Laminate, method for producing laminate, and adhesive composition

By grafting modification in polyolefins to form a carbodiimide-based polymer, combined with coextrusion molding process, the problem of insufficient bonding strength between polyolefins and polar resins at low temperatures is solved, and polyterephthalene is achieved The high bonding strength of ethylene glycol formate and biodegradable polymer layer improves the overall performance of the material.

CN118922307APending Publication Date: 2024-11-08MITSUI CHEMICALS INC
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202380029446.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-25
Filing Date
2023-03-24
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing polyolefins have poor adhesive properties with polar resins, especially inadequate bonding strength at low temperatures, and the heat resistance and adhesion of biodegradable polymers are defective, making it difficult to meet the application needs at high temperatures.

Method used

The polyolefin matrix polymer with graft-modified carbodiimide monomer containing a carbodiimide group and a polymerizable double bond is formed to form an adhesive composition with excellent bonding strength, and is then coextruded and layered. The laminate is made by press forming and other processes to ensure firm bonding between the layers.

Benefits of technology

It realizes firm bonding with the resin layer containing polar groups at low temperature, especially the high bonding strength of polyethylene terephthalate and biodegradable polymer layer, avoids thermal degradation problems and improves The overall performance of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005054493440000021
    Figure BDA0005054493440000021
  • Figure BDA0005054493440000031
    Figure BDA0005054493440000031
  • Figure BDA0005054493440000041
    Figure BDA0005054493440000041
Patent Text Reader

Abstract

One embodiment of the present invention relates to a laminate, a method for producing the laminate, or an adhesive composition. The laminate comprises: a layer (A) containing polyethylene terephthalate or a biodegradable polymer; and an adhesive layer (B) containing an adhesive composition, at least a portion of the adhesive layer (B) being in contact with the layer (A), the adhesive composition containing a graft-modified body obtained by graft-modifying at least one type of matrix polymer selected from polyolefins with a carbodiimide monomer having a carbodiimide group and a polymerizable double bond, the adhesive composition contains 0.1 to 50 mmol of carbodiimide groups per 100 g of the adhesive composition, and the density of the adhesive composition is 0.870 to 0.940 g / cm < 3 >.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] One embodiment of the present invention relates to a laminate, a method for producing a laminate, and an adhesive composition. Background Art

[0002] Polyolefins such as polyethylene and polypropylene have excellent mechanical strength, rigidity, heat resistance, chemical resistance, oil resistance, transparency, and impact resistance at low temperatures. Taking advantage of these characteristics, they are widely used as packaging materials such as films, sheets, and bottles, and covering materials or decorative materials such as wallpaper.

[0003] However, polyolefins do not contain polar groups in their molecules and therefore have poor adhesion to polar resins such as polyesters, and their applications in lamination with these materials are limited.

[0004] In order to solve such problems, a method of grafting a polar group-containing monomer onto polyolefin to improve the compatibility and adhesion is widely used. For example, a method of grafting glycidyl (meth)acrylate onto polyolefin is widely used (for example, Patent Document 1).

[0005] In addition, in recent years, due to environmental considerations, attention has been focused on technologies that replace petroleum raw materials such as petroleum-derived resins with biodegradable polymers that have a lower environmental load. However, compared with petroleum-derived resins, biodegradable polymers generally have the disadvantages of being inferior in various physical properties such as heat resistance and having low bonding strength with existing adhesive resin compositions.

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent Document 1: Japanese Patent Application Laid-Open No. 6-145260 Summary of the invention

[0009] Technical problem to be solved by the invention

[0010] The modified polyolefin obtained by the method described in Patent Document 1 can improve the above-mentioned adhesiveness to a certain extent, but the adhesiveness is still insufficient, especially the adhesive strength is insufficient. In order to exhibit sufficient adhesive strength, a relatively high temperature is required.

[0011] One embodiment of the present invention provides an adhesive composition that can be firmly bonded to a layer containing polyethylene terephthalate or a biodegradable polymer as a resin having a polar group even at low temperatures, a laminate having excellent bonding strength using the adhesive composition, and a method for producing the same.

[0012] Technical solutions for solving technical problems

[0013] The configuration examples of the present invention are as follows.

[0014] [1] A laminate comprising: a layer (A) containing polyethylene terephthalate or a biodegradable polymer; and an adhesive layer (B) containing an adhesive composition,

[0015] At least a portion of the adhesive layer (B) is in contact with the layer (A),

[0016] The above adhesive composition satisfies the following requirements (i) to (iii):

[0017] (i) a graft-modified product obtained by graft-modifying at least one base polymer selected from polyolefins with a carbodiimide monomer having a carbodiimide group and a polymerizable double bond;

[0018] (ii) containing 0.1 to 50 mmol of carbodiimide groups per 100 g of the adhesive composition;

[0019] (iii) Density: 0.870 to 0.940 g / cm 3 .

[0020] [2] The laminate according to [1], wherein the carbodiimide monomer is at least one monomer selected from the group consisting of a compound represented by the following formula (1) and a compound represented by the following formula (2),

[0021]

[0022] In formula (1), R1 is a hydrogen atom or a methyl group, R2 is an alkyl group or an aryl group which may have a substituent, and in formula (2), R3 is a hydrogen atom or a methyl group, R4 is an alkyl group or an aryl group which may have a substituent, and m is an integer greater than 2.

[0023] [3] The laminate according to [1] or [2], wherein the layer (A) is made of polyethylene terephthalate.

[0024] [4] The laminate according to [1] or [2], wherein the layer (A) contains polylactic acid.

[0025] [5] The laminate according to [1] or [2], wherein the layer (A) is composed of a biodegradable polymer.

[0026] [6] The laminate according to [1] or [2], wherein the layer (A) is composed of polylactic acid.

[0027] [7] The laminate according to any one of [1] to [6], wherein the laminate is obtained by lamination molding, co-extrusion molding, blow molding or co-injection molding.

[0028] [8] A method for producing a laminate, wherein the laminate comprises: a layer (A) containing polyethylene terephthalate or a biodegradable polymer; and an adhesive layer (B) containing an adhesive composition, at least a portion of the adhesive layer (B) being in contact with the layer (A);

[0029] The manufacturing method comprises step 1 of co-extrusion molding, lamination molding, blow molding or co-injection molding of a resin composition containing polyethylene terephthalate or a biodegradable polymer and the adhesive composition.

[0030] The above adhesive composition satisfies the following requirements (i) to (iii):

[0031] (i) a graft-modified product obtained by graft-modifying at least one base polymer selected from polyolefins with a carbodiimide monomer having a carbodiimide group and a polymerizable double bond;

[0032] (ii) containing 0.1 to 50 mmol of carbodiimide groups per 100 g of the adhesive composition;

[0033] (iii) Density: 0.870 to 0.940 g / cm 3 .

[0034] [9] The method for producing a laminate according to [8], wherein, when the layer (A) is a layer containing a biodegradable polymer, the step 1 is performed at a temperature lower than the thermal degradation temperature of the biodegradable polymer.

[0035]

[10] The method for producing a laminate according to [8] or [9], wherein the carbodiimide monomer is at least one monomer selected from the group consisting of a compound represented by the following formula (1) and a compound represented by the following formula (2),

[0036]

[0037] In formula (1), R1 is a hydrogen atom or a methyl group, R2 is an alkyl group or an aryl group which may have a substituent, and in formula (2), R3 is a hydrogen atom or a methyl group, R4 is an alkyl group or an aryl group which may have a substituent, and m is an integer greater than 2.

[0038]

[11] An adhesive composition that satisfies the following requirements (i) to (iii):

[0039] (i) a graft-modified product obtained by graft-modifying at least one base polymer selected from polyolefins with a carbodiimide monomer having a carbodiimide group and a polymerizable double bond;

[0040] (ii) containing 0.1 to 50 mmol of carbodiimide groups per 100 g of the adhesive composition;

[0041] (iii) Density: 0.870 to 0.940 g / cm 3 .

[0042]

[12] The adhesive composition according to

[11] , wherein the carbodiimide monomer is at least one monomer selected from the group consisting of a compound represented by the following formula (1) and a compound represented by the following formula (2),

[0043]

[0044] In formula (1), R1 is a hydrogen atom or a methyl group, R2 is an alkyl group or an aryl group which may have a substituent, and in formula (2), R3 is a hydrogen atom or a methyl group, R4 is an alkyl group or an aryl group which may have a substituent, and m is an integer greater than 2.

[0045] Effects of the Invention

[0046] According to one embodiment of the present invention, there can be provided an adhesive composition that can be firmly bonded to a layer containing polyethylene terephthalate as a resin having a polar group even at low temperatures (eg, 230° C.), a laminate having excellent bonding strength using the adhesive composition, and a method for producing the same.

[0047] Furthermore, according to one embodiment of the present invention, there can be provided an adhesive composition that can be firmly bonded to a layer containing a biodegradable polymer even when bonding is performed at a low temperature where the biodegradable polymer does not thermally degrade, a laminate having excellent bonding strength using the adhesive composition, and a method for producing the same. DETAILED DESCRIPTION

[0048] <<Adhesive composition>>

[0049] The adhesive composition according to one embodiment of the present invention (hereinafter also referred to as “the present composition”) satisfies the following requirements (i) to (iii):

[0050] (i) a graft-modified product obtained by graft-modifying at least one base polymer selected from polyolefins with a carbodiimide monomer having a carbodiimide group and a polymerizable double bond (hereinafter also referred to as "the present modified product");

[0051] (ii) containing 0.1 to 50 mmol of carbodiimide groups per 100 g of the composition;

[0052] (iii) Density: 0.870 to 0.940 g / cm 3 .

[0053] The amount of the carbodiimide group in the present composition is 0.1 to 50 mmol, preferably 0.2 to 20 mmol, more preferably 0.5 to 5 mmol per 100 g of the present composition.

[0054] When the amount of the carbodiimide group is within the above range, the present composition can be easily obtained which can be firmly bonded to an adherend, particularly a layer containing polyethylene terephthalate or a biodegradable polymer even at low temperatures.

[0055] The amount of the carbodiimide groups is specifically measured by the method described in the following Examples.

[0056] The density of the present composition measured according to JIS K 7210 is 0.870 to 0.940 g / cm 3 , preferably 0.880 to 0.925 g / cm 3 , more preferably 0.890 to 0.920 g / cm 3 .

[0057] When the density is within the above range, the present composition can be easily obtained which can be firmly bonded to an adherend, particularly a layer containing polyethylene terephthalate or a biodegradable polymer even at low temperatures.

[0058] The melt flow rate (MFR) of the present composition measured at 190°C and under a load of 2.16 kg in accordance with JIS K 7210 is preferably 0.1 to 10 g / 10 min, more preferably 0.2 to 5 g / 10 min.

[0059] When the MFR is within the above range, a desired laminate can be easily formed by a molding method such as co-extrusion molding, lamination molding, blow molding, and coinjection molding, which is preferred.

[0060] The present composition is not particularly limited as long as it contains the present modified product, and may be composed only of the present modified product.

[0061] Since the present composition contains the present modified product, a layer having high adhesive strength can be formed in a short time with an adherend, particularly a layer containing a biodegradable polymer and a layer having a polar group such as polyester (particularly a layer containing polyethylene terephthalate).

[0062] Since the present modified body has higher reactivity with polar groups present in polyethylene terephthalate and biodegradable polymers than a graft modified body obtained by graft modification with glycidyl (meth)acrylate, the present composition containing the present modified body has significantly excellent adhesion to a layer containing polyethylene terephthalate and a biodegradable polymer.

[0063] Since the present modified product is not a block copolymer or a random copolymer of an olefin monomer such as ethylene or propylene and the above-mentioned carbodiimide monomer but a graft modified product, the present composition can exhibit the above-mentioned effects by using the present modified product.

[0064] The present modified product used in the present composition may be one kind or two or more kinds.

[0065] The content of the present modified body in the present composition is not particularly limited, but is usually 0.5 mass % or more, preferably 1 mass % or more, and usually 60 mass % or less, preferably 50 mass % or less, from the viewpoints of molding processability, controllability of adhesiveness, economy, etc.

[0066] The present composition preferably contains the present modified product described above and one or more olefin-based polymers other than the present modified product.

[0067] As the above-mentioned olefin polymers that can be used in the present composition, there are no particular restrictions as long as they are polymers made of olefins as raw materials, and various known olefin polymers can be used. For example, specific examples include homopolymers or copolymers of α-olefins such as ethylene, propylene, 1-butene, 1-hexene, 4-methyl-1-pentene, and 1-octene (for example, high-pressure low-density polyethylene, linear low-density polyethylene (LLDPE), medium-density polyethylene, high-density polyethylene, polypropylene, poly-1-butene, poly-4-methyl-1-pentene, low-crystalline or amorphous ethylene-propylene random copolymers, ethylene-1-butene random copolymers, propylene-1-butene random copolymers), ethylene-vinyl acetate copolymers (EVA) or saponified products thereof, ethylene-(meth)acrylic acid copolymers or metal salts thereof (ionomers), ethylene-cyclic olefin copolymers, and polymers obtained by grafting and modifying these (co)polymers with polar compounds such as maleic acid and silane compounds.

[0068] Among them, when the present composition contains a certain present modified body, from the viewpoint of being able to easily obtain the present composition with excellent compatibility and better ability to exert the desired effect, the above-mentioned olefin-based polymer is preferably a polymer that is the same as the matrix polymer used for the synthesis of the present modified body.

[0069] The olefin-based polymer may be a polymer using only biomass-derived raw materials as its raw materials (eg olefins), a polymer using only fossil fuel-derived raw materials, or a polymer using both biomass-derived raw materials and fossil fuel-derived raw materials.

[0070] From the viewpoint of reducing environmental load (mainly reducing greenhouse gases), the olefin-based polymer is preferably a polymer obtained using a biomass-derived raw material.

[0071] In this specification, biomass-derived raw materials refer to raw materials formed from any (renewable) natural raw materials of plant or animal origin, including fungi, yeast, algae, and bacteria, and their residues, such as carbon with a carbon content of 1×10 -12 The ratio of about 14 A raw material having a biomass carbon concentration (unit: pMC) of about 100 pMC as measured in accordance with ASTM D6866 and having a C isotope. A biomass-derived raw material can be obtained by, for example, a conventionally known method.

[0072] For a certain polymer, as long as the production conditions of the polymer, such as the polymerization catalyst, polymerization process, and polymerization temperature, are the same, even if the polymer contains a biomass-derived raw material, except for the 1×10 -12 ~1×10 -14 The ratio of about 14 The molecular structure other than the C isotope is equivalent to that of a polymer composed of a raw material derived from fossil fuels. Therefore, it is believed that there is no difference in performance between a polymer containing a raw material derived from biomass and a polymer composed of a raw material derived from fossil fuels.

[0073] When the present composition contains the above-mentioned olefin-based polymer, the content of the olefin-based polymer in the present composition is not particularly limited, but is usually 40% by mass or more, preferably 50% by mass or more, and usually 99.5% by mass or less, preferably 99% by mass or less, from the viewpoints of molding processability, controllability of adhesion ability, economy, etc.

[0074] The present composition may contain various additives other than the present modified product and the above-mentioned olefin-based polymer, as necessary, within the range not impairing the purpose of the present invention.

[0075] Examples of the additive include softeners, stabilizers, fillers, antioxidants, crystal nucleating agents, waxes, tackifiers, mechanical stability imparting agents, leveling agents, wetting agents, film-forming aids, crosslinking agents, preservatives, rust inhibitors, pigments, dispersants, antifreeze agents, defoamers, adhesiveness imparting agents, other thermoplastic polymers, water, and organic solvents. These additives may be used alone or in combination of two or more.

[0076] The additive may be an additive using only biomass-derived raw materials, an additive using only fossil fuel-derived raw materials, or an additive using both biomass-derived raw materials and fossil fuel-derived raw materials.

[0077] The present composition can be used in various known adhesive forms, for example, a water-dispersible adhesive, an organic solvent-based adhesive, or a hot-melt adhesive.

[0078] Examples of the bonding objects of the present composition include metals, glass, wood, paper, cloth, thermoplastic resins such as polyester, polyphenylene sulfide, polyamide, polyacetal, polycarbonate, poly(meth)acrylate, olefin polymers, polystyrene, rubber, modified fluororesins, biomass plastics, biodegradable polymers, and other engineering plastics; and layers containing thermosetting resins or layers consisting of these materials.

[0079] Among them, since the present composition has excellent adhesion to a layer containing a biodegradable polymer and a layer containing polyethylene terephthalate (especially a layer composed of polyethylene terephthalate), it is preferably used as an adhesive for these layers from the viewpoint of better exerting the effects of the present invention.

[0080] <This modified body>

[0081] The modified product is a graft-modified product obtained by graft-modifying at least one base polymer selected from polyolefins with a carbodiimide monomer having a carbodiimide group and a polymerizable double bond. In other words, the modified product is a graft-modified product obtained by graft-modifying at least one base polymer selected from polyolefins with a carbodiimide monomer having a carbodiimide group and a polymerizable double bond. In addition, the modified product can be said to be a graft-modified product comprising at least one base polymer portion selected from polyolefins and a graft portion derived from a carbodiimide monomer having a carbodiimide group and a polymerizable double bond.

[0082] From the viewpoints of the ease of synthesis of the present modified body, the ability to easily obtain the above-mentioned grafted modified body with better adhesion, and the fact that the obtained grafted modified body does not become too hard, the grafting rate in the present modified body is preferably 0.3% by mass or more, more preferably 0.5% by mass or more, and preferably 8% by mass or less, more preferably 5% by mass or less.

[0083] The grafting rate is the mass of the structure derived from the carbodiimide monomer in the grafted modified product, which can be calculated by 1 H-NMR measurement was specifically determined by the method described in the following Examples.

[0084] [Carbodiimide monomer]

[0085] The carbodiimide monomer used for graft modification of the matrix polymer is not particularly limited as long as it is a compound having a carbodiimide group and a polymerizable double bond, but is preferably a compound represented by the following formula (1) or (2) from the viewpoint of better exerting the effects of the present invention.

[0086] The carbodiimide monomers used in graft-modifying the above-mentioned base polymer may be two or more, but are usually one.

[0087] The carbodiimide monomer may be a monomer derived from biomass, a monomer derived from fossil fuels, or a monomer derived from both biomass and fossil fuels.

[0088] From the viewpoint of reducing environmental load (mainly reducing greenhouse gas), the carbodiimide monomer is preferably a monomer derived from biomass or a monomer derived from biomass and fossil fuels.

[0089]

[0090] In the formula (1), R1 is a hydrogen atom or a methyl group, and is preferably a hydrogen atom from the viewpoint of easily obtaining the present modified product having a high grafting rate.

[0091] In formula (1), R2 is an alkyl group or an aryl group which may have a substituent. The alkyl group which may have a substituent may be a chain (may be straight chain or branched) or may contain an alicyclic ring.

[0092] The number of carbon atoms of the alkyl group which may have a substituent is preferably 1 or more, more preferably 3 or more, preferably 20 or less, more preferably 12 or less, and further preferably 8 or less. In addition, the number of carbon atoms of the aryl group which may have a substituent is preferably 5 or more, more preferably 6 or more, preferably 20 or less, more preferably 12 or less, and further preferably 8 or less.

[0093] Examples of the substituent which the alkyl group and the aryl group may have include a halogen atom, a hydrocarbon group having 1 to 8 carbon atoms, an alkoxy group having 1 to 8 carbon atoms, a carboxylate group having 1 to 8 carbon atoms, a sulfonate group having 1 to 8 carbon atoms, a carbonyl group having 1 to 8 carbon atoms, an amide group having 1 to 8 carbon atoms, an amino group having 1 to 8 carbon atoms, a thioether group having 1 to 8 carbon atoms, a phosphate group having 1 to 8 carbon atoms, an alkylsilyl group having 1 to 8 carbon atoms, and an alkoxysilyl group having 1 to 8 carbon atoms.

[0094] Among them, from the viewpoints of solubility and availability of the carbodiimide monomer, and easy purification of the obtained graft modified product, R2 is preferably an aliphatic hydrocarbon group having 4 to 20 carbon atoms including an alicyclic ring, and more preferably an alicyclic hydrocarbon group having 5 to 7 carbon atoms.

[0095] Examples of the alicyclic ring include cyclobutane ring, cyclopentane ring, cyclohexane ring, cycloheptane ring, and these rings having a hydrocarbon group. The alicyclic ring may also be a polycyclic ring such as an adamantyl ring and a methyladamantyl ring.

[0096]

[0097] In formula (2), R3 is a hydrogen atom or a methyl group, and is preferably a methyl group from the viewpoint of easily obtaining the present composition having excellent bonding strength to a substrate having a polar group.

[0098] In formula (2), R4 is an alkyl group or an aryl group which may have a substituent. The alkyl group which may have a substituent may be a chain (may be straight chain or branched) or may contain an alicyclic ring.

[0099] The number of carbon atoms of the alkyl group which may have a substituent is preferably 1 or more, more preferably 3 or more, preferably 20 or less, more preferably 12 or less, and further preferably 8 or less. In addition, the number of carbon atoms of the aryl group which may have a substituent is preferably 5 or more, more preferably 6 or more, preferably 20 or less, more preferably 12 or less, and further preferably 8 or less.

[0100] Examples of the alicyclic ring include cyclobutane ring, cyclopentane ring, cyclohexane ring, cycloheptane ring, and these rings having a hydrocarbon group. The alicyclic ring may also be a polycyclic ring such as an adamantyl ring and a methyladamantyl ring.

[0101] Examples of the substituent which the alkyl group and the aryl group may have include a halogen atom, a hydrocarbon group having 1 to 8 carbon atoms, an alkoxy group having 1 to 8 carbon atoms, a carboxylate group having 1 to 8 carbon atoms, a sulfonate group having 1 to 8 carbon atoms, a carbonyl group having 1 to 8 carbon atoms, an amide group having 1 to 8 carbon atoms, an amino group having 1 to 8 carbon atoms, a thioether group having 1 to 8 carbon atoms, a phosphate group having 1 to 8 carbon atoms, an alkylsilyl group having 1 to 8 carbon atoms, and an alkoxysilyl group having 1 to 8 carbon atoms.

[0102] Among them, from the viewpoint of easily obtaining the present composition having excellent bonding strength with a layer containing polyethylene terephthalate, R4 is preferably an unbranched and unringed alkyl group, and more preferably an unbranched and unringed alkyl group having 3 to 7 carbon atoms.

[0103] Furthermore, from the viewpoints of improving the stability of the carbodiimide group in the air and when heated, improving the yield when synthesizing the modified product, reducing the manufacturing cost, etc., and from the viewpoint of easily obtaining the present composition having excellent bonding strength with the layer containing the biodegradable polymer, the above-mentioned R4 is preferably an alkyl group having a branch but no ring, and more preferably an alkyl group having a branch but no ring and having 3 to 7 carbon atoms.

[0104] In addition, when the above R4 does not have a ring, the steric hindrance caused by the ring structure can be suppressed, and the reactivity of the carbodiimide group can be improved.

[0105] Preferred examples of the unbranched and ring-free alkyl group include n-propyl, n-butyl, n-pentyl, n-hexyl, n-heptyl, n-octyl and n-nonyl.

[0106] Preferred examples of the branched but non-cyclic alkyl group include isopropyl, sec-butyl, isobutyl, tert-butyl, 1-methylbutyl, 1,2-dimethylpropyl, 2-methylbutyl, 3-methylbutyl, 1-ethylpropyl, 1,1-dimethylpropyl, 2,2-dimethylpropyl, 1-methylpentyl, 1,2-dimethylbutyl, 1,3-dimethylbutyl, 1,2,2-trimethylpropyl, 2-methylpentyl, 2,2-dimethylbutyl, 1,3-dimethylbutyl, 1,2,2-trimethylpropyl, 2-methylpentyl, 2,2-dimethylbutyl, 1,2,2-tri ...-trimethylbutyl, 1,2-trimethylbutyl, 1,2-trimethylbutyl, 1,2-trimethylbutyl, 1,2-trimethylbutyl, 1,2-trimethylbutyl, 1,2-trimethylbutyl, 1,2-trimethylbutyl, 1,2-trimethylbutyl, 1,2-trimethylbutyl, 1,2-trimethylbutyl, 1,2-trimethylbutyl, 1,2-trimethylbutyl, Methylbutyl, 2,3-dimethylbutyl, 2-ethylbutyl, 3-methylpentyl, 3,3-dimethylbutyl, 4-methylpentyl, 1-ethyl-2-methylpropyl, 1-ethylbutyl, 1,1-dimethylbutyl, 1,1,2-trimethylpropyl, 1-ethyl-1-methylpropyl, 1-methylhexyl, 1,2-dimethylpentyl, 1,3-dimethylpentyl, 1,4-dimethylpentyl, 1,2,3-trimethylbutyl, 1, 2,2-trimethylbutyl, 1,3,3-trimethylbutyl, 2-dimethylhexyl, 2,3-dimethylpentyl, 2,4-dimethylpentyl, 2,3,3-trimethylbutyl, 1,1-dimethylpentyl, 1,1,2-trimethylbutyl, 1,1,3-trimethylbutyl, 1,1,2,2-tetramethylpropyl, 2,2-dimethylpentyl, 2,2,3-trimethylbutyl, 3-methylhexyl, 3,4-dimethylpentyl, 3 ,3-dimethylpentyl, 1-ethylpentyl, 1-ethyl-2-methylbutyl, 1-ethyl-3-methylbutyl, 1-ethyl-2,2-dimethylpropyl, 2-ethylpentyl, 2-ethyl-3-methylbutyl, 1-ethyl-1-methylbutyl, 1-ethyl-1,2-dimethylpropyl, 3-ethylpentyl, 1,1-diethylpropyl, 2,2-diethylpropyl, 1-propylbutyl, diisopropylmethyl, 1-isopropylbutyl.

[0107] In formula (2), m is an integer of 2 or more, and is preferably an integer of 2 to 6, more preferably an integer of 2 to 4, and particularly preferably 2, from the viewpoint of the solubility and availability of the carbodiimide monomer, and the ease of purification of the obtained graft modified product.

[0108] [Matrix polymer]

[0109] The base polymer before being graft-modified with the carbodiimide monomer is at least one polymer selected from polyolefins.

[0110] Specific examples of the olefin include ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 1-octene, 1-decene, and 4-methyl-1-pentene.

[0111] The polyolefin may be a homopolymer of these olefins, a copolymer of two or more of these olefins, or a copolymer of one or more of these olefins and one or more of the following comonomers. The polyolefin may be preferably at least one polymer selected from ethylene polymers, propylene polymers and butene polymers. When a solvent is used during the graft reaction, it is more preferably at least one polymer selected from ethylene polymers and propylene polymers from the viewpoints of excellent solubility in the solvent and excellent separation from impurities after the graft reaction.

[0112] The matrix polymer of the present modified product may be two or more types, but is usually one type.

[0113] From the viewpoint of better exerting the effects of the present invention, the matrix polymer is preferably a polymer having no at least one active hydrogen-containing group selected from the group consisting of a carboxyl group, an acid anhydride group, an amino group, a hydroxyl group, and a thiol group.

[0114] In order to better exert the effects of the present invention, the matrix polymer is preferably a polymer having no carboxylic acid derivative groups such as acyl halide, amide, imide, and ester, and no groups such as epoxy groups that are easily converted to groups having active hydrogen by water or the like.

[0115] The weight average molecular weight (Mw) of the matrix polymer is not particularly limited, but is preferably 100,000 or more, more preferably 150,000 or more, and preferably 1,000,000 or less, more preferably 700,000 or less, from the viewpoint of ease of synthesis of the modified product.

[0116] The number average molecular weight (Mn) of the matrix polymer is not particularly limited either, but is preferably 40,000 or more, more preferably 50,000 or more, and is preferably 500,000 or less, more preferably 300,000 or less for the same reason.

[0117] The molecular weight distribution (Mw / Mn) of the matrix polymer is not particularly limited, but is preferably 1.5 or more, more preferably 2.0 or more, and is preferably 6.0 or less, more preferably 5.0 or less.

[0118] The above-mentioned Mw and Mn are values ​​measured under the following conditions using HLC-8321GPC / HT gel permeation chromatograph (GPC) manufactured by Tosoh Corporation.

[0119] Separation columns: TSKgel GMH6-HT (2 columns) and TSKgel GMH6-HTL (2 columns) (both 7.5 mm ID × 30 cm, manufactured by Tosoh Corporation)

[0120] Column temperature: 140°C

[0121] Mobile phase: o-dichlorobenzene (containing 0.025% butylated hydroxytoluene (BHT))

[0122] Development speed: 1.0mL / min

[0123] Sample concentration: 0.1% (w / v)

[0124] Sample injection volume: 0.4mL

[0125] Detector: Differential Refractometer

[0126] Calibration of the device: Calibrated using monodisperse polystyrene (manufactured by Tosoh Corporation, #3std set)

[0127] The above-mentioned matrix polymer can be synthesized by a conventionally known method, or a commercially available product can be used.

[0128] The above-mentioned conventionally known methods are not particularly limited, and for example, methods using a coordination polymerization catalyst system containing a transition metal can be cited. Specifically, a method of synthesizing by (co)polymerizing olefins such as ethylene and propylene with the following comonomers as required in the presence of a catalyst such as a magnesium chloride-supported titanium catalyst, a vanadium-based catalyst containing a soluble vanadium compound and an alkyl aluminum halide compound, or a metallocene catalyst containing a metallocene compound and an organic aluminum oxide compound can be cited.

[0129] The raw materials of the matrix polymer (for example, olefins and monomers such as the comonomer described below) may be only biomass-derived raw materials, only fossil fuel-derived raw materials, or both biomass-derived raw materials and fossil fuel-derived raw materials.

[0130] From the viewpoint of reducing environmental load (mainly reducing greenhouse gases), the matrix polymer is preferably a polymer made from a biomass-derived raw material.

[0131] [Ethylene polymers]

[0132] The above-mentioned ethylene-based polymer is not particularly limited as long as the content of the structural unit of the ethylene source in the polymer is a polymer of more than 50 mass %, and can be a homopolymer of ethylene or a copolymer of ethylene and a comonomer. In the case of a copolymer, its structure is not particularly limited.

[0133] Examples of the comonomer include at least one monomer selected from the group consisting of propylene, α-olefins having 4 to 20 carbon atoms, and conjugated polyenes. Among them, propylene and α-olefins having 4 to 20 carbon atoms are preferred.

[0134] The α-olefins having 4 to 20 carbon atoms may be linear or branched, and examples thereof include 1-butene, 2-butene, 1-pentene, 3-methyl-1-butene, 1-hexene, 4-methyl-1-pentene, 3-methyl-1-pentene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecene, and 1-eicosene.

[0135] From the viewpoint that pellet, powder etc. are not easy to occur agglomeration, easy handling etc., the content of the structural unit in the above-mentioned comonomer source in the above-mentioned ethylene-based polymer is preferably below 50 mass %, more preferably below 30 mass %, particularly preferably below 20 mass %.It should be noted that the content of the structural unit in propylene source, butene source is 50 mass % ethylene-based polymer referred to as ethylene-based polymer in this manual.

[0136] [Propylene polymer]

[0137] The propylene-based polymer is not particularly limited as long as the content of the structural unit derived from propylene in the polymer is 50% by mass or more, and may be a homopolymer of propylene or a copolymer of propylene and a comonomer. The structure of these (co)polymers is not particularly limited.

[0138] Examples of the comonomer include at least one monomer selected from the group consisting of ethylene, α-olefins having 4 to 20 carbon atoms, and conjugated polyenes. Among them, ethylene and α-olefins having 4 to 20 carbon atoms are preferred.

[0139] Examples of the α-olefin having 4 to 20 carbon atoms include the same α-olefin having 4 to 20 carbon atoms as mentioned in the ethylene-based polymer section.

[0140] From the viewpoint of pellets, powders, etc. being less prone to agglomeration and easy handling, the content of the structural unit derived from the comonomer in the propylene polymer is preferably 50% by mass or less, more preferably 30% by mass or less, and particularly preferably 20% by mass or less. It should be noted that the propylene polymer having a content of 50% by mass of the structural unit derived from butene is referred to as the propylene polymer in this specification.

[0141] [Butene polymer]

[0142] The butene polymer is not particularly limited as long as the content of structural units derived from butene in the polymer is 50% by mass or more, and can be a homopolymer of butene, especially 1-butene, or a copolymer of butene (especially 1-butene) and a comonomer. The structure of these (co)polymers is not particularly limited.

[0143] Examples of the comonomer include at least one monomer selected from the group consisting of ethylene, propylene, α-olefins having 5 to 20 carbon atoms, and conjugated polyenes. Among them, ethylene, propylene, and α-olefins having 5 to 20 carbon atoms are preferred.

[0144] Examples of the α-olefin having 5 to 20 carbon atoms include the same α-olefin having 5 to 20 carbon atoms as mentioned in the ethylene-based polymer section.

[0145] From the viewpoint of preventing pellets, powders, etc. from agglomerating and easy handling, the content of the structural unit derived from the comonomer in the butene-based polymer is preferably 50% by mass or less, more preferably 30% by mass or less, and particularly preferably 20% by mass or less.

[0146] <Method for synthesizing the modified product>

[0147] The synthesis method of the modified body is not particularly limited as long as a graft modified body obtained by grafting the above-mentioned matrix polymer with the above-mentioned carbodiimide monomer can be obtained. However, from the viewpoint of being able to easily synthesize the modified body, it is preferred to add a free radical initiator and the above-mentioned carbodiimide monomer to a liquid obtained by dissolving or dispersing the above-mentioned matrix polymer in a solvent, preferably a solution obtained by dissolving the above-mentioned matrix polymer in an organic solvent to react (grafting reaction). It should be noted that in the case of using a reaction device with a stirring ability that can make the matrix polymer flow evenly, a solvent may not be used.

[0148] By initiating graft polymerization by the above method, a graft-modified product can be obtained.

[0149] From the viewpoints of being able to easily obtain the modified product having a grafting ratio within the above-mentioned range and being able to suppress the formation of a polymer of the carbodiimide monomer itself (hereinafter also referred to as a "non-grafted polymer"), the amount of the carbodiimide monomer used in the above-mentioned grafting reaction is preferably 10 to 1000 mol, more preferably 10 to 800 mol, relative to 1 mol of the matrix polymer.

[0150] Examples of the free radical initiator include organic peroxides and azo compounds, and specifically include benzoyl peroxide, dichlorobenzoyl peroxide, diisopropyl peroxide, di-tert-butyl peroxide, 2,5-dimethyl-2,5-di(peroxybenzoate)hexyne-3, 1,4-di(tert-butylperoxyisopropyl)benzene, lauroyl peroxide, tert-butyl peroxyacetate, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexyne-3 , 2,5-dimethyl-2,5-di(tert-butyl peroxide)hexane, tert-butyl perbenzoate, tert-butyl peroxyphenylacetate, tert-butyl peroxyisobutyrate, tert-butyl peroxysec-octanoate, tert-butyl peroxypivalate, isopropyl peroxypivalate, tert-butyl peroxydiethylacetate, tert-butyl peroxyisopropyl monocarbonate (tert-butyl peroxyisopropyl monocarbonate) and other organic peroxides; azo compounds such as azobisisobutyronitrile and dimethyl azoisobutyrate. Among them, organic peroxide compounds such as diisopropyl peroxide, di-tert-butyl peroxide, 2,5-dimethyl-2,5-di(tert-butyl peroxide)hexyne-3, 2,5-dimethyl-2,5-di(tert-butyl peroxide)hexane, 1,4-di(tert-butylperoxyisopropyl)benzene, and tert-butyl peroxyisopropyl monocarbonate are preferred.

[0151] The above-mentioned radical initiators may be used alone or in combination of two or more.

[0152] From the viewpoint of being able to efficiently initiate the grafting reaction and easily obtain the modified product with a grafting ratio within the above-mentioned range, the amount of the free radical initiator used in the above-mentioned grafting reaction is preferably 0.01 mol or more, more preferably 0.05 mol or more, and preferably 0.7 mol or less, more preferably 0.5 mol or less, relative to 1 mol of the carbodiimide monomer.

[0153] As the above-mentioned organic solvent, it is preferred that the grafting reaction of the above-mentioned carbodiimide monomer is not significantly hindered and that the organic solvent has affinity with the matrix polymer in the temperature range of the grafting reaction. As a specific example of such an organic solvent, aromatic hydrocarbon solvents such as benzene, toluene, and xylene, aliphatic hydrocarbon solvents such as pentane, hexane, heptane, octane, nonane, and decane, alicyclic hydrocarbon solvents such as cyclohexane, methylcyclohexane, and decalin, chlorinated hydrocarbon solvents such as chlorobenzene, dichlorobenzene, trichlorobenzene, methylene chloride, chloroform, carbon tetrachloride, and tetrachloroethylene, alcohol solvents such as methanol, ethanol, n-propanol, isopropanol, n-butanol, sec-butanol, and tert-butanol, ketone solvents such as acetone, methyl ethyl ketone, and methyl isobutyl ketone, ester solvents such as ethyl acetate and dimethyl phthalate, and ether solvents such as dimethyl ether, diethyl ether, di-n-pentyl ether, tetrahydrofuran, and dihydroxyanisole can be cited. In addition, water can also be used as a solvent for suspension polymerization and emulsion polymerization. These solvents may be used alone or in combination of two or more.

[0154] It should be noted that, although it is preferred that the reaction solution be a homogeneous phase by using these solvents, it may be a heterogeneous multi-phase.

[0155] In order to carry out the graft reaction in a region where the liquid containing the matrix polymer can be uniformly stirred, the concentration of the matrix polymer in the liquid is generally set to 50 to 500 g / L, and preferably to 200 to 500 g / L to achieve a high grafting rate.

[0156] The free radical initiator and carbodiimide monomer can be added to the liquid containing the matrix polymer (or the matrix polymer itself) at once to initiate the grafting reaction. However, in order to achieve a high grafting rate, it is preferred to add them successively over a period of about 0.1 to 5 hours to carry out the grafting reaction.

[0157] It should be noted that, when adding a free radical initiator and a carbodiimide monomer to a matrix polymer or to a liquid obtained by dissolving or dispersing the matrix polymer in a solvent, the order of adding these substances is not particularly limited. For example, when adding these substances one by one as described above, the free radical initiator and the carbodiimide monomer may be added one by one, or the free radical initiator may be added one by one after the carbodiimide monomer is added first.

[0158] The grafting reaction is preferably carried out at a temperature usually above 60°C, preferably at a temperature above 100°C, usually below 200°C, preferably below 160°C, for usually 2 hours or more, preferably 3 hours or more, usually 10 hours or less, preferably 8 hours or less.

[0159] The modified product obtained by the above grafting reaction can be purified and separated by known methods such as filtration, centrifugation, reprecipitation and / or washing to remove the used solvent, unreacted radical initiator, carbodiimide monomer, by-product non-grafted polymer, etc.

[0160] In this case, from the viewpoint of easily obtaining the present composition having better adhesiveness, it is desirable to purify and separate so that the content of the non-grafted polymer contained in the present modified product is preferably 5% by mass or less, more preferably 2% by mass or less.

[0161] "Laminated Body"

[0162] A laminate according to one embodiment of the present invention comprises: a layer (A) containing polyethylene terephthalate or a biodegradable polymer; and an adhesive layer (B) containing the present composition, wherein at least a portion of the layer (B) is in contact with the layer (A).

[0163] Since the laminate has the layer (B), it has excellent interlayer adhesion.

[0164] As long as the laminate comprises the above-mentioned layer (A) and layer (B), there is no particular limitation, and the laminate may comprise two or more layers of the layer (A), or two or more layers of the layer (B). When comprising two or more layers of the layer (A), these layers may be the same layers or different layers. Also, in the case of comprising two or more layers of the layer (B), these layers may be the same layers or different layers.

[0165] The above-mentioned laminate is preferably a laminate comprising layer (A) and layer (B), particularly preferably a laminate consisting of layer (A) and layer (B), or a laminate comprising layer (A), layer (B) and layer (A) in sequence, particularly preferably a laminate in which layer (A), layer (B) and layer (A) are stacked in sequence.

[0166] In addition, as a laminate including the above-mentioned layer (A) and layer (B), for example, a laminate including layer (A), layer (B), and layer (C) in this order may be sufficient.

[0167] The layer (C) is not particularly limited as long as it is a layer other than layer (A) and layer (B), and examples thereof include a layer containing metal; glass; wood; paper; cloth; polyester; thermoplastic resins such as polyphenylene sulfide, polyamide, polyacetal, polycarbonate, poly(meth)acrylate, olefin polymer, polystyrene, rubber, modified fluororesin, biomass plastic, and other engineering plastics; and a layer containing a thermosetting resin or a layer consisting of these materials.

[0168] The laminated body is not limited to the laminated film (sheet) shape, and may be any of various known shapes such as a hollow container, a cup, a tray, etc.

[0169] The layer (B) is a layer comprising the present composition and can be obtained using the present composition.

[0170] The content of the present composition in the layer (B) is preferably 80 to 100% by mass, more preferably 90 to 100% by mass.

[0171] The presence of the modified product in the layer (B) can be determined by infrared spectroscopy.

[0172] The thickness of the layer (B) is not particularly limited and may be appropriately selected depending on the intended use of the laminate, but is preferably 2 to 1000 μm.

[0173] The thickness of the layer (A) is not particularly limited and can be appropriately selected depending on the application of the laminate, but is preferably 2 to 1000 μm.

[0174] The layer (A) is not particularly limited as long as it contains polyethylene terephthalate or a biodegradable polymer, but is preferably a layer consisting (only) of polyethylene terephthalate or (only) of a biodegradable polymer.

[0175] The polyethylene terephthalate and biodegradable polymer may be polymers using only biomass-derived raw materials, only fossil fuel-derived raw materials, or both biomass-derived raw materials and fossil fuel-derived raw materials as their raw materials (e.g., olefins).

[0176] From the viewpoint of reducing environmental load (mainly reducing greenhouse gases), the polyethylene terephthalate and the biodegradable polymer are preferably polymers made from biomass-derived raw materials.

[0177] Examples of the biodegradable polymer include polylactic acid, polyglycolic acid, a lactic acid-glycolic acid copolymer, polyhydroxybutyrate, polybutylene succinate, polyvinyl alcohol, cellulose, cellulose acetate, polyethylene succinate, polycaprolactone, a modified polybutylene succinate / adipate, a modified polybutylene succinate / carbonate, and polybutylene adipate terephthalate. Among these, polylactic acid is preferred.

[0178] The layer (A) may contain additives such as phenolic antioxidants, phosphorus antioxidants, sulfur antioxidants, metal compounds, and metal salts of higher fatty acids which are usually added to resins as needed, within the range not impairing the purpose of the present invention.

[0179] The additive may be an additive using only a biomass-derived raw material as its raw material, an additive using only a fossil fuel-derived raw material, or an additive using both a biomass-derived raw material and a fossil fuel-derived raw material.

[0180] The laminate is preferably a laminate obtained by lamination molding, co-extrusion molding, blow molding or coinjection molding from the viewpoint of easily obtaining a laminate having excellent adhesive strength.

[0181] The method for manufacturing the above-mentioned laminate varies depending on the shape, size, required physical properties, etc. of the final product and is not particularly limited. However, from the viewpoint of being able to easily manufacture the present laminate having the required physical properties of excellent interlayer adhesion, it is preferably manufactured by a method comprising step 1 of co-extrusion molding, lamination molding, blow molding or co-injection molding of a resin composition containing polyethylene terephthalate or a biodegradable polymer and the above-mentioned present composition.

[0182] As the co-extrusion molding, lamination molding, blow molding and coinjection molding, conventionally known methods can be adopted.

[0183] The temperature during production of the laminate is preferably 160 to 250°C, more preferably 200 to 230°C.

[0184] Since the laminate includes the layer (B), a laminate having excellent adhesive strength can be easily obtained even if the temperature during the production of the laminate is low, specifically, even if it is 230° C. or lower.

[0185] When the layer (A) is a layer containing a biodegradable polymer, the step 1 is preferably performed at a temperature lower than the thermal degradation temperature of the biodegradable polymer from the viewpoint of easily producing the present laminate having the desired physical properties of excellent interlayer adhesion.

[0186] The temperature lower than the thermal degradation temperature (Td) is preferably a temperature lower than the thermal degradation temperature (Td) of the biodegradable polymer by 20° C. or more.

[0187] When process 1 is carried out at the above-mentioned temperature, thermal degradation of the biodegradable polymer can be suppressed (for example, the reduction rate of the number average molecular weight of the biodegradable polymer measured by gel permeation chromatography (GPC) before and after the bonding process can be controlled to be less than 10% by mass), and the reduction in the mechanical properties of the biodegradable polymer can be suppressed, thereby obtaining a laminate.

[0188] Examples of the lamination molding include the following methods (1) and (2).

[0189] (1) A method of heat-sealing at a temperature equal to or higher than the temperature at which at least one of the preformed layers (A) and (B) melts using a calendar roll forming machine, a compression forming machine, or the like.

[0190] (2) A method of heat-fusion bonding a preformed layer (A) or layer (B) to another layer obtained by extrusion molding or calendar molding.

[0191] When a laminate is manufactured by pressing (heat sealing) the preformed layer (A) and layer (B) using a compression molding machine in the above-mentioned method (1), when heat sealing is performed at, for example, 230°C, a layer with high bonding strength can be formed even if the heat sealing time is set to a short time such as preferably less than 20 seconds, more preferably less than 10 seconds, and further preferably less than 5 seconds.

[0192] Examples of the co-extrusion molding include a method in which a resin composition containing polyethylene terephthalate or a biodegradable polymer is simultaneously extruded with the present composition using a multilayer extruder to form heat-fused layers (A) and (B).

[0193] Examples of the above-mentioned coinjection molding include a method in which a resin composition containing molten polyethylene terephthalate or a biodegradable polymer and the molten present composition are injected into a mold at the same time or at different injection timings (eg, double injection molding, sandwich injection molding).

[0194] Example

[0195] Hereinafter, one embodiment of the present invention will be described based on examples, but the present invention is not limited to these examples.

[0196] <Method for measuring grafting rate>

[0197] Using an AVANCE III cryo-500 nuclear magnetic resonance apparatus (500 MHz) manufactured by Bruker Biospin Co., Ltd., under the measurement conditions of 1,1,2,2-tetrachloroethane-d2 as the measurement solvent, 120°C as the measurement temperature, 20 ppm as the spectrum width, 7.0 seconds as the pulse repetition time, and 5.00 μsec as the pulse width (45° pulse), the graft polymer obtained in the following synthesis example was obtained. 1 H-NMR spectrum. In the obtained spectrum, the grafting ratio of the grafted polymer obtained in the following synthesis example was calculated based on the peak intensity ratio of the protons of the hydrocarbon group bonded to the carbodiimide group present at 3.0 ppm to 4.0 ppm and the protons bonded to all hydrocarbon groups derived from the matrix polymer present at 0.3 ppm to 2.5 ppm.

[0198] [Synthesis example 1]

[0199] In a 1L autoclave, 25.0g of LLDPE (matrix polymer, comonomer species: 1-hexene, comonomer amount: 1.6% by mass, Mw: 164,000, Mn: 63,000, Mw / Mn: 2.60) and 150mL of toluene were placed, and the autoclave was nitrogen purged and sealed. Then, the internal temperature of the autoclave was raised to 140°C, and while maintaining this temperature, a double anchor blade was used to stir at a stirring speed of 400rpm, and 28.1mmol of vinylphenylcyclohexylcarbodiimide and 2.2mmol of diisopropylbenzene peroxide (PERCUMYL D, manufactured by NOF Corporation) were fed over 2 hours. Then, after stirring for another two hours, 250mL of toluene was passed over 15 minutes to dilute the reaction solution.

[0200] Then, the internal temperature of the autoclave was cooled to 50°C, and after the pressure was removed, the slurry-like reaction liquid was taken out. 400 mL of acetone was added to the obtained reaction liquid, and after stirring for 10 minutes, the stirred liquid was filtered to separate into a solid component and a filtrate. The steps from adding the acetone to filtering were repeated twice for the obtained solid component. Through these three filtrations, unreacted vinylphenylcyclohexylcarbodiimide and homopolymers of vinylphenylcyclohexylcarbodiimide were removed.

[0201] The solid content after the third filtration was dried in a vacuum dryer at 70° C. for 10 hours to obtain 25.71 g of a graft polymer (P-1). The graft ratio was 2.7% by mass.

[0202] [Synthesis example 2]

[0203] 25.0 g of polypropylene (matrix polymer, Mw: 313,000, Mn: 70,800, Mw / Mn: 4.42) and 110 mL of xylene were placed in a 500 mL separable flask, and after nitrogen substitution, the internal temperature of the separable flask was raised to 120° C., and while maintaining the temperature, 28.1 mmol of vinylphenylcyclohexylcarbodiimide was placed, and then 2.2 mmol of tert-butylperoxyisopropylmonocarbonate (PERBUTYL I, manufactured by NOF Corporation) dissolved in 10 mL of xylene was fed over 10 minutes while stirring at a stirring speed of 400 rpm using a double anchor blade. Then, after stirring for another 3 hours, 200 mL of xylene was introduced to dilute the reaction solution.

[0204] Then, the internal temperature of the separable flask was cooled to 50°C, and the slurry-like reaction liquid was taken out. 400 mL of acetone was added to the obtained reaction liquid, and after stirring for 10 minutes, the stirred liquid was filtered to separate into a solid component and a filtrate. The steps from adding the acetone to filtering were repeated three times for the obtained solid component. Through these four filtrations, unreacted vinylphenylcyclohexylcarbodiimide and homopolymers of vinylphenylcyclohexylcarbodiimide were removed.

[0205] The solid content after the fourth filtration was dried in a vacuum dryer at 90° C. for 10 hours to obtain 25.13 g of a graft polymer (P-2). The graft ratio was 1.5% by mass.

[0206] [Synthesis example 3]

[0207] 25.0 g of LLDPE (the same polymer as the matrix polymer used in Synthesis Example 1) and 110 mL of xylene were placed in a 500 mL separable flask, and after nitrogen substitution in the separable flask, the internal temperature was raised to 120° C., and while maintaining the temperature, 33.4 mmol of ethylphenylcarbodiimide methacrylate was placed, and then 2.2 mmol of tert-butyl peroxyisopropyl monocarbonate (PERBUTYL I, manufactured by NOF Corporation) dissolved in 10 mL of xylene was fed over 10 minutes while stirring at a stirring speed of 400 rpm using a double anchor blade. Then, after stirring for another 3 hours, 200 mL of xylene was introduced to dilute the reaction solution.

[0208] Then, the internal temperature of the separable flask was cooled to 50°C, and the slurry-like reaction liquid was taken out. 400 mL of acetone was added to the obtained reaction liquid, and after stirring for 10 minutes, the stirred liquid was filtered to separate into a solid component and a filtrate. The steps from adding the acetone to filtering were repeated three times for the obtained solid component. By these four filtrations, unreacted ethylphenylcarbodiimide methacrylate and homopolymers of ethylphenylcarbodiimide methacrylate were removed.

[0209] The solid content after the fourth filtration was dried in a vacuum dryer at 90° C. for 10 hours to obtain 25.87 g of a graft polymer (P-3). The graft ratio was 2.4% by mass.

[0210] [Synthesis Example 4]

[0211] 17.0 g of LLDPE (the same polymer as the matrix polymer used in Synthesis Example 1) and 78 mL of xylene were placed in a 500 mL separable flask, and after nitrogen substitution, the internal temperature of the separable flask was raised to 120° C., and while maintaining the temperature, 24.5 mmol of ethylcyclohexylcarbodiimide methacrylate was placed, and then 1.68 mmol of tert-butyl peroxyisopropyl monocarbonate (PERBUTYL I, manufactured by NOF Corporation) dissolved in 10 mL of xylene was fed over 10 minutes while stirring at a stirring speed of 400 rpm using a double anchor blade. Then, after stirring for another 3 hours, 150 mL of xylene was introduced to dilute the reaction solution.

[0212] Then, the internal temperature of the separable flask was cooled to 50°C, and the slurry-like reaction liquid was taken out. 400 mL of acetone was added to the obtained reaction liquid, and after stirring for 10 minutes, the stirred liquid was filtered to separate into a solid component and a filtrate. The steps from adding the acetone to filtering were repeated three times for the obtained solid component. By these four filtrations, unreacted methacrylate ethylcyclohexylcarbodiimide and methacrylate ethylcyclohexylcarbodiimide homopolymer were removed.

[0213] The solid content after the fourth filtration was dried in a vacuum dryer at 90° C. for 10 hours to obtain 17.49 g of a graft polymer (P-4). The graft ratio was 3.0% by mass.

[0214] [Synthesis example 5]

[0215] 25.0 g of LLDPE (the same polymer as the matrix polymer used in Synthesis Example 1) and 110 mL of xylene were placed in a 500 mL separable flask, and after nitrogen substitution in the separable flask, the internal temperature was raised to 120° C., and while maintaining the temperature, 35.0 mmol of ethyl tert-butylcarbodiimide methacrylate was placed, and then 2.2 mmol of tert-butyl peroxyisopropyl monocarbonate (PERBUTYL I, manufactured by NOF Corporation) dissolved in 10 mL of xylene was fed over 10 minutes while stirring at a stirring speed of 400 rpm using a double anchor blade. Then, after stirring for another 3 hours, 200 mL of xylene was introduced to dilute the reaction solution.

[0216] Then, the internal temperature of the separable flask was cooled to 50°C, and the slurry-like reaction liquid was taken out. 400 mL of acetone was added to the obtained reaction liquid, and after stirring for 10 minutes, the stirred liquid was filtered to separate into a solid component and a filtrate. The steps from adding the acetone to filtering were repeated three times for the obtained solid component. By these four filtrations, unreacted methacrylate ethyl tert-butylcarbodiimide and methacrylate ethyl tert-butylcarbodiimide homopolymer were removed.

[0217] The solid content after the fourth filtration was dried in a vacuum dryer at 90° C. for 10 hours to obtain 25.49 g of a graft polymer (P-5). The graft ratio was 1.7% by mass.

[0218] [Synthesis example 6]

[0219] 17.1 g of LLDPE (the same polymer as the matrix polymer used in Synthesis Example 1) and 73 mL of xylene were placed in a 500 mL separable flask, and after nitrogen substitution in the separable flask, the internal temperature was raised to 120° C., and while maintaining the temperature, 23.8 mmol of ethyl-n-butylcarbodiimide methacrylate was placed, and then 1.6 mmol of tert-butyl peroxyisopropyl monocarbonate (PERBUTYL I, manufactured by NOF Corporation) dissolved in 10 mL of xylene was fed over 10 minutes while stirring at a stirring speed of 400 rpm using a double anchor blade. Then, after stirring for another 3 hours, 150 mL of xylene was introduced to dilute the reaction solution.

[0220] Then, the internal temperature of the separable flask was cooled to 50°C, and the slurry-like reaction liquid was taken out. 400 mL of acetone was added to the obtained reaction liquid, and after stirring for 10 minutes, the stirred liquid was filtered to separate into a solid component and a filtrate. The steps from adding the acetone to filtering were repeated three times for the obtained solid component. By these four filtrations, unreacted ethyl-n-butylcarbodiimide methacrylate and homopolymers of ethyl-n-butylcarbodiimide methacrylate were removed.

[0221] The solid content after the fourth filtration was dried in a vacuum dryer at 90° C. for 10 hours to obtain 17.38 g of a graft polymer (P-6). The graft ratio was 1.6% by mass.

[0222] [Synthesis Example 7]

[0223] 14.0 g of LLDPE (the same polymer as the matrix polymer used in Synthesis Example 1) and 57 mL of xylene were placed in a 500 mL separable flask, and after nitrogen substitution in the separable flask, the internal temperature was raised to 120° C., and while maintaining the temperature, 19.0 mmol of ethyl p-chlorophenylcarbodiimide methacrylate was placed, and then 1.3 mmol of tert-butyl peroxyisopropyl monocarbonate (PERBUTYL I, manufactured by NOF Corporation) dissolved in 10 mL of xylene was fed over 10 minutes while stirring at a stirring speed of 400 rpm using a double anchor blade. Then, after stirring for another 3 hours, 150 mL of xylene was introduced to dilute the reaction solution.

[0224] Then, the internal temperature of the separable flask was cooled to 50°C, and the slurry-like reaction liquid was taken out. 400 mL of acetone was added to the obtained reaction liquid, and after stirring for 10 minutes, the stirred liquid was filtered to separate into a solid component and a filtrate. The steps from adding the acetone to filtering were repeated three times for the obtained solid component. By these four filtrations, unreacted methacrylate ethyl p-chlorophenylcarbodiimide and methacrylate ethyl p-chlorophenylcarbodiimide homopolymer were removed.

[0225] The solid content after the fourth filtration was dried in a vacuum dryer at 90° C. for 10 hours to obtain 14.43 g of a graft polymer (P-7). The graft ratio was 2.8% by mass.

[0226] [Synthesis example 8]

[0227] 17.0 g of LLDPE (the same polymer as the matrix polymer used in Synthesis Example 1) and 73 mL of xylene were placed in a 500 mL separable flask, and after nitrogen substitution in the separable flask, the internal temperature was raised to 120° C., and while maintaining the temperature, 22.5 mmol of ethyl p-methoxyphenylcarbodiimide of methacrylate was placed, and then 1.5 mmol of tert-butyl peroxyisopropyl monocarbonate (PERBUTYL I, manufactured by NOF Corporation) dissolved in 10 mL of xylene was fed over 10 minutes while stirring at a stirring speed of 400 rpm using a double anchor blade. Then, after stirring for another 3 hours, 150 mL of xylene was introduced to dilute the reaction solution.

[0228] Then, the internal temperature of the separable flask was cooled to 50°C, and the slurry-like reaction liquid was taken out. 400 mL of acetone was added to the obtained reaction liquid, and after stirring for 10 minutes, the stirred liquid was filtered to separate into a solid component and a filtrate. The steps from adding the acetone to filtering were repeated three times for the obtained solid component. By these four filtrations, unreacted methacrylate ethyl p-methoxyphenylcarbodiimide and methacrylate ethyl p-methoxyphenylcarbodiimide homopolymer were removed.

[0229] The solid content after the fourth filtration was dried in a vacuum dryer at 90° C. for 10 hours to obtain 17.37 g of a graft polymer (P-8). The graft ratio was 1.6% by mass.

[0230] [Synthesis Example 9]

[0231] 20.0 g of polypropylene (the same polymer as the matrix polymer used in Synthesis Example 2) and 86 mL of xylene were placed in a 500 mL separable flask, and after nitrogen substitution in the separable flask, the internal temperature was raised to 120° C., and while maintaining the temperature, 22.6 mmol of ethylphenylcarbodiimide methacrylate was placed, and then 9.2 mmol of tert-butyl peroxyisopropyl monocarbonate (PERBUTYL I, manufactured by NOF Corporation) dissolved in 10 mL of xylene was fed over 10 minutes while stirring at a stirring speed of 400 rpm using a double anchor blade. Then, after stirring for another 3 hours, 200 mL of xylene was introduced to dilute the reaction solution.

[0232] Then, the internal temperature of the separable flask was cooled to 50°C, and the slurry-like reaction liquid was taken out. 400 mL of acetone was added to the obtained reaction liquid, and after stirring for 10 minutes, the stirred liquid was filtered to separate into a solid component and a filtrate. The steps from adding the acetone to filtering were repeated three times for the obtained solid component. By these four filtrations, unreacted ethylphenylcarbodiimide methacrylate and homopolymers of ethylphenylcarbodiimide methacrylate were removed.

[0233] The solid content after the fourth filtration was dried in a vacuum dryer at 90° C. for 10 hours to obtain 19.89 g of a graft polymer (P-9). The graft ratio was 1.5% by mass.

[0234] [Synthesis Example 10]

[0235] 19.0 g of polypropylene (the same polymer as the matrix polymer used in Synthesis Example 2) and 81 mL of xylene were placed in a 500 mL separable flask, and after nitrogen substitution in the separable flask, the internal temperature was raised to 120° C., and while maintaining the temperature, 20 mmol of ethylcyclohexylcarbodiimide methacrylate was placed, and then 9.2 mmol of tert-butyl peroxyisopropyl monocarbonate (PERBUTYL I, manufactured by NOF Corporation) dissolved in 10 mL of xylene was fed over 10 minutes while stirring at a stirring speed of 400 rpm using a double anchor blade. Then, after stirring for another 3 hours, 200 mL of xylene was introduced to dilute the reaction solution.

[0236] Then, the internal temperature of the separable flask was cooled to 50°C, and the slurry-like reaction liquid was taken out. 400 mL of acetone was added to the obtained reaction liquid, and after stirring for 10 minutes, the stirred liquid was filtered to separate into a solid component and a filtrate. The steps from adding the acetone to filtering were repeated three times for the obtained solid component. By these four filtrations, unreacted methacrylate ethylcyclohexylcarbodiimide and methacrylate ethylcyclohexylcarbodiimide homopolymer were removed.

[0237] The solid content after the fourth filtration was dried in a vacuum dryer at 90° C. for 10 hours to obtain 18.89 g of a graft polymer (P-10). The graft ratio was 1.4% by mass.

[0238] [Synthesis Example 11]

[0239] 15.0 g of polypropylene (the same polymer as the matrix polymer used in Synthesis Example 2) and 62 mL of xylene were placed in a 500 mL separable flask, and after nitrogen substitution in the separable flask, the internal temperature was raised to 120° C., and while maintaining the temperature, 22.1 mmol of ethyl tert-butylcarbodiimide methacrylate was placed in the flask, and then 9.2 mmol of tert-butyl peroxyisopropyl monocarbonate (PERBUTYL I, manufactured by NOF Corporation) dissolved in 10 mL of xylene was fed over 10 minutes while stirring at a stirring speed of 400 rpm using a double anchor blade. Then, after stirring for another 3 hours, 150 mL of xylene was introduced to dilute the reaction solution.

[0240] Then, the internal temperature of the separable flask was cooled to 50°C, and the slurry-like reaction liquid was taken out. 400 mL of acetone was added to the obtained reaction liquid, and after stirring for 10 minutes, the stirred liquid was filtered to separate into a solid component and a filtrate. The steps from adding the acetone to filtering were repeated three times for the obtained solid component. By these four filtrations, unreacted methacrylate ethyl tert-butylcarbodiimide and methacrylate ethyl tert-butylcarbodiimide homopolymer were removed.

[0241] The solid content after the fourth filtration was dried in a vacuum dryer at 90° C. for 10 hours to obtain 15.37 g of a graft polymer (P-11). The graft ratio was 1.3% by mass.

[0242] [Synthesis Example 12]

[0243] 15.0 g of polypropylene (the same polymer as the matrix polymer used in Synthesis Example 2) and 62 mL of xylene were placed in a 500 mL separable flask, and after nitrogen substitution in the separable flask, the internal temperature was raised to 120° C., and while maintaining the temperature, 17.8 mmol of ethyl p-chlorophenylcarbodiimide methacrylate was placed, and then 6.9 mmol of tert-butyl peroxyisopropyl monocarbonate (PERBUTYL I, manufactured by NOF Corporation) dissolved in 10 mL of xylene was fed over 10 minutes while stirring at a stirring speed of 400 rpm using a double anchor blade. Then, after stirring for another 3 hours, 150 mL of xylene was introduced to dilute the reaction solution.

[0244] Then, the internal temperature of the separable flask was cooled to 50°C, and the slurry-like reaction liquid was taken out. 400 mL of acetone was added to the obtained reaction liquid, and after stirring for 10 minutes, the stirred liquid was filtered to separate into a solid component and a filtrate. The steps from adding the acetone to filtering were repeated three times for the obtained solid component. By these four filtrations, unreacted methacrylate ethyl p-chlorophenylcarbodiimide and methacrylate ethyl p-chlorophenylcarbodiimide homopolymer were removed.

[0245] The solid content after the fourth filtration was dried in a vacuum dryer at 90° C. for 10 hours to obtain 14.60 g of a graft polymer (P-12). The graft ratio was 1.6% by mass.

[0246] [Synthesis Example 13]

[0247] 20.0 g of polypropylene (the same polymer as the matrix polymer used in Synthesis Example 2) and 86 mL of xylene were placed in a 500 mL separable flask, and after nitrogen substitution in the separable flask, the internal temperature was raised to 120° C., and while maintaining the temperature, 22.5 mmol of ethyl p-methoxyphenylcarbodiimide of methacrylate was placed, and then 9.2 mmol of tert-butyl peroxyisopropyl monocarbonate (PERBUTYL I, manufactured by NOF Corporation) dissolved in 10 mL of xylene was fed over 10 minutes while stirring at a stirring speed of 400 rpm using a double anchor blade. Then, after stirring for another 3 hours, 200 mL of xylene was introduced to dilute the reaction solution.

[0248] Then, the internal temperature of the separable flask was cooled to 50°C, and the slurry-like reaction liquid was taken out. 400 mL of acetone was added to the obtained reaction liquid, and after stirring for 10 minutes, the stirred liquid was filtered to separate into a solid component and a filtrate. The steps from adding the acetone to filtering were repeated three times for the obtained solid component. By these four filtrations, unreacted methacrylate ethyl p-methoxyphenylcarbodiimide and methacrylate ethyl p-methoxyphenylcarbodiimide homopolymer were removed.

[0249] The solid content after the fourth filtration was dried in a vacuum dryer at 90° C. for 10 hours to obtain 20.30 g of a graft polymer (P-13). The graft ratio was 1.6% by mass.

[0250] [Synthesis Example 14]

[0251] 23 g of LLDPE (the same polymer as the matrix polymer used in Synthesis Example 1) and 100 mL of xylene were placed in a 500 mL separable flask, and after nitrogen substitution in the separable flask, the internal temperature was raised to 120° C., and while maintaining the temperature, 30 mmol of ethylisopropylcarbodiimide methacrylate was placed in the flask, and then 2.0 mmol of tert-butylperoxyisopropylmonocarbonate (PERBUTYL I, manufactured by NOF Corporation) dissolved in 10 mL of xylene was fed over 10 minutes while stirring at a stirring speed of 400 rpm using a double anchor blade. After stirring for another 3 hours, 150 mL of xylene was introduced to dilute the reaction solution.

[0252] Then, the internal temperature of the separable flask was cooled to 50°C, and the slurry-like reaction liquid was taken out. 400 mL of acetone was added to the obtained reaction liquid, and after stirring for 10 minutes, the stirred liquid was filtered to separate into a solid component and a filtrate. The steps from adding the acetone to filtering were repeated three times for the obtained solid component.

[0253] The solid content after the fourth filtration was dried in a vacuum dryer at 90° C. for 10 hours to obtain 23.54 g of a graft polymer (P-14). The graft ratio was 1.7% by mass.

[0254] [Synthesis Example 15]

[0255] 13.2 g of polypropylene (the same polymer as the matrix polymer used in Synthesis Example 2) and 54 mL of xylene were placed in a 500 mL separable flask, and after nitrogen substitution in the separable flask, the internal temperature was raised to 120° C., and while maintaining the temperature, 19.5 mmol of ethylisopropylcarbodiimide methacrylate was placed, and then 8.0 mmol of tert-butylperoxyisopropylmonocarbonate (PERBUTYL I, manufactured by NOF Corporation) dissolved in 10 mL of xylene was fed over 10 minutes while stirring at a stirring speed of 400 rpm using a double anchor blade. Then, after stirring for another 3 hours, 150 mL of xylene was introduced to dilute the reaction solution.

[0256] Then, the internal temperature of the separable flask was cooled to 50°C, and the slurry-like reaction liquid was taken out. 400 mL of acetone was added to the obtained reaction liquid, and after stirring for 10 minutes, the stirred liquid was filtered to separate into a solid component and a filtrate. The steps from adding the acetone to filtering were repeated three times for the obtained solid component.

[0257] The solid content after the fourth filtration was dried in a vacuum dryer at 90° C. for 10 hours to obtain 13.29 g of a graft polymer (P-13). The graft ratio was 1.7% by mass.

[0258] [Synthesis Example 16]

[0259] 25.0 g of LLDPE (the same polymer as the matrix polymer used in Synthesis Example 1) and 120 mL of xylene were placed in a 500 mL separable flask, and after nitrogen substitution in the separable flask, the internal temperature was raised to 120° C., and while maintaining the temperature, 33.4 mmol of glycidyl methacrylate was placed, and then 2.2 mmol of tert-butyl peroxyisopropyl monocarbonate (PERBUTYL I, manufactured by NOF Corporation) dissolved in 10 mL of xylene was fed over 10 minutes while stirring at a stirring speed of 400 rpm using a double anchor blade. Then, after stirring for another 3 hours, 200 mL of xylene was introduced to dilute the reaction solution.

[0260] Then, the internal temperature of the separable flask was cooled to 50°C, and the slurry-like reaction liquid was taken out. 400 mL of acetone was added to the obtained reaction liquid, and after stirring for 10 minutes, the stirred liquid was filtered to separate into a solid component and a filtrate. The steps from the addition of acetone to the filtration were repeated three times. Unreacted glycidyl methacrylate and homopolymer of glycidyl methacrylate were removed by these four filtrations.

[0261] The solid content after the fourth filtration was dried in a vacuum dryer at 90° C. for 10 hours to obtain 25.95 g of a graft polymer (P-16). The graft ratio was 2.4% by mass.

[0262] [Synthesis Example 17]

[0263] 25.0 g of polypropylene (the same polymer as the matrix polymer used in Synthesis Example 2) and 120 mL of xylene were placed in a 500 mL separable flask, and after nitrogen substitution in the separable flask, the internal temperature was raised to 120° C., and while maintaining the temperature, 33.4 mmol of glycidyl methacrylate was placed, and then 11 mmol of tert-butyl peroxyisopropyl monocarbonate (PERBUTYL I, manufactured by NOF Corporation) dissolved in 10 mL of xylene was fed over 10 minutes while stirring at a stirring speed of 400 rpm using a double anchor blade. Then, after stirring for another 3 hours, 200 mL of xylene was introduced to dilute the reaction solution.

[0264] Then, the internal temperature of the separable flask was cooled to 50°C, and the slurry-like reaction liquid was taken out. 400 mL of acetone was added to the obtained reaction liquid, and after stirring for 10 minutes, the stirred liquid was filtered to separate into a solid component and a filtrate. The steps from adding the acetone to filtering were repeated three times for the obtained solid component. By these four filtrations, unreacted glycidyl methacrylate and homopolymers of glycidyl methacrylate were removed.

[0265] The solid content after the fourth filtration was dried in a vacuum dryer at 90° C. for 10 hours to obtain 25.26 g of a graft polymer (P-17). The graft ratio was 1.0% by mass.

[0266] [Synthesis Example 18]

[0267] 12.5 g of LLDPE (the same polymer as the matrix polymer used in Synthesis Example 1) and 50 mL of xylene were placed in a 500 mL separable flask, and after nitrogen substitution in the separable flask, the internal temperature was raised to 120° C., and while maintaining the temperature, 16.7 mmol of vinylphenylcyclohexylcarbodiimide was placed, and then 1.1 mmol of tert-butylperoxyisopropylmonocarbonate (PERBUTYL I, manufactured by NOF Corporation) dissolved in 10 mL of xylene was fed over 10 minutes while stirring at a stirring speed of 400 rpm using a double anchor blade. Then, after stirring for another 3 hours, 200 mL of xylene was introduced to dilute the reaction solution.

[0268] Then, the internal temperature of the separable flask was cooled to 50°C, and the slurry-like reaction liquid was taken out. 400 mL of acetone was added to the obtained reaction liquid, and after stirring for 10 minutes, the stirred liquid was filtered to separate into a solid component and a filtrate. The steps from adding the acetone to filtering were repeated three times for the obtained solid component. Through these four filtrations, unreacted vinylphenylcyclohexylcarbodiimide and homopolymers of vinylphenylcyclohexylcarbodiimide were removed.

[0269] The solid content after the fourth filtration was dried in a vacuum dryer at 90° C. for 10 hours to obtain 13.48 g of a graft polymer (P-18). The graft ratio was 7.6% by mass.

[0270] [Synthesis Example 19]

[0271] 25.0 g of polypropylene (the same polymer as the matrix polymer used in Synthesis Example 2) and 110 mL of xylene were placed in a 500 mL separable flask, and after nitrogen substitution in the separable flask, the internal temperature was raised to 120° C., and while maintaining the temperature, 14.1 mmol of vinylphenylcyclohexylcarbodiimide was placed, and then 1.1 mmol of tert-butylperoxyisopropylmonocarbonate (PERBUTYL I, manufactured by NOF Corporation) dissolved in 10 mL of xylene was fed over 10 minutes while stirring at a stirring speed of 400 rpm using a double anchor blade. Then, after stirring for another 3 hours, 200 mL of xylene was introduced to dilute the reaction solution.

[0272] Then, the internal temperature of the separable flask was cooled to 50°C, and the slurry-like reaction liquid was taken out. 400 mL of acetone was added to the obtained reaction liquid, and after stirring for 10 minutes, the stirred liquid was filtered to separate into a solid component and a filtrate. The steps from adding the acetone to filtering were repeated three times for the obtained solid component. By these four filtrations, unreacted vinylphenylcyclohexylcarbodiimide and homopolymers of vinylphenylcyclohexylcarbodiimide were removed.

[0273] The solid content after the fourth filtration was dried in a vacuum dryer at 90° C. for 10 hours to obtain 24.72 g of a graft polymer (P-19). The graft ratio was 0.5% by mass.

[0274] [Synthesis Example 20]

[0275] 15.0 g of polypropylene (the same polymer as the matrix polymer used in Synthesis Example 2) and 62 mL of xylene were placed in a 500 mL separable flask, and after nitrogen substitution in the separable flask, the internal temperature was raised to 120° C., and while maintaining the temperature, 44.2 mmol of ethyl tert-butylcarbodiimide methacrylate was placed in the flask, and then 18.4 mmol of tert-butyl peroxyisopropyl monocarbonate (PERBUTYL I, manufactured by NOF Corporation) dissolved in 10 mL of xylene was fed over 10 minutes while stirring at a stirring speed of 400 rpm using a double anchor blade. Then, after further stirring for 3 hours, 150 mL of xylene was introduced to dilute the reaction solution.

[0276] Then, the internal temperature of the separable flask was cooled to 50°C, and the slurry-like reaction liquid was taken out. 400 mL of acetone was added to the obtained reaction liquid, and after stirring for 10 minutes, the stirred liquid was filtered to separate into a solid component and a filtrate. The steps from adding the acetone to filtering were repeated three times for the obtained solid component. By these four filtrations, unreacted methacrylate ethyl tert-butylcarbodiimide and methacrylate ethyl tert-butylcarbodiimide homopolymer were removed.

[0277] The solid content after the fourth filtration was dried in a vacuum dryer at 90° C. for 10 hours to obtain 16.11 g of a graft polymer (P-20). The graft ratio was 3.5% by mass.

[0278] [Synthesis Example 21]

[0279] 15.0 g of polypropylene (the same polymer as the matrix polymer used in Synthesis Example 2) and 62 mL of xylene were placed in a 500 mL separable flask, and after nitrogen substitution in the separable flask, the internal temperature was raised to 120° C., and while maintaining the temperature, 11.1 mmol of ethyl tert-butylcarbodiimide methacrylate was placed, and then 4.6 mmol of tert-butyl peroxyisopropyl monocarbonate (PERBUTYL I, manufactured by NOF Corporation) dissolved in 10 mL of xylene was fed over 10 minutes while stirring at a stirring speed of 400 rpm using a double anchor blade. Then, after stirring for another 3 hours, 150 mL of xylene was introduced to dilute the reaction solution.

[0280] Then, the internal temperature of the separable flask was cooled to 50°C, and the slurry-like reaction liquid was taken out. 400 mL of acetone was added to the obtained reaction liquid, and after stirring for 10 minutes, the stirred liquid was filtered to separate into a solid component and a filtrate. The steps from adding the acetone to filtering were repeated three times for the obtained solid component. By these four filtrations, unreacted methacrylate ethyl tert-butylcarbodiimide and methacrylate ethyl tert-butylcarbodiimide homopolymer were removed.

[0281] The solid content after the fourth filtration was dried in a vacuum dryer at 90° C. for 10 hours to obtain 15.12 g of a graft polymer (P-21). The graft ratio was 0.6% by mass.

[0282] [Examples A to C]

[0283] In Example A, 100% by mass of the graft polymer obtained in Synthesis Example 1 was used as the adhesive composition.

[0284] In Example B, 100% by mass of the graft polymer obtained in Synthesis Example 18 was used as the adhesive composition.

[0285] In Example C, 100% by mass of the graft polymer obtained in Synthesis Example 20 was used as the adhesive composition.

[0286] <Carbodiimide Group Amount>

[0287] The amount (mmol) of carbodiimide groups per 100 g of the adhesive compositions obtained in Examples A to C was calculated by the following formula (I). The results are shown in Table 1 as the amount of carbodiimide groups (mmol / 100 g).

[0288] (Grafting ratio [mass %] of the graft modified product used in the adhesive composition / molecular weight of the carbodiimide monomer used in the synthesis of the graft modified product)×100×100 / 10…(I)

[0289] <density>

[0290] The density (g / cm 3 ) was measured in accordance with JIS K 7210. The results are shown in Table 1.

[0291] <Adhesion Evaluation>

[0292] ·Preparation of compressed tablets

[0293] The adhesive compositions obtained in Examples A to C were press-molded at a temperature of 180°C, a pressure of 4 MPa, a preheating time of 5 minutes, and a pressing time of 3 minutes, and then rapidly cooled using a press molding machine set at 20°C to produce pressed sheets with a thickness of 500 μm, a length of 80 mm, and a width of 80 mm.

[0294] ·Production of polyethylene terephthalate laminates

[0295] As the base material layer, a polyethylene terephthalate (PET) sheet (product name: Lumirror T60, manufactured by Toray Industries, Inc.) having a thickness of 50 μm, a length of 80 mm, and a width of 80 mm was used.

[0296] The PET sheet, the above-mentioned pressed sheet and the PET sheet are stacked in sequence, and the stacked body is clamped with Teflon (registered trademark) sheets and heat-sealed for 5 seconds, 10 seconds and 15 seconds using a heat sealing machine with a pressing plate (lower) temperature set to 230°C and a pressing plate (upper) temperature set to 230°C to produce a polyethylene terephthalate laminate consisting of three layers.

[0297] Peel test

[0298] The polyethylene terephthalate laminate was subjected to T-type peeling of the upper PET sheet (PET sheet on the press plate (upper) side) and the pressed sheet under the conditions of a peeling atmosphere temperature of 23° C., a peeling speed of 300 mm / min, and a peeling width of 15 mm, thereby measuring the peel strength of the PET sheet and the pressed sheet. The results are shown in Table 1.

[0299] It should be noted that the case where the PET sheet itself breaks not at the interface between the PET sheet and the pressed sheet due to strong adhesive force is referred to as "PET resin breakage".

[0300] [Table 1]

[0301]

[0302] <mfr>

[0303] The MFR (g / 10 min) of the adhesive compositions obtained in the following Examples and Comparative Examples was measured in accordance with JIS K 7210 under the conditions of 190° C. and a load of 2.16 kg.

[0304] <Carbodiimide Group Amount>

[0305] The amount (mmol) of carbodiimide groups per 100 g of the adhesive compositions obtained in the following Examples and Comparative Examples was calculated by the following formula (I). The results are shown in Tables 2 to 4 as the amount of carbodiimide groups (mmol / 100 g).

[0306] (Grafting ratio of grafted modified body used in adhesive composition [mass %] / molecular weight of carbodiimide monomer used in synthesis of the grafted modified body)×100×amount of grafted modified body used in adhesive composition [mass %] / 10…(I)

[0307] <density>

[0308] The density (g / cm 3 ) was measured in accordance with JIS K 7210. The results are shown in Tables 2 to 4.

[0309] [Example 1]

[0310] Using LABO PLASTOMILL, 11 parts by mass of the graft polymer (P-1) produced in Synthesis Example 1 and 89 parts by mass of LLDPE (the same polymer as the matrix polymer used in the above-mentioned Synthesis Example 1) were mixed at a temperature of 190°C, a screw speed of 60 rpm, and a mixing time of 10 minutes to obtain an adhesive composition C-1.

[0311] The MFR (190°C, 2.16 kg load) of the obtained adhesive composition C-1 was 2.7 g / 10 min and the density was 0.903 g / cm 3 The amount of carbodiimide groups in each 100 g of the composition was 1.3 mmol.

[0312] [Example 2]

[0313] Adhesive composition C-2 was obtained in the same manner as in Example 1 except that 12 parts by mass of the graft polymer (P-2) produced in Synthesis Example 2 and 88 parts by mass of polypropylene (the same polymer as the matrix polymer used in Synthesis Example 2) were used.

[0314] The MFR (190°C, 2.16 kg load) of the obtained adhesive composition C-2 was 0.6 g / 10 min and the density was 0.893 g / cm 3 The amount of carbodiimide groups in each 100 g of the composition was 0.8 mmol.

[0315] [Example 3]

[0316] Adhesive composition C-3 was obtained in the same manner as in Example 1 except that 12 parts by mass of the graft polymer (P-3) produced in Synthesis Example 3 and 88 parts by mass of LLDPE (the same polymer as the matrix polymer used in Synthesis Example 1) were used.

[0317] The MFR (190°C, 2.16 kg load) of the obtained adhesive composition C-3 was 2.93 g / 10 min, and the density was 0.903 g / cm 3 The amount of carbodiimide groups in each 100 g of the composition was 1.3 mmol.

[0318] [Example 4]

[0319] Adhesive composition C-4 was obtained in the same manner as in Example 1 except that 10 parts by mass of the graft polymer (P-4) produced in Synthesis Example 4 and 90 parts by mass of LLDPE (the same polymer as the matrix polymer used in Synthesis Example 1) were used.

[0320] The MFR (190°C, 2.16 kg load) of the obtained adhesive composition C-4 was 3.1 g / 10 min and the density was 0.902 g / cm 3 The amount of carbodiimide groups in each 100 g of the composition was 1.3 mmol.

[0321] [Example 5]

[0322] Adhesive composition C-5 was obtained in the same manner as in Example 1 except that 16 parts by mass of the graft polymer (P-5) produced in Synthesis Example 5 and 84 parts by mass of LLDPE (the same polymer as the matrix polymer used in Synthesis Example 1) were used.

[0323] The MFR (190°C, 2.16 kg load) of the obtained adhesive composition C-5 was 3.5 g / 10 min and the density was 0.902 g / cm 3 The amount of carbodiimide groups in each 100 g of the composition was 1.3 mmol.

[0324] [Example 6]

[0325] Adhesive composition C-6 was obtained in the same manner as in Example 1 except that 17 parts by mass of the graft polymer (P-6) produced in Synthesis Example 6 and 83 parts by mass of LLDPE (the same polymer as the matrix polymer used in Synthesis Example 1) were used.

[0326] The MFR (190°C, 2.16 kg load) of the obtained adhesive composition C-6 was 2.73 g / 10 min and the density was 0.907 g / cm 3 The amount of carbodiimide groups in each 100 g of the composition was 1.3 mmol.

[0327] [Example 7]

[0328] Adhesive composition C-7 was obtained in the same manner as in Example 1 except that 12 parts by mass of the graft polymer (P-7) produced in Synthesis Example 7 and 88 parts by mass of LLDPE (the same polymer as the matrix polymer used in Synthesis Example 1) were used.

[0329] The density of the obtained adhesive composition C-7 was 0.903 g / cm 3 The amount of carbodiimide groups in each 100 g of the composition was 1.3 mmol.

[0330] [Example 8]

[0331] Adhesive composition C-8 was obtained in the same manner as in Example 1 except that 21 parts by mass of the graft polymer (P-8) produced in Synthesis Example 8 and 79 parts by mass of LLDPE (the same polymer as the matrix polymer used in Synthesis Example 1) were used.

[0332] The density of the obtained adhesive composition C-8 was 0.904 g / cm 3 The amount of carbodiimide groups in each 100 g of the composition was 1.3 mmol.

[0333] [Example 9]

[0334] Adhesive composition C-9 was obtained in the same manner as in Example 1 except that 12 parts by mass of the graft polymer (P-9) produced in Synthesis Example 9 and 88 parts by mass of polypropylene (the same polymer as the matrix polymer used in Synthesis Example 2) were used.

[0335] The MFR (190°C, 2.16 kg load) of the obtained adhesive composition C-9 was 1.0 g / 10 min and the density was 0.893 g / cm 3 The amount of carbodiimide groups in each 100 g of the composition was 0.8 mmol.

[0336] [Example 10]

[0337] Adhesive composition C-10 was obtained in the same manner as in Example 1 except that 14 parts by mass of the graft polymer (P-10) produced in Synthesis Example 10 and 86 parts by mass of polypropylene (the same polymer as the matrix polymer used in Synthesis Example 2) were used.

[0338] The MFR (190°C, 2.16 kg load) of the obtained adhesive composition C-10 was 1.8 g / 10 min and the density was 0.892 g / cm 3 The amount of carbodiimide groups in each 100 g of the composition was 0.8 mmol.

[0339] [Example 11]

[0340] Adhesive composition C-11 was obtained in the same manner as in Example 1 except that 13 parts by mass of the graft polymer (P-11) produced in Synthesis Example 11 and 87 parts by mass of polypropylene (the same polymer as the matrix polymer used in Synthesis Example 2) were used.

[0341] The MFR (190°C, 2.16 kg load) of the obtained adhesive composition C-11 was 2.0 g / 10 min and the density was 0.892 g / cm 3 The amount of carbodiimide groups in each 100 g of the composition was 0.8 mmol.

[0342] [Example 12]

[0343] Adhesive composition C-12 was obtained in the same manner as in Example 1 except that 13 parts by mass of the graft polymer (P-12) produced in Synthesis Example 12 and 87 parts by mass of polypropylene (the same polymer as the matrix polymer used in Synthesis Example 2) were used.

[0344] The density of the obtained adhesive composition C-12 was 0.893 g / cm 3 The amount of carbodiimide groups in each 100 g of the composition was 0.8 mmol.

[0345] [Example 13]

[0346] Adhesive composition C-13 was obtained in the same manner as in Example 1 except that 13 parts by mass of the graft polymer (P-3) produced in Synthesis Example 13 and 87 parts by mass of polypropylene (the same polymer as the matrix polymer used in Synthesis Example 2) were used.

[0347] The density of the obtained adhesive composition C-13 was 0.892 g / cm 3 The amount of carbodiimide groups in each 100 g of the composition was 0.8 mmol.

[0348] [Example 14]

[0349] Adhesive composition C-14 was obtained in the same manner as in Example 1 except that 15 parts by mass of the graft polymer (P-14) produced in Synthesis Example 14 and 85 parts by mass of LLDPE (the same polymer as the matrix polymer used in Synthesis Example 1) were used.

[0350] The density of the obtained adhesive composition C-14 was 0.903 g / cm 3 The amount of carbodiimide groups in each 100 g of the composition was 1.3 mmol.

[0351] [Example 15]

[0352] Adhesive composition C-15 was obtained in the same manner as in Example 1 except that 9 parts by mass of the graft polymer (P-15) produced in Synthesis Example 15 and 91 parts by mass of polypropylene (the same polymer as the matrix polymer used in Synthesis Example 2) were used.

[0353] The density of the obtained adhesive composition C-15 was 0.892 g / cm 3 The amount of carbodiimide groups in each 100 g of the composition was 0.8 mmol.

[0354] [Example 16]

[0355] Adhesive composition C-16 was obtained in the same manner as in Example 1 except that 12 parts by mass of the graft polymer (P-19) produced in Synthesis Example 19 and 88 parts by mass of polypropylene (the same polymer as the matrix polymer used in Synthesis Example 2) were used.

[0356] The MFR (190°C, 2.16 kg load) of the obtained adhesive composition C-16 was 1.3 g / 10 min and the density was 0.893 g / cm 3 The amount of carbodiimide groups in each 100 g of the composition was 0.3 mmol.

[0357] [Example 17]

[0358] Adhesive composition C-17 was obtained in the same manner as in Example 1 except that 12 parts by mass of the graft polymer (P-21) produced in Synthesis Example 21 and 88 parts by mass of polypropylene (the same polymer as the matrix polymer used in Synthesis Example 2) were used.

[0359] The MFR (190°C, 2.16 kg load) of the obtained adhesive composition C-17 was 1.6 g / 10 min, and the density was 0.893 g / cm 3 The amount of carbodiimide groups in each 100 g of the composition was 0.3 mmol.

[0360] [Example 18]

[0361] Adhesive composition C-18 was obtained in the same manner as in Example 1 except that 25 parts by mass of the graft polymer (P-1) produced in Synthesis Example 1 and 75 parts by mass of LLDPE (the same polymer as the matrix polymer used in Synthesis Example 1) were used.

[0362] The MFR (190°C, 2.16 kg load) of the obtained adhesive composition C-18 was 1.0 g / 10 min and the density was 0.920 g / cm 3 The amount of carbodiimide groups in each 100 g of the composition was 2.9 mmol.

[0363] [Example 19]

[0364] Adhesive composition C-19 was obtained in the same manner as in Example 1 except that 50 parts by mass of the graft polymer (P-1) produced in Synthesis Example 1 and 50 parts by mass of LLDPE (the same polymer as the matrix polymer used in Synthesis Example 1) were used.

[0365] The MFR (190°C, 2.16 kg load) of the obtained adhesive composition C-19 was 0.2 g / 10 min and the density was 0.918 g / cm 3 The amount of carbodiimide groups in each 100 g of the composition was 5.9 mmol.

[0366] [Comparative Example 1]

[0367] Adhesive composition CC-1 was obtained in the same manner as in Example 1 except that 10 parts by mass of the graft polymer (P-16) produced in Synthesis Example 16 and 90 parts by mass of LLDPE (the same polymer as the matrix polymer used in Synthesis Example 1) were used.

[0368] The MFR (190°C, 2.16 kg load) of the obtained adhesive composition CC-1 was 3.2 g / 10 min and the density was 0.902 g / cm 3 The amount of carbodiimide groups in each 100 g of the composition was 1.3 mmol, and the composition did not contain a graft-modified product obtained by graft-modifying a carbodiimide monomer.

[0369] [Comparative Example 2]

[0370] Lotader (manufactured by ARKEMA, density 0.940 g / cm 3 , the epoxy group content per 100 g of the composition is 56 mmol, and does not contain a graft-modified product obtained by grafting modification of a carbodiimide monomer) as an adhesive composition CC-2.

[0371] [Comparative Example 3]

[0372] Adhesive composition CC-3 was obtained in the same manner as in Example 1 except that 12 parts by mass of the graft polymer (P-17) produced in Synthesis Example 17 and 88 parts by mass of polypropylene (the same polymer as the matrix polymer used in Synthesis Example 2) were used.

[0373] The MFR (190°C, 2.16 kg load) of the obtained adhesive composition CC-3 was 1.9 g / 10 min and the density was 0.892 g / cm 3 The epoxy group content of each 100 g of the composition was 0.8 mmol, and the composition did not contain a graft-modified product obtained by graft-modifying a carbodiimide monomer.

[0374] [Comparative Example 4]

[0375] Adhesive composition CC-4 was obtained in the same manner as in Example 1 except that 100 parts by mass of LLDPE (the same polymer as the matrix polymer used in Synthesis Example 1) was used.

[0376] The MFR (190°C, 2.16 kg load) of the obtained adhesive composition CC-4 was 3.7 g / 10 min and the density was 0.919 g / cm 3 , the amount of carbodiimide groups in each 100 g of the composition is 0 mmol.

[0377] [Comparative Example 5]

[0378] Adhesive composition CC-5 was obtained in the same manner as in Example 1 except that 100 parts by mass of polypropylene (the same polymer as the matrix polymer used in Synthesis Example 2) was used.

[0379] The MFR (190°C, 2.16 kg load) of the obtained adhesive composition CC-5 was 3.7 g / 10 min and the density was 0.893 g / cm 3 , the amount of carbodiimide groups in each 100 g of the composition is 0 mmol.

[0380] <Adhesion Evaluation>

[0381] ·Preparation of compressed tablets

[0382] The adhesive compositions obtained in Examples 1 to 19 and Comparative Examples 1 to 5 were press-molded at a temperature of 180°C, a pressure of 4 MPa, a preheating time of 5 minutes, and a pressing time of 3 minutes, and then rapidly cooled using a press-molding machine set at 20°C to produce pressed sheets with a thickness of 500 μm, a length of 80 mm, and a width of 80 mm.

[0383] ·Production of polyethylene terephthalate laminates

[0384] As the base material layer, a polyethylene terephthalate (PET) sheet (product name: Lumirror T60, manufactured by Toray Industries, Inc.) having a thickness of 50 μm, a length of 80 mm, and a width of 80 mm was used.

[0385] The PET sheet, the above-mentioned pressed sheet and the PET sheet are stacked in sequence, and the stacked body is clamped with Teflon (registered trademark) sheets and heat-sealed for 3 seconds using a heat sealer with a press plate (lower) temperature set to 200°C and a press plate (upper) temperature set to 200°C or 230°C, to produce a polyethylene terephthalate laminate consisting of three layers.

[0386] Peel test

[0387] The polyethylene terephthalate laminate was subjected to T-type peeling of the upper PET sheet (PET sheet on the press plate (upper) side) and the pressed sheet under the conditions of a peeling environment temperature of 23°C, a peeling speed of 300 mm / min, and a peeling width of 15 mm, thereby measuring the peel strength of the PET sheet and the pressed sheet. The results are shown in Tables 2 and 3.

[0388] It should be noted that the situation in which the PET sheet itself breaks rather than at the interface between the PET sheet and the pressed sheet due to strong adhesive force is expressed as "PET resin breakage".

[0389] Table 2 describes the ethylene-based adhesive composition, and Table 3 describes the propylene-based adhesive composition.

[0390] [Table 2]

[0391]

[0392] [Table 3]

[0393]

[0394] <Adhesion Evaluation>

[0395] ·Preparation of compressed tablets

[0396] The adhesive compositions obtained in Examples 2, 5, 11 and Comparative Examples 2 to 3 were press-molded at a temperature of 180°C, a pressure of 4 MPa, a preheating time of 5 minutes, and a pressing time of 3 minutes, and then rapidly cooled using a press-molding machine set at 20°C to produce pressed sheets with a thickness of 500 μm, a length of 80 mm, and a width of 80 mm.

[0397] Preparation of biodegradable polymer laminates

[0398] As the substrate layer, a polylactic acid (PLA) sheet (product name: Ingeo, manufactured by NatureWorks, thermal degradation temperature Td measured by thermogravimetric analysis (TGA): 262° C.) having a thickness of 100 μm, a length of 80 mm, and a width of 80 mm was used.

[0399] The PLA sheet, the above-mentioned pressed sheet and the PLA sheet are stacked in sequence, and the stacked body is clamped with Teflon (registered trademark) sheets and heat-sealed for 3 seconds using a heat sealer with the upper and lower temperatures of the pressing plates set to 170°C or 230°C to prepare a biodegradable polymer stack consisting of three layers.

[0400] Peel test

[0401] For the biodegradable polymer laminate, the upper PLA sheet (PLA sheet on the press plate (upper) side) and the pressed sheet were subjected to T-type peeling under the conditions of a peeling environment temperature of 23°C, a peeling speed of 300 mm / min, and a peeling width of 15 mm, thereby measuring the peel strength of the PLA sheet and the pressed sheet. The results are shown in Table 4.

[0402] It should be noted that the situation where the PLA sheet itself breaks rather than at the interface between the PLA sheet and the pressed sheet due to strong adhesion is referred to as "resin breakage".

[0403] [Table 4]

[0404] < / mfr>

Claims

1. A laminate, characterized in that: have: a layer (A) comprising polyethylene terephthalate or a biodegradable polymer; and an adhesive layer (B) comprising an adhesive composition, At least a portion of the adhesive layer (B) is in contact with the layer (A), The adhesive composition satisfies the following requirements (i) to (iii): (i) a graft-modified product obtained by graft-modifying at least one base polymer selected from polyolefins with a carbodiimide monomer having a carbodiimide group and a polymerizable double bond; (ii) containing 0.1 to 50 mmol of carbodiimide groups per 100 g of the adhesive composition; (iii) Density: 0.870 to 0.940 g / cm 3 .

2. The laminate according to claim 1, wherein: The carbodiimide monomer is at least one monomer selected from the group consisting of a compound represented by the following formula (1) and a compound represented by the following formula (2), In formula (1), R1 is a hydrogen atom or a methyl group, and R2 is an alkyl group or an aryl group which may have a substituent. In formula (2), R3 is a hydrogen atom or a methyl group, R4 is an alkyl group or an aryl group which may have a substituent, and m is an integer of 2 or more.

3. The laminate according to claim 1 or 2, characterized in that: The layer (A) is composed of polyethylene terephthalate.

4. The laminate according to claim 1 or 2, wherein: The layer (A) contains polylactic acid.

5. The laminate according to claim 1 or 2, wherein: The layer (A) is composed of a biodegradable polymer.

6. The laminate according to claim 1 or 2, wherein: The layer (A) consists of polylactic acid.

7. The laminate according to claim 1 or 2, wherein: The laminate is obtained by lamination molding, co-extrusion molding, blow molding or co-injection molding.

8. A method for manufacturing a laminate, characterized in that: The laminate comprises: a layer (A) containing polyethylene terephthalate or a biodegradable polymer; and an adhesive layer (B) containing an adhesive composition, wherein at least a portion of the adhesive layer (B) is in contact with the layer (A). The manufacturing method comprises step 1 of co-extrusion molding, lamination molding, blow molding or co-injection molding of a resin composition containing polyethylene terephthalate or a biodegradable polymer and the adhesive composition, The adhesive composition satisfies the following requirements (i) to (iii): (i) a graft-modified product obtained by graft-modifying at least one base polymer selected from polyolefins with a carbodiimide monomer having a carbodiimide group and a polymerizable double bond; (ii) containing 0.1 to 50 mmol of carbodiimide groups per 100 g of the adhesive composition; (iii) Density: 0.870 to 0.940 g / cm 3 .

9. The method for manufacturing a laminate according to claim 8, wherein: When the layer (A) is a layer containing a biodegradable polymer, the step 1 is performed at a temperature lower than the thermal degradation temperature of the biodegradable polymer.

10. The method for producing a laminate according to claim 8 or 9, wherein: The carbodiimide monomer is at least one monomer selected from the group consisting of a compound represented by the following formula (1) and a compound represented by the following formula (2), In formula (1), R1 is a hydrogen atom or a methyl group, and R2 is an alkyl group or an aryl group which may have a substituent. In formula (2), R3 is a hydrogen atom or a methyl group, R4 is an alkyl group or an aryl group which may have a substituent, and m is an integer of 2 or more.

11. An adhesive composition, characterized in that: The following requirements (i) to (iii) must be met: (i) a graft-modified product obtained by graft-modifying at least one base polymer selected from polyolefins with a carbodiimide monomer having a carbodiimide group and a polymerizable double bond; (ii) containing 0.1 to 50 mmol of carbodiimide groups per 100 g of the adhesive composition; (iii) Density: 0.870 to 0.940 g / cm 3 .

12. The adhesive composition according to claim 11, characterized in that: The carbodiimide monomer is at least one monomer selected from the group consisting of a compound represented by the following formula (1) and a compound represented by the following formula (2), In formula (1), R1 is a hydrogen atom or a methyl group, and R2 is an alkyl group or an aryl group which may have a substituent. In formula (2), R3 is a hydrogen atom or a methyl group, R4 is an alkyl group or an aryl group which may have a substituent, and m is an integer of 2 or more.

Citation Information

Patent Citations

  • Modified polyolefin

    JP1994145260A

  • Adhesive and laminates made by using the same

    CN101278026A

  • Method used for improving water resistance and flexibility of polyacrylic acid film with MPEGPLA and poly trimethylene carbonate

    CN106987136A

  • Graft-modified product, adhesive, olefin resin composition, and laminate

    CN116438076A

  • Carbodiimide compound and polymer thereof, gelatinous composition, ionic conductive composition, electrochemical element, and surface-modified substrate

    JP2005048127A