Piezoelectric composite material, preparation method thereof and ultrasonic transducer
By adding mica powder, glass microbeads and boron nitride to the passive phase, and using specific process methods, the problem of poor thermal stability of type 1-3 piezoelectric composites is solved, and the high temperature resistance is improved and The yield rate ensures the stable output and service life of the ultrasonic transducer.
Patent Information
- Application Number
- CN202310503752.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-06
- Publication Date
- 2024-11-08
AI Technical Summary
The thermal stability of the 1-3 type piezoelectric composite material is poor, resulting in the problems of degradation of mechanical properties, weakening of bonding strength and insufficient thermal conductivity in high-strength focused ultrasonic transducers, especially when the high-power continuous operation is performed. .
Add fillers such as mica powder, glass microbeads and boron nitride to the passive phase, and use specific process methods, such as constant temperature treatment and molding treatment, to prepare piezoelectric composite materials with improved high temperature resistance.
It improves the high temperature resistance of piezoelectric composite materials, reduces the risk of cracking and deformation, enhances the yield and scope of application, and ensures the stable output and service life of ultrasonic transducers under high temperature conditions.
Smart Images

Figure CN118922053A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of material technology, and in particular to a piezoelectric composite material, a preparation method thereof and an ultrasonic transducer. Background Art
[0002] Ultrasound therapy is a treatment method for certain diseases that utilizes the mechanical, cavitation, and thermal effects of ultrasound. High-intensity focused ultrasound (HIFU) is a minimally invasive technology that can treat deep and superficial tumors in the body, especially in the treatment of various benign and malignant solid tumors such as uterine fibroids, liver cancer, and pancreatic cancer. Usually, high-intensity focused ultrasound therapy technology uses a high-power ultrasonic transducer with a special focusable geometry as the core component of the treatment device. This transducer is a functional device based on the inverse piezoelectric effect that realizes the mutual conversion of electrical energy and acoustic energy.
[0003] Piezoelectric composite materials refer to materials with piezoelectric effect that are composed of at least one piezoelectric phase material and a non-piezoelectric phase material in a specific connection mode. They are the key core materials of ultrasonic transducers. According to the connectivity of each phase material (i.e., the self-connection mode of each phase material in spatial distribution), two-phase piezoelectric composite materials can be divided into 0-0, 0-1, 0-2, 0-3, 1-1, 1-2, 1-3 and other types. Usually, the first number represents the piezoelectric phase and the second number represents the non-piezoelectric phase.
[0004] Among them, 1-3 piezoelectric composite materials are the key core materials of the new generation of ultrasonic transducers. They have the advantages of low acoustic impedance and high electromechanical coupling coefficient. They are important materials for transducers in hydrophones, medical imaging, non-destructive testing, etc. 1-3 piezoelectric composite ceramics are made of piezoelectric ceramics and polymers. The piezoelectric effect of piezoelectric ceramics produces deformation to form ultrasonic waves. Therefore, piezoelectric ceramics are called active phases and polymers are called passive phases.
[0005] However, high molecular polymers have a low softening point, large thermal expansion and poor thermal diffusion, which means that there is a risk of mismatch in thermal and mechanical properties between the piezoelectric ceramic phase and the high molecular polymer in type 1-3 piezoelectric composites. In particular, focused ultrasonic transducers require the 1-3 piezoelectric composites to be prepared into a spherical or curved surface, and the complex processing technology results in a low yield. Ultrasonic transducers will generate a large amount of heat when working continuously at high power. This heat will cause the high molecular polymer of the passive phase material to soften, reduce mechanical properties, and weaken bonding strength, ultimately affecting the normal output and service life of the transducer. The passive phase has weak thermal conductivity, and this defect is prominent when the temperature of the transducer rises during operation. Summary of the invention
[0006] In view of this, the present invention provides a piezoelectric composite material, a preparation method thereof and an ultrasonic transducer, which are used to solve the technical problem of poor thermal stability of the existing 1-3 type piezoelectric composite materials.
[0007] In an exemplary embodiment of the present invention, the present invention provides a piezoelectric composite material, which is composed of an active phase and a passive phase, the passive phase includes epoxy resin, filler and curing agent, and the filler includes at least one of mica powder, glass beads and boron nitride.
[0008] In an exemplary embodiment of the present invention, the active phase comprises a piezoelectric ceramic.
[0009] In an exemplary embodiment of the present invention, the epoxy resin includes bisphenol A type epoxy resin.
[0010] In an exemplary embodiment of the present invention, in the passive phase, the filler accounts for 0.02wt%-40wt%, preferably 0.02wt%-35wt%.
[0011] In an exemplary embodiment of the present invention, the curing agent includes an amine curing agent.
[0012] In an exemplary embodiment of the present invention, in the passive phase, the mass ratio of the curing agent to the epoxy resin is 1-3:5, preferably 1.5-3:5.
[0013] In an exemplary embodiment of the present invention, the volume ratio of the active phase to the epoxy resin is 30-80:100, preferably 30-65:100.
[0014] In an exemplary embodiment of the present invention, the filler includes mica powder, glass microspheres and boron nitride.
[0015] In an exemplary embodiment of the present invention, the mass ratio of mica powder, glass microspheres and boron nitride is 10-15:5-10:5-15, preferably 10-12:8-10:5-12.
[0016] In an exemplary embodiment of the present invention, the passive phase further includes an additive, and the additive includes at least one of a toughening agent and a coupling agent.
[0017] In an exemplary embodiment of the present invention, the toughening agent includes a polymer containing a hydroxyl group, an ester group, and an ether group.
[0018] In an exemplary embodiment of the present invention, the coupling agent includes a silane coupling agent.
[0019] In an exemplary embodiment of the present invention, in the passive phase, the additive accounts for 0.02wt%-13wt%, preferably 0.05wt%-12wt%.
[0020] In addition, the inventors have also discovered that the piezoelectric composite materials prepared by the existing process are prone to cracking and deformation.
[0021] In order to solve the technical problem that the piezoelectric composite material is prone to cracking and deformation when prepared by the existing process, in an exemplary embodiment of the present invention, the present invention also provides a method for preparing the piezoelectric composite material as described above, the preparation method comprising:
[0022] After the active phase is cut, cleaned, dried, and placed in a caulking mold;
[0023] Add filler to epoxy resin, stir evenly, then add curing agent to obtain a mixture, pour the mixture into the caulking mold, fill the gap, degas, and then place it in an oven for constant temperature treatment. After the surface of the mixture is cured, it is processed to a preset thickness, heated again until the mixture is completely softened, and then placed in a molding mold and taken out after it is completely cured.
[0024] In an exemplary embodiment of the present invention, the constant temperature treatment includes: first constant temperature treatment at 35±5°C for 2-4h, then constant temperature treatment at 40±5°C for 1-2h, preferably, first constant temperature treatment at 35±3°C for 2.5-4h, then constant temperature treatment at 40±3°C for 1.5-2h.
[0025] In an exemplary embodiment of the present invention, the heating is performed to 60±5°C, preferably 60±3°C.
[0026] In an exemplary embodiment of the present invention, the present invention further provides an ultrasonic transducer, wherein the ultrasonic transducer comprises the piezoelectric composite material as described above or the piezoelectric composite material prepared according to the preparation method as described above.
[0027] As described above, the piezoelectric composite material, the preparation method thereof and the ultrasonic transducer of the present invention have the following beneficial effects:
[0028] The invention can improve the high temperature resistance of the piezoelectric composite material by adding a specific filler into the passive phase.
[0029] The piezoelectric composite material of the present invention can be die-cast into various shapes as the tooling changes, has a high yield rate and a wide range of applications.
[0030] The present invention further solves the technical problem that piezoelectric composite materials are prone to cracking and deformation when prepared using existing processes. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 This is the cutting flow chart of piezoelectric ceramics;
[0032] Figure 2 The graph is a trend diagram of the electromechanical coupling coefficient of the piezoelectric composite materials prepared in Examples 1-4 and Comparative Example 1 as a function of temperature. DETAILED DESCRIPTION
[0033] The present invention is further described below through specific examples, but it should be pointed out that the specific material ratios, process conditions and results described in the embodiments of the present invention are only used to illustrate the present invention and cannot be used to limit the scope of protection of the present invention. All equivalent changes or modifications made according to the spirit of the present invention should be included in the scope of protection of the present invention.
[0034] The present invention provides a piezoelectric composite material, which is composed of an active phase and a passive phase, wherein the passive phase includes epoxy resin, filler and curing agent;
[0035] The volume ratio of the active phase to the epoxy resin is 30-80:100, and the active phase includes piezoelectric ceramics;
[0036] In the passive phase, the filler accounts for 0.02wt%-40wt%, and the additive accounts for 0.02wt%-13wt%;
[0037] In the passive phase, the mass ratio of the curing agent to the epoxy resin is 1-3:5, and the curing agent includes an amine curing agent;
[0038] Epoxy resins include bisphenol A epoxy resins;
[0039] The filler includes at least one of mica powder, glass microspheres and boron nitride.
[0040] In an exemplary embodiment of the present invention, the filler includes mica powder, glass microspheres and boron nitride, and the mass ratio of mica powder, glass microspheres and boron nitride is 10-15:5-10:5-15.
[0041] In an exemplary embodiment of the present invention, the passive phase further includes an additive, the additive includes at least one of a toughening agent and a coupling agent, the toughening agent includes a polymer containing a hydroxyl group, an ester group, and an ether group, and the coupling agent includes a silane coupling agent.
[0042] In an exemplary embodiment of the present invention, the present invention also provides a method for preparing the piezoelectric composite material as described above, comprising:
[0043] After the active phase is cut, cleaned, dried, and placed in a caulking mold;
[0044] Adding filler to epoxy resin, stirring evenly, and then adding curing agent to obtain a mixture;
[0045] Pour the mixture into the caulking mold, fill the gap, degas, and then place it in an oven for constant temperature treatment at 35±5℃ for 2-4h, then at 40±5℃ for 1-2h. After the surface of the mixture is cured, process it to the preset thickness, heat it to 60±5℃ again to soften the mixture completely, then place it in the molding mold and take it out after it is completely cured.
[0046] In an exemplary embodiment of the present invention, the present invention further provides an ultrasonic transducer, wherein the ultrasonic transducer comprises the piezoelectric composite material as described above or the piezoelectric composite material prepared according to the preparation method as described above.
[0047] The scheme of the present invention is illustrated by specific embodiments below. It should also be understood that the following embodiments are only used to specifically illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the above content of the present invention belong to the scope of protection of the present invention. The specific process parameters and the like in the following examples are also only examples within a suitable range, that is, those skilled in the art can make a selection within a suitable range through the description herein, and are not limited to the specific values exemplified below.
[0048] Example 1
[0049] This embodiment provides a piezoelectric composite material, which is prepared by the following steps:
[0050] S1. Figure 1 As shown, the piezoelectric ceramic PZT-8 (as shown in FIG. a) is fixed and cut one by one. After cutting one side, the piezoelectric ceramic PZT-8 is rotated 90° and the other side is cut. Then, it is cleaned and dried, and then placed in a caulking mold.
[0051] S2. 15g of mica powder was added to 70.83g of bisphenol A epoxy resin E-51, stirred, and then 14.17g593 modified fatty amine curing agent was added to obtain a mixture;
[0052] Among them, the volume ratio of piezoelectric ceramic PZT-8 and bisphenol A epoxy resin E-51 is 60:100;
[0053] S3. Pour the mixture into the caulking mold in which the piezoelectric ceramic PZT-8 has been placed in step S1, fill the gap, vacuum degas for 10 minutes, and then place it in an oven, first treat it at a constant temperature of 35°C for 2 hours, and then treat it at a constant temperature of 40°C for 2 hours. After the surface of the mixture is solidified, it is processed to a thickness of 2mm, and heated to 60°C again to completely soften the mixture. Then, it is placed in a molding mold with a curvature radius of 170mm, and taken out after it is completely solidified to obtain a piezoelectric composite material.
[0054] The piezoelectric composite material prepared in this embodiment did not show cracking, deformation and the like.
[0055] Example 2
[0056] This embodiment provides a piezoelectric composite material, which is prepared by the following steps:
[0057] S1. Figure 1 As shown, the piezoelectric ceramic PZT-4 is fixed and one side is cut as a whole (as shown in FIG. b). After completion, the piezoelectric ceramic PZT-4 is rotated 90° and the other side is cut (as shown in FIG. c). Then, it is cleaned and dried, and then placed in a caulking mold.
[0058] S2. 15 g of glass beads were added to 70.83 g of bisphenol A epoxy resin E-51 and stirred, followed by addition of 14.17 g of 593 modified fatty amine curing agent to obtain a mixture;
[0059] Among them, the volume ratio of piezoelectric ceramic PZT-4 and bisphenol A epoxy resin E-51 is 50:100;
[0060] S3. Pour the mixture into the caulking mold in which the piezoelectric ceramic PZT-4 has been placed in step S1, fill the gap, vacuum degas for 10 minutes, and then place it in an oven, first treat it at a constant temperature of 35°C for 2 hours, and then treat it at a constant temperature of 40°C for 2 hours. After the surface of the mixture is solidified, it is processed to a thickness of 3mm, and heated to 60°C again to completely soften the mixture. Then, it is placed in a molding mold with a curvature radius of 140mm, and taken out after it is completely solidified to obtain a piezoelectric composite material.
[0061] Example 3
[0062] This embodiment provides a piezoelectric composite material, which is prepared by the following steps:
[0063] S1. Figure 1 As shown, the piezoelectric ceramic PZT-8 (as shown in FIG. a) is fixed and cut one by one. After cutting one side, the piezoelectric ceramic PZT-8 is rotated 90° and the other side is cut. Then, it is cleaned and dried, and then placed in a caulking mold.
[0064] S2. 15 g of boron nitride was added to 70.83 g of bisphenol A epoxy resin E-51, stirred, and then 14.17 g of 593 modified fatty amine curing agent was added to obtain a mixture;
[0065] Among them, the volume ratio of piezoelectric ceramic PZT-8 and bisphenol A epoxy resin E-51 is 30:100;
[0066] S3. Pour the mixture into the caulking mold in which the piezoelectric ceramic PZT-8 has been placed in step S1, fill the gap, degas in vacuum for 10 minutes, and then place it in an oven, first treat it at a constant temperature of 35°C for 4 hours, and then treat it at a constant temperature of 40°C for 2 hours. After the surface of the mixture is solidified, it is processed to a thickness of 2 mm, and heated to 60°C again to completely soften the mixture. Then it is bent and completely applied to a cylindrical tooling with a diameter of 10 mm. After it is completely solidified, it is taken out to obtain a piezoelectric composite material.
[0067] Example 4
[0068] The difference between this embodiment and embodiment 1 is that:
[0069] S2. 5g of mica powder, 5g of glass beads and 5g of boron nitride were added to 70.83g of bisphenol A epoxy resin E-51, stirred, then added 593 modified fatty amine, stirred, and then added 14.17g 593 modified fatty amine curing agent to obtain a mixture;
[0070] The volume ratio of the piezoelectric ceramic PZT-8 to the bisphenol A epoxy resin E-51 is 60:100.
[0071] Example 5
[0072] The difference between this embodiment and embodiment 1 is that:
[0073] S2. 9g of mica powder, 3g of glass beads and 3g of boron nitride were added to 70.83g of bisphenol A epoxy resin E-51 and stirred, followed by addition of 14.17g of 593 modified fatty amine curing agent to obtain a mixture;
[0074] The volume ratio of the piezoelectric ceramic PZT-8 to the bisphenol A epoxy resin E-51 is 60:100.
[0075] Example 6
[0076] The difference between this embodiment and embodiment 1 is that:
[0077] S2. 15g of mica powder, 5g of VL-1 toughening agent and 1g of γ-aminopropyl triethoxysilane were added to 64.83g of bisphenol A epoxy resin E-51 and stirred, followed by addition of 14.17g of 593 modified fatty amine curing agent to obtain a mixture;
[0078] The volume ratio of the piezoelectric ceramic PZT-8 to the bisphenol A epoxy resin E-51 is 60:100.
[0079] Comparative Example 1
[0080] The difference between this comparative example and Example 1 is that:
[0081] S2 was added 14.17g 593 modified fatty amine curing agent to 70.83g bisphenol A epoxy resin E-51 to obtain a mixture;
[0082] The volume ratio of the piezoelectric ceramic PZT-8 to the bisphenol A epoxy resin E-51 is 60:100.
[0083] Performance Testing
[0084] The high temperature resistance of the piezoelectric composite materials obtained in Examples 1-4 and Comparative Example 1 is tested. The specific steps are: directly reading the resonant frequency f of the piezoelectric composite materials obtained in Examples 1-4 and Comparative Example 1 on an impedance analyzer at 20°C, 25°C, 30°C, 35°C, 40°C, 45°C, and 50°C, respectively. r and the anti-resonance frequency f a Then, the electromechanical coupling coefficient k of the piezoelectric composite materials prepared in Examples 1-4 and Comparative Example 1 at the corresponding temperature is calculated according to formula (I): t :
[0085]
[0086] Among them, k t is the electromechanical coupling coefficient; f r is the resonant frequency in KHz, f a is the anti-resonance frequency in KHz. The results are shown in Table 1 and Figure 2 shown.
[0087] Table 1 Test results
[0088]
[0089] As shown in Table 1, as the temperature increases, the change trend of the electromechanical coupling coefficient of the piezoelectric composite material of Comparative Example 1 (without adding filler) is relatively steep, and the change trend of the electromechanical coupling coefficient of the piezoelectric composite material of Example 1 (adding filler) is relatively gentle. This result shows that the addition of specific fillers in the passive phase of the present invention can improve the high temperature stability of the piezoelectric composite material.
[0090] From Table 1 and Figure 2It can be seen that compared with the piezoelectric composite materials of Examples 1, 2 and 3 (fillers are one of mica powder, glass beads and boron nitride), as the temperature increases, the electromechanical coupling coefficient of the piezoelectric composite material of Example 4 (fillers are composed of mica powder, glass beads and boron nitride in a mass ratio of 10:10:10) remains relatively stable. This result shows that the present invention can further improve the high temperature stability of the piezoelectric composite material by selecting the filler composition (including mica powder, glass beads and boron nitride, the mass ratio of mica powder, glass beads and boron nitride is 10-15:5-10:5-15).
[0091] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.
Claims
1. A piezoelectric composite material, It is characterized in that The piezoelectric composite material consists of an active phase and a passive phase. The passive phase includes epoxy resin, filler and curing agent. The filler includes at least one of mica powder, glass microbeads and boron nitride.
2. The piezoelectric composite material according to claim 1, It is characterized in that The active phase includes piezoelectric ceramics; and / or, the volume ratio of the active phase to the epoxy resin is 30-80:100; And / or, the epoxy resin comprises bisphenol A epoxy resin; And / or, in the passive phase, the filler accounts for 0.02wt%-40wt%; and / or, the curing agent comprises an amine curing agent; And / or, in the passive phase, the mass ratio of the curing agent to the epoxy resin is 1-3:
5.
3. The piezoelectric composite material according to claim 1, It is characterized in that The filler includes mica powder, glass microspheres and boron nitride.
4. The piezoelectric composite material according to claim 3, It is characterized in that The mass ratio of the mica powder, the glass microbeads and the boron nitride is 10-15:5-10:5-15.
5. The piezoelectric composite material according to claim 1, It is characterized in that The passive phase further includes an additive, wherein the additive includes at least one of a toughening agent and a coupling agent.
6. The piezoelectric composite material according to claim 5, It is characterized in that The toughening agent includes a polymer containing a hydroxyl group, an ester group and an ether group; And / or, the coupling agent includes a silane coupling agent.
7. The piezoelectric composite material according to claim 5, It is characterized in that In the passive phase, the additive accounts for 0.02wt%-13wt%.
8. A method for preparing the piezoelectric composite material according to any one of claims 1 to 7, It is characterized in that The preparation method comprises: After the active phase is cut, cleaned, dried, and placed in a caulking mold; Add filler to epoxy resin, stir evenly, then add curing agent to obtain a mixture, pour the mixture into the caulking mold, fill the gap, degas, and then place it in an oven for constant temperature treatment. After the surface of the mixture is cured, it is processed to a preset thickness, heated again until the mixture is completely softened, and then placed in a molding mold and taken out after it is completely cured.
9. The preparation method according to claim 8, It is characterized in that The constant temperature treatment includes: firstly, constant temperature treatment at 35±5°C for 2-4h, and then constant temperature treatment at 40±5°C for 1-2h; and / or, heated to 60±5°C.