (a) is relatively high; in (b), the sintered sample is ground and measured layer by layer. The first layer matches the V standard card well, and V is found in the second layer. 3 The formation of Si phase, and the third layer with Mn 15Si 26 The results of EDS scan also show that the elements on both sides are evenly distributed, the interface is well bonded, and no cracks are found, indicating that when V is used as a barrier layer raw material, it does not affect the sample itself and has good mechanical properties.
[0077] Figure 6 The SEM characterization images and elemental surface scans of the V / HMS interface after aging treatment of p-HMS for 1, 2, 4, and 7 days, where (a) is 1 day, (b) is 2 days, (c) is 4 days, and (d) is 7 days. Figure 6 It can be seen that after 7 days of aging treatment, there are no cracks or holes at the interface, showing good mechanical properties. This is mainly due to the V generated during the SPS sintering process. 3 The Si reaction layer blocks the further reaction and diffusion of V and HMS.
[0078] Figure 7 The curve of the contact resistivity of the V / HMS interface of p-HMS versus aging time is shown in Figure 2. Figure 7 It can be seen that after 7 days of aging treatment, the interface contact resistivity is 9.47μΩcm 2 , the change is small (18.5%), which may be because HMS is prepared at a temperature of 1050℃, and the aging treatment at 450℃ has little effect on it. This shows that when working in a medium temperature environment, the interface of the V / HMS sample is relatively stable, so V can be selected as the barrier layer of the HMS thermoelectric material.
[0079] Figure 8 The XRD pattern of the Mo / InSb interface of n-InSb, the SEM characterization pattern and the elemental surface scan of the Mo / InSb interface, among which (a) is the XRD pattern of the Mo / InSb interface of n-InSb, (b) is the SEM characterization pattern of the Mo / InSb interface, and (c) to (f) are the elemental surface scans of the Mo / InSb interface. Figure 8 It can be seen that the first layer of diffraction peaks in (a) is the diffraction spectrum of Mo, which matches the Mo standard card, and the second and third layers are consistent with the standard card spectrum of InSb, indicating that during the sintering process, no reaction occurs between Mo and InSb (the sintered samples are ground and measured layer by layer); there is a relatively obvious stratification at the interface in (b) to (f), and no element reaction and diffusion occur, which is consistent with the XRD results, and the EDS surface scan results also show that the elements on both sides are evenly distributed, the interface is well bonded, and no cracks are found, indicating that its mechanical properties are good.
[0080] Fig. 9 The SEM characterization images and elemental surface scans of the Mo / InSb interface after aging treatment of n-InSb for 1, 2, 4, and 7 days, where (a) is 1 day, (b) is 2 days, (c) is 4 days, and (d) is 7 days. Fig. 9 It can be seen that after 7 days of aging treatment, there are no cracks or holes at the interface, showing good mechanical properties. Even after 7 days of aging treatment, no obvious elemental reaction occurs between Mo and InSb.
[0081] Fig.10 The Mo / InSb interface contact resistivity of n-InSb varies with aging time. Fig.10 It can be seen that after 7 days of aging treatment, the interface contact resistivity is 21.05μΩcm 2 , the change is small (17.4%), and is lower than the standard value of the device, indicating that the interface is relatively stable when working in a high temperature environment.
[0082] Fig.11 The graph of the thermoelectric conversion efficiency of the π-type p-HMS / n-InSb medium-temperature thermoelectric device as a function of height and the ratio of the p and n cross-sectional areas (a), the simulated temperature field distribution (b), the maximum conversion efficiency and maximum output power of the device (c), and the power density as a function of temperature (d). Fig.11 It can be seen from (a) that when the size of p-type HMS is 2.5mm×2.5mm×6.0mm and the size of n-type InSb is 2.8mm×2.5mm×6.0mm, the single pair of devices can achieve a maximum conversion efficiency of 3.75%; (c) shows that at a temperature difference of 420K, the maximum output power of the device is 106.9mW, the maximum conversion efficiency is 3.75%, and the power density is 0.81W / cm 2 .
[0083] Fig.12 The curves of voltage, output power, conversion efficiency with current, maximum conversion efficiency, maximum output power, power density, and device internal resistance with temperature difference of π-type p-HMS / n-InSb medium-temperature thermoelectric device are shown in Figure 1. (a) is the curve of device voltage with current, (b) is the curve of device output power with current, (c) is the curve of device conversion efficiency with current, (d) is the curve of maximum conversion efficiency and maximum output power with temperature difference, (e) is the curve of power density with temperature difference, and (f) is the curve of device internal resistance with temperature difference. Fig.12It can be seen that in (a) to (c), the open circuit voltage, output power and thermoelectric conversion efficiency of the π-type p-HMS / n-InSb medium-temperature thermoelectric device increase with the increase of the temperature difference between the two ends of the device. h When the temperature is 450℃ and the temperature difference ΔT is 420K, the open circuit voltage is 120.4mV, the internal resistance is 82.5mΩ, and the maximum output power and maximum conversion efficiency of the device are 43.9mW and 1.56%, respectively; in (d) to (f), the bottom area of the π-type p-HMS / n-InSb medium-temperature thermoelectric device is 13.25mm 2 , the power density of the device can be calculated. When the temperature difference ΔT is 420K, its power density reaches 0.33W / cm 2 As the test temperature increases, the internal resistance of the device remains in the range of 80.5 to 87.8 mΩ, and the change is relatively stable.
[0084] Fig.13 For n-type Mg 2 Performance curves of segmented thermoelectric devices with Si and p-type high manganese silicide (HMS) as high temperature segments and n-type and p-type Bi-Te as low temperature segments, where (a) is the output power variation curve of two pairs of segmented thermoelectric devices with load current under different temperature differences, and (b) is the maximum conversion efficiency variation of two pairs of segmented thermoelectric devices with temperature; Fig.14 p-HMS / n-InSb medium-temperature thermoelectric devices and commercial Bi 2 Te 3 The devices are assembled in series and parallel to obtain p-HMS / n-InSb / commercial Bi 2 Te 3 Performance curve of the double-layer thermoelectric device based on the PCB, where (a) is the maximum output power and (b) is the maximum conversion efficiency curve with temperature. Figures 13-14 It can be seen that with n-type Mg 2 The segmented thermoelectric device with Si and p-type high manganese silicide (HMS) as the high temperature segment and n-type and p-type Bi-Te as the low temperature segment has a load current of 3.4A, a resistance of 41mΩ and a maximum output power of 0.48W at a temperature of 498°C. The p-HMS / n-InSb medium-temperature thermoelectric device prepared by the present invention is compared with the commercial Bi 2 Te 3 The devices are assembled in series and parallel to obtain p-HMS / n-InSb / commercial Bi 2 Te 3 When the temperature difference is 420K, the maximum output power of the double-layer thermoelectric device is 2.68W, which is much greater than 0.48W.
[0085] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.
Claims
1. A π-type p-HMS / n-InSb medium-temperature thermoelectric device, characterized in that: The π-type p-HMS / n-InSb medium-temperature thermoelectric device is composed of a p-type HMS thermoelectric single arm and an n-type InSb thermoelectric single arm welded together; The p-type HMS thermoelectric single arm uses Mn powder and Si powder as thermoelectric materials and V as a barrier layer raw material; The n-type InSb thermoelectric single arm uses InSb as the thermoelectric material and Mo as the barrier layer.
2. The π-type p-HMS / n-InSb medium-temperature thermoelectric device according to claim 1, characterized in that: The molar ratio of the Mn powder to the Si powder is 1:1.68-1.
80.
3. A method for preparing a π-type p-HMS / n-InSb medium-temperature thermoelectric device as claimed in claim 1 or 2, characterized in that the steps include: The Mn powder and the Si powder are mixed, ball-milled and dried to obtain the HMS-based precursor powder; The HMS-based precursor powder is used as the thermoelectric material, and the V powder is used as the barrier layer raw material. After assembling according to the barrier layer-thermoelectric material-barrier layer structure, the p-type HMS thermoelectric single arm is obtained by sintering. In particles and Sb particles are used as reaction raw materials, and InSb powder is obtained through calcination, quenching and grinding; The InSb powder is used as the thermoelectric material, the Mo powder is used as the barrier layer, and the structure of barrier layer-thermoelectric material-barrier layer is assembled, and then sintered to obtain an n-type InSb thermoelectric single arm; The p-type HMS thermoelectric single arm and the n-type InSb thermoelectric single arm are welded on a substrate to form a pn pair, thereby obtaining the π-type p-HMS / n-InSb medium-temperature thermoelectric device.
4. The preparation method according to claim 3, characterized in that: The ball milling is a wet ball milling, with a ball-to-material ratio of 20:1, a rotation speed of 350 rpm, a time of 1 to 4 hours, and a solvent of n-hexane; the drying temperature is 55° C., and the drying time is 12 hours.
5. The preparation method according to claim 3, characterized in that: The p-type HMS thermoelectric single arm is obtained by sintering by spark plasma sintering under vacuum conditions.
6. The preparation method according to claim 5, characterized in that: The vacuum condition is 1.0×10 -4 ~1.0×10 - 3 Pa; the spark plasma sintering pressure is 40 to 80 MPa, the temperature is 950 to 1100°C, the heating rate is 50°C / min, and the time is 5 to 20 min.
7. The preparation method according to claim 3, characterized in that: The calcination is carried out under vacuum conditions not exceeding 4×10 - 3 Pa, and then heated to 800 °C at a heating rate of 60 K / h and kept at that temperature for 6 h.
8. The preparation method according to claim 3, characterized in that: The n-type InSb thermoelectric single arm is obtained by sintering by SPS under vacuum conditions.
9. The preparation method according to claim 8, characterized in that: The vacuum condition is 1.0×10 -4 ~1.0×10 - 3 The SPS sintering pressure is 40-80MPa, the temperature is 450°C, the heating rate is 50°C / min, and the holding time is 10min.
10. Use of the π-type p-HMS / n-InSb medium-temperature thermoelectric device according to claim 1 or 2 in medium-temperature waste heat recovery.
Citation Information
Cited By
Packaging structure of bismuth telluride thermoelectric device and preparation method thereof
CN119522016A
Packaging structure of bismuth telluride thermoelectric device and preparation method thereof
CN119522016B