Glass plate manufacturing method, glass plate, and glass plate package
By controlling the distribution of the median crack depth of the scribe lines during the glass manufacturing process, the problem of glass plate breakage when the bundle is loaded in a longitudinal orientation is solved, achieving stable breakage and precise cutting of the glass plate and reducing the risk of breakage caused by scribe lines.
Patent Information
- Application Number
- CN202380030051.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-05-10
- Filing Date
- 2023-04-26
- Publication Date
- 2024-11-08
AI Technical Summary
During the manufacturing process of glass plates, scratches remain on both ends of the glass plates bundled in the width direction due to the engraving lines. This makes them prone to breakage during handling, especially when they are loaded longitudinally at the bottom of a pallet.
In the manufacturing process of glass plates, a scribing process is used to form scribing lines along the vertical direction. In the breaking process, the depth of the median crack of the scribing lines is controlled to make the maximum depth of the median crack at the bottom of the scribing lines shallower, thereby reducing the risk of end face breakage during breaking. The depth distribution of the scribing marks is controlled in the bundle to prevent breakage.
It effectively prevents glass plates from breaking when loaded onto a pallet in a longitudinal orientation, reduces the occurrence of poor cutting, improves the breaking accuracy and stability of the glass plates, and reduces the amount of glass powder generated.
Smart Images

Figure CN118922386A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for producing a glass plate, a glass plate, and a glass plate package. Background Art
[0002] As is well known, a glass plate is used as a glass substrate or a cover glass in displays such as liquid crystal displays and organic EL displays. As a method for manufacturing a glass plate, a method using a down-draw method represented by an overflow down-draw method, a slit down-draw method, and a re-draw method is widely used. As an example of a method for manufacturing a glass plate using an overflow down-draw method, the following method for manufacturing a glass plate can be cited.
[0003] In the method for producing a glass sheet, as disclosed in Patent Document 1, a forming step of forming a glass ribbon and a first cutting step (X-cutting step) of cutting a glass sheet from the formed glass ribbon by scoring and cutting are performed.
[0004] In the forming process, molten glass is supplied to the overflow trough provided at the top of the wedge-shaped forming body and overflowed. The overflowing molten glass flows down along the side portions of the forming body and then fuses and integrates at the lower end portion of the forming body. Thus, a plate-shaped glass ribbon is formed. After that, the formed glass ribbon is pulled downward while being clamped from both sides by roller pairs arranged in multiple stages from top to bottom. Ear portions having a thickness greater than that of the central portion in the width direction are formed at both ends of the glass ribbon obtained in this way.
[0005] The scoring and cutting performed in the first cutting step forms a scoring line along the width direction on the main surface of the glass ribbon conveyed downward, bends the area around the scoring line to apply bending stress, and cuts the glass ribbon along the scoring line, thereby cutting a rectangular glass plate from the glass ribbon.
[0006] Next, in the method for manufacturing a glass plate, as disclosed in Patent Document 2, a second cutting step (Y cutting step) is performed to remove the ear portions formed at both ends in the width direction of the glass plate by scoring and cutting.
[0007] The scoring and cutting performed in the second cutting step forms a scoring line along the vertical direction on the main surface of the end side in the width direction of the glass sheet held in a vertical posture. Then, the peripheral area of the scoring line is bent to apply bending stress and the glass ribbon is cut along the scoring line. The scoring and cutting is performed separately on one end side and the other end side in the width direction of the glass sheet. As a result, a glass sheet without ears at both ends in the width direction is obtained.
[0008] Next, in the method for manufacturing a glass plate, a step (packing step) of loading the glass plate with the ears removed on a pallet and packing the glass plate is performed as disclosed in Patent Document 3. Through this packing step, a glass plate package is formed in which a plurality of glass plates are packed in a vertical posture on a pallet. The glass plate package is transferred to the next step or stored until the next step is performed.
[0009] Prior art literature
[0010] Patent Literature
[0011] Patent Document 1: Japanese Patent Application Publication No. 2017-202958
[0012] Patent Document 2: Japanese Patent Application Publication No. 2017-226549
[0013] Patent Document 3: Japanese Patent Application Publication No. 2020-75752 Summary of the invention
[0014] Problems to be solved by the invention
[0015] In the above-mentioned conventional method for manufacturing glass plates, the glass plates packed in the glass plate package have scratches on both end faces in the width direction thereof due to the formation of the score lines. Therefore, when the glass plate package is transported, for example, there is a possibility that the glass plates may be cracked due to impact or excessive stress. Such cracks are particularly likely to occur at the lower part of the glass plates loaded on the pallet in a vertical position.
[0016] The present invention has been made in view of the above-mentioned circumstances, and a technical object of the present invention is to prevent breakage of a glass plate loaded on a tray in a vertical posture.
[0017] Solutions to Solve Problems
[0018] The present invention is a method for manufacturing a glass plate for solving the above-mentioned problems, including a cutting process for removing the end portions of the glass plate in the width direction while the glass plate is supported in a longitudinal posture. The method for manufacturing the glass plate is characterized in that the cutting process includes: a scoring process for forming a scoring line including a median crack on the glass plate along the up and down directions using a scoring tool; and a breaking process for applying bending stress to the glass plate with the scoring line formed thereon to break it, wherein in the scoring process, the scoring line is formed in such a way that the maximum depth of the median crack at the lower portion of the scoring line is shallower than the maximum depth of the median crack at the upper portion or the middle portion of the scoring line.
[0019] Scratches caused by the scoring lines remain on the end surface of the glass plate after the breaking process, and the scoring lines include a median crack. The deeper the maximum depth of the median crack at the lower part of the end surface of the glass plate is, the easier it is to break. In the present invention, as described above, by making the maximum depth of the median crack at the lower part of the scoring line shallower, the maximum depth of the median crack at the lower part of the end surface of the obtained glass plate can be made shallower. Thus, the lower part of the glass plate loaded on the tray in a vertical posture can be prevented from being damaged.
[0020] Furthermore, by making the maximum depth of the median crack at the upper or middle portion of the scribed line deeper than the maximum depth of the median crack at the lower portion of the scribed line, the median crack at the upper or middle portion of the scribed line becomes the starting point and the crack progresses in the breaking process, so that the bending stress applied to the glass sheet can be minimized. Thus, the amount of glass powder generated from the upper or middle portion of the scribed line can be minimized in the breaking process.
[0021] In the method for manufacturing a glass sheet of the present invention, the maximum depth of the median crack in the middle portion of the scribed line may be shallower than the maximum depth of the median crack in the upper portion of the scribed line.
[0022] According to this structure, the crack can be stably developed from the upper part of the scribed line toward the middle part and the lower part below in the breaking process. Thus, the occurrence of poor cutting in the cutting process can be prevented. In addition, even if the glass plate is warped, the glass plate can be broken without causing poor cutting.
[0023] In the method for manufacturing a glass sheet of the present invention, the maximum depth of the median crack in the upper portion of the scribed line may be shallower than the maximum depth of the median crack in the middle portion of the scribed line.
[0024] According to this structure, the crack can be stably advanced upward and downward from the middle of the score line in the breaking process. As a result, the glass plate can be broken with good accuracy. In addition, the maximum depth of the median crack above the score line is shallow, so when the glass plate after the cutting process is transported, even if the upper part of the glass plate is held by a holding mechanism such as a chuck, the upper part can be prevented from being damaged.
[0025] The present invention is a glass plate package for solving the above-mentioned problems, comprising rectangular glass plates and a tray for stacking the glass plates in a vertical posture, wherein the glass plates have end faces extending in the vertical direction at the ends in the width direction, the end faces are fractured faces having a scratch mark including a median crack, and the maximum depth of the median crack at the lower portion of the end face is shallower than the maximum depth of the median crack at the upper portion or the middle portion of the end face.
[0026] The deeper the maximum depth of the median crack at the lower part of the end face of the glass plate, the easier it is to break. In the present invention, as described above, by making the maximum depth of the median crack at the lower part of the end face extending in the vertical direction shallower, it is possible to prevent the lower part of the glass plate loaded on the tray in a vertical posture from being damaged.
[0027] In the glass plate package of the present invention, the maximum depth of the median crack in the middle portion of the end surface may be shallower than the maximum depth of the median crack in the upper portion of the end surface.
[0028] In the glass plate package of the present invention, the maximum depth of the median crack in the upper portion of the end surface may be shallower than the maximum depth of the median crack in the middle portion of the end surface.
[0029] According to this configuration, when manufacturing a glass plate package, even when the upper portion of the glass plate is held by a holding mechanism such as a chuck, it is possible to prevent the upper portion of the glass plate from being damaged by impact or the like.
[0030] The present invention is a glass plate for solving the above-mentioned problems, which is in a rectangular shape. The glass plate is characterized in that the glass plate has an end face extending in the pulling direction, and the end face is a broken surface having a scratch mark including a median crack, and the maximum depth of the median crack at one end of the end face in the pulling direction is shallower than the maximum depth of the median crack at the other end or middle part of the end face in the pulling direction.
[0031] According to this configuration, by placing the glass plate on the tray so that one end of the end surface having the shallowest maximum depth of the median crack is located below the glass plate, breakage of the lower portion of the glass plate can be prevented.
[0032] Effects of the Invention
[0033] According to the present invention, it is possible to prevent breakage of a glass plate placed on a tray in a vertical posture. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 1 is a flowchart showing a method for manufacturing a glass plate.
[0035] Figure 2 This is a perspective view showing a part of the method for manufacturing a glass plate.
[0036] Figure 3 This is a side view showing the second cutting step in the method for producing a glass sheet.
[0037] Figure 4 It is a perspective view showing an example of a glass plate.
[0038] Figure 5 is shown and Figure 4 Graph showing the relationship between the position of the score line and the median crack depth for a glass plate.
[0039] Figure 6 It is a perspective view showing another example of the glass plate.
[0040] Figure 7 is shown and Figure 6 Graph showing the relationship between the position of the score line and the median crack depth for a glass plate.
[0041] Figure 8 It is a perspective view showing another example of the glass plate.
[0042] Fig. 9 is shown and Figure 8 Graph showing the relationship between the position of the score line and the median crack depth for a glass plate.
[0043] Fig.10 This is a perspective view showing a packing step in the method for producing a glass plate.
[0044] Fig.11 It is a perspective view of a glass plate package. DETAILED DESCRIPTION
[0045] Hereinafter, embodiments of the present invention will be described with reference to the drawings. Figures 1 to 11 One embodiment of the glass plate and the method for producing the same, and the glass plate package of the present invention is described.
[0046] like Figure 1 As shown, the method for manufacturing a glass sheet of the present invention mainly includes a forming step S1 , a first cutting step S2 , a second cutting step S3 , and a packing step S4 .
[0047] The forming step S1 is a step of forming a glass ribbon GR from molten glass GM. Figure 2 As shown, in the forming step S1, molten glass GM is supplied to the overflow channel 1a at the top of the wedge-shaped forming body 1 and overflowed. The overflowed molten glass GM flows down along the side surface of the forming body 1, and then is integrated at the lower end of the forming body 1.
[0048] Thus, a plate-shaped glass ribbon GR is formed. After that, the formed glass ribbon GR is pulled downward while being clamped from both the front and back sides by a pair of rollers (not shown) arranged in multiple stages up and down. A pair of cooling rollers is arranged at the top of the pair of rollers arranged in multiple stages up and down. In this embodiment, the pulling direction Y in the forming step S1 is set to be along the vertical direction.
[0049] The formed glass ribbon GR has a first main surface 2 and a second main surface 3. In the present embodiment, the glass ribbon GR in which the first main surface 2 is a non-guaranteed surface and the second main surface 3 is a guaranteed surface is exemplified. Here, the guaranteed surface is a surface formed by the supply element and the like in the glass sheet finally obtained from the glass ribbon GR and is a surface whose surface properties are guaranteed, while the non-guaranteed surface is a surface whose surface properties may not be guaranteed to the extent of the guaranteed surface.
[0050] The glass ribbon GR has ear portions formed at both widthwise ends Ga. The thickness of the widthwise center portion of the glass ribbon GR is 1000 μm or less, preferably 700 μm or less, more preferably 500 μm or less, and its lower limit is, for example, 50 μm or more.
[0051] The first cutting step S2 is a step of cutting out a first glass sheet G1 from the glass ribbon GR formed in the forming step S1 by scoring and cutting along the width direction X. The first cutting step S2 includes a scoring step of forming a score line SL1 in the glass ribbon GR using a scoring tool, and a breaking step of applying bending stress to the glass ribbon GR formed with the score line SL1 to break it.
[0052] In the scribing step, the scribing wheel 4 as a scribing tool moves from a position indicated by a dashed line to a position indicated by a solid line while being pressed against the surface of the glass ribbon GR, thereby forming a scribing line SL1 along the width direction X on the first main surface 2 of the glass ribbon GR.
[0053] At this time, the formation region of the scribe line SL1 is supported by a support member (not shown) from the second main surface 3. A gripping mechanism 5 is disposed below the scribing wheel 4 and the support member, but the gripping mechanism 5 does not operate during the scribing step.
[0054] After the scoring line SL1 is formed, the scoring wheel 4 and the supporting member are retracted to the retracted position. In the example shown in the figure, the scoring line SL1 does not reach both ends of the glass ribbon GR in the width direction, but may reach the both ends.
[0055] Next, in the breaking step, the holding mechanism 5 holding the lower end of the glass ribbon GR is rotated in the direction of arrow a while the breaking member 6 supports the formation area of the score line SL1 from the second main surface 3 side, thereby applying bending stress to the score line SL1. As a result, the glass ribbon GR can be broken along the score line SL1. The first glass sheet G1 having a rectangular shape and ears at both ends Ga in the width direction is cut out by the scoring and cutting based on the breaking.
[0056] The first glass sheet G1 is conveyed to a position where the second cutting step S3 can be performed by the conveying device 7 (conveying step). The conveying device 7 is configured to convey the first glass sheet G1 while holding it in a vertical posture. The conveying device 7 includes a holding portion 7a that holds the upper portion of the first glass sheet G1.
[0057] The holding part 7a is composed of, for example, a chuck for holding the first glass plate G1, but is not limited thereto and may be composed of a holding mechanism such as a suction pad. The holding part 7a is configured to be movable in a predetermined direction by a guide rail, etc. The holding part 7a holds only the upper part of the first glass plate G1 and transports the first glass plate G1 in a vertical posture in a suspended state.
[0058] The second cutting step S3 is a step of cutting the width direction end portions Ga of the first glass sheet G1. That is, in the second cutting step S3, the width direction end portions Ga of the first glass sheet G1 are removed by scoring and cutting along the longitudinal direction while the first glass sheet G1 is supported in a longitudinal posture by the conveying device 7, thereby cutting out the second glass sheet G2.
[0059] The second cutting step S3 includes a scribing step of forming a scribed line SL2 including a median crack MC on the first glass sheet G1 using a scribing tool, and a breaking step of applying bending stress to the first glass sheet G1 on which the scribed line SL2 is formed to break the first glass sheet G1.
[0060] In the scribing step, a portion of the second main surface 3 of the first glass plate G1 is supported by two supporting members (not shown). In this state, two scribing wheels 8 as scribing tools form scribing lines SL2 at predetermined positions (slightly inward in the width direction from the ears) at both ends Ga in the width direction of the first glass plate G1.
[0061] The two scoring wheels 8 move from the position indicated by the dashed line to the position indicated by the solid line while pressing the predetermined positions of the widthwise ends Ga of the first main surface 2 of the first glass plate G1, thereby forming two scoring lines SL2 along the longitudinal direction on the first main surface 2 of the first glass plate G1.
[0062] The scoring line SL2 is formed as a straight line along the vertical direction in a manner corresponding to the pulling direction Y. The scoring line SL2 has a starting end SL2a and an ending end SL2b. In the present embodiment, the starting end SL2a of the scoring line SL2 is located below the upper end of the first glass plate G1, but it is not limited to this. The starting end SL2a of the scoring line SL2 can also be set at the upper end of the first glass plate G1. The distance from the upper end surface of the first glass plate G1 to the starting end SL2a of the scoring line SL2 is, for example, 10 mm to 300 mm.
[0063] The terminal end SL2b of the scribed line SL2 is located above the lower end of the first glass plate G1, but it is not limited to this. The terminal end SL2b of the scribed line SL2 can also be set at the lower end of the first glass plate G1. The distance from the lower end surface of the first glass plate G1 to the terminal end SL2a of the scribed line SL2 is, for example, 10 mm to 300 mm. In this case, the two scribed lines SL2 can be formed at the same time or separately over time. In addition, the starting end SL2a and the terminal end SL2b of the scribed line SL2 can also be in opposite positions up and down.
[0064] Hereinafter, the upper portion of the score line SL2 is indicated by reference numeral UP1, with the upper end portion (starting end portion SL2a) of the score line SL2 as the starting point and the position of the first glass plate G1 located 25% downward from the upper end surface as the end point. In addition, the lower portion of the score line SL2 is indicated by reference numeral BP1, with the lower end portion (terminating end portion SL2b) of the score line SL2 as the starting point and the position of the first glass plate G1 located 25% upward from the lower end surface as the end point. In addition, the portion between the upper portion UP1 and the lower portion BP1 of the score line SL2 is referred to as the middle portion of the score line SL2 and is indicated by reference numeral MP1. It should be noted that the position located 25% downward from the upper end surface means that the distance A is located at a position located downward from the upper end surface when the value obtained by multiplying the length from the upper end surface to the lower end surface of the first glass plate G1 by 0.25 is defined as the distance A. Furthermore, the phrase “located 25% upward from the lower end surface” means located at a position the distance A above the lower end surface.
[0065] like Figure 3 As shown, the scribe line SL2 forms a plastic deformation layer PDL and a median crack MC on the first glass plate G1. The plastic deformation layer PDL is formed by pressing the first main surface 2 of the first glass plate G1 by the scribe wheel 8. The median crack MC is integrally formed with a first crack MCa called a rib mark and a second crack MCb formed at a position deeper than the first crack MCa. In the present embodiment, the depth (D1+D2) obtained by adding the depth D1 of the first crack MCa and the depth D1 of the second crack MCb is referred to as the "depth of the median crack".
[0066] In the scribing step of the present embodiment, the pressing force of the scribing wheel 8 on the first main surface 2 of the first glass sheet G1 is adjusted so that the scribing line SL2 is formed so that the depth of the median crack MC varies along the longitudinal direction (the pulling direction Y).
[0067] like Figure 2As shown, in the breaking step, the first glass sheet G1 is broken along the two score lines SL2 while being supported on the second main surface 3 side by two support members 9. In this case, the first glass sheet G1 is supported slightly closer to the center side in the width direction than the two score lines SL2 by the support members 9. In this state, both end portions Ga in the width direction of the first glass sheet G1 are pressed toward the back side (second main surface 3 side) from the first main surface 2 side by a pressing member (not shown), thereby breaking the first glass sheet G1.
[0068] By scoring and cutting based on the breakage at the two locations, the two end portions Ga in the width direction including the ears of the first glass plate G1 are removed. Thus, a second glass plate G2 without ears is obtained. In this case, the scoring and cutting at the two locations can be performed simultaneously or separately over time. The dimension of the width direction of the obtained second glass plate G2 is, for example, greater than 1500 mm, preferably greater than 2000 mm, and more preferably greater than 3000 mm. On the other hand, the upper limit can be, for example, less than 4000 mm. In addition, the dimension of the second glass plate G2 in the pulling direction is, for example, greater than 1300 mm, preferably greater than 2000 mm, and more preferably greater than 2500 mm. On the other hand, the upper limit can be, for example, less than 3600 mm.
[0069] It should be noted that the pulling direction of the second glass sheet G2 can be observed as a stripe pattern by, for example, adjusting the angle of the second glass sheet G2 in a dark room, irradiating light from a light source (e.g., a xenon lamp), and projecting the transmitted light onto a screen. Therefore, even in the state of the second glass sheet G2 after forming, the pulling direction Y during forming can be determined.
[0070] The second glass sheet G2 has an upper end surface ESU, a lower end surface ESB, and a pair of side end surfaces ESS newly formed by removing both ends Ga in the width direction of the first glass sheet G1. The upper end surface ESU and the lower end surface ESB of the second glass sheet G2 are long strip-shaped surfaces extending in the horizontal direction in the second glass sheet G2 in a vertical position. The side end surface ESS of the second glass sheet G2 is a long strip-shaped fracture surface extending in the vertical direction corresponding to the pulling direction Y. Scratches including the median crack MC formed by the second cutting step S3 (scratching step) remain on the side end surface ESS.
[0071] Hereinafter, the portion of the side end surface ESS in the range of 25% downward from the upper end surface ESU of the second glass sheet G2 (25% of the length from the upper end surface ESU to the lower end surface ESB) is referred to as the upper portion (end portion) of the side end surface ESS, and is indicated by the reference symbol UP2. In addition, the portion of the side end surface ESS in the range of 25% upward from the lower end surface ESB of the second glass sheet G2 is referred to as the lower portion (end portion) of the side end surface ESS, and is indicated by the reference symbol BP2. In addition, the portion between the upper portion UP2 and the lower portion BP2 of the side end surface ESS is referred to as the middle portion of the side end surface ESS, and is indicated by the reference symbol MP2.
[0072] The depth of the median crack MC of the scribed line SL2 formed on the first glass sheet G1 by the second cutting step S3 corresponds to the depth of the median crack of the scribed mark remaining on the side end surface ESS of the second glass sheet G2. Therefore, by measuring the depth of the median crack of the scribed mark remaining on the side end surface ESS of the second glass sheet G2 (the depth from the first main surface 2), the depth of the median crack MC related to the scribed line SL2 formed by the second cutting step S3 can be determined. The depth of the median crack is measured by observing the side end surface ESS of the second glass sheet G2 or the side end surface including both ends Ga in the width direction of the ear portion of the first glass sheet G1 using an electron microscope, for example. In the glass sheet package and the glass sheet of the present invention, the maximum depth of the median cracks in the upper part, the middle part, and the lower part is set to the maximum depth obtained from the depth distribution obtained by measuring the depth of the median crack at 100 mm intervals along the pulling direction. The depth of the median crack is measured by taking out a sample including the side end surface ESS of the second glass sheet G2 and observing the side end surface ESS with an electron microscope using the sample.
[0073] Below, refer to Figures 4 to 9 The relationship between the pattern of the median crack of the scratch remaining on the side end surface ESS of the second glass sheet G2 and the median crack MC of the scribe line SL2 will be described.
[0074] Figures 4 to 9 The second glass sheet G2 is formed by the scribe line SL2 having different patterns of the median crack MC. Figure 4 , Figure 6 as well as Figure 8 The middle part shows the median crack MC of the scratch SM remaining on the side end surface ESS of the second glass sheet G2.
[0075] exist Figure 4 , Figure 6 as well as Figure 8 In the figure, the upper end SMa of the scribe mark SM corresponds to the starting end SL2a of the scribe line SL2, and the lower end SMb of the scribe mark SM corresponds to the terminal end SL2b of the scribe line SL2.
[0076] Since the upper portion of the score mark SM is equivalent to the upper portion of the score line SL2, the same reference numeral UP1 is used. Since the lower portion of the score mark SM is equivalent to the lower portion of the score line SL2, the same reference numeral BP1 is used. Since the middle portion of the score mark SM is equivalent to the middle portion of the score line SL2, the same reference numeral MP1 is used. The upper portion UP1 of the score mark SM is included in the upper portion UP2 of the side end surface ESS of the second glass sheet G2. The lower portion BP1 of the score mark SM is included in the lower portion BP2 of the side end surface ESS, and the middle portion MP1 of the score mark SM is included in the middle portion MP2 of the side end surface ESS.
[0077] Figure 5 is shown for forming the Figure 4 Graph showing the relationship between the position of the scribe line SL2 of the second glass sheet G2 in the pulling direction Y and the depth of the median crack MC shown in FIG. Figure 7 Shown for forming the Figure 6 The relationship between the position of the scribe line SL2 of the second glass sheet G2 and the depth of the median crack MC is shown in FIG. Fig. 9 is shown for forming the Figure 8 Graph showing the relationship between the position of the scribe line SL2 of the second glass sheet G2 and the depth of the median crack MC shown in FIG. Figure 5 , Figure 7 as well as Fig. 9 The position of the illustrated scribe line SL2 corresponds to the position of the scribe mark SM in the pulling direction Y of the side end surface ESS of the second glass sheet G2.
[0078] like Figure 4 As shown, the depth (depth from the first main surface 2) of the median crack MC of the scratch remaining on the side end surface ESS of the second glass sheet G2 of the first embodiment gradually decreases as it moves from the upper part UP1 to the lower part BP1. The depth of the median crack MC is deepest at the upper end SMa of the scratch SM and shallowest at the lower end SMb of the scratch SM.
[0079] Therefore, the maximum depth of the median crack MC at the lower portion BP2 (one end of the end surface ESS in the plate pulling direction Y) of the side end surface ESS of the second glass sheet G2 is shallower than the maximum depth of the median crack MC at the upper portion UP2 of the side end surface ESS (the other end of the end surface ESS in the plate pulling direction Y). In addition, the maximum depth of the median crack MC at the lower portion BP2 of the side end surface ESS is shallower than the maximum depth of the median crack MC at the middle portion MP2 of the side end surface ESS. In addition, the maximum depth of the median crack MC at the middle portion MP2 of the side end surface ESS is shallower than the maximum depth of the median crack MC at the upper portion UP2 of the side end surface ESS.
[0080] In other words, if Figure 5As shown, the depth of the median crack MC formed on the scribe line SL2 of the first glass sheet G1 in the second cutting step S3 is the deepest at the starting end SL2a of the scribe line SL2 (D MAX ), which is shallowest at the terminal SL2b (D MIN ). Thus, the maximum depth of the median crack MC in the lower portion BP1 of the scribe line SL2 is shallower than the maximum depth of the median crack MC in the upper portion UP1 thereof. In addition, the maximum depth of the median crack MC in the lower portion BP1 of the scribe line SL2 is shallower than the maximum depth of the median crack MC in the middle portion MP1 thereof. In addition, the maximum depth of the median crack MC in the middle portion MP1 of the scribe line SL2 is shallower than the maximum depth of the median crack MC in the upper portion UP1 thereof.
[0081] exist Figure 6 In the example of the second glass plate G2 of the second embodiment shown, the depth of the median crack MC of the scratch SM remaining on the side end surface ESS gradually increases as it goes downward from the upper end SMa of the scratch SM located at the upper part UP2 of the side end surface ESS. The depth of the median crack MC becomes maximum at the middle part MP2 of the side end surface ESS. The depth of the median crack MC gradually decreases as it goes downward from the maximum position. The depth of the median crack MC becomes minimum at the lower end SMb of the scratch SM located at the lower part BP2 of the side end surface ESS.
[0082] Therefore, in this example, the maximum depth of the median crack MC in the upper portion UP2 of the side end surface ESS is shallower than the maximum depth of the median crack MC in the middle portion MP2 of the side end surface ESS.
[0083] In other words, if Figure 7 As shown in FIG. 1 , the depth of the median crack MC formed on the scribed line SL2 of the first glass sheet G1 in the second cutting step S3 is the deepest in the middle portion MP1 (D MAX ), which is shallowest at the terminal SL2b (D MIN ). In addition, the scribe line SL2 is formed so that the maximum depth of the median crack MC in the upper portion UP1 is shallower than the maximum depth of the median crack MC in the middle portion MP1.
[0084] exist Figure 8In the modified example of the second glass plate G2 of the first embodiment shown, the depth of the median crack MC of the scratch SM remaining on the side end surface ESS is the largest at the upper end SMa of the scratch SM, and gradually decreases as it goes downward from the upper end SMa. The depth of the median crack MC gradually increases in the middle part MP2 of the side end surface ESS as it goes downward from the boundary position with the upper part UP2 of the side end surface ESS, and becomes the maximum in the middle part. The depth of the median crack MC that becomes the maximum in the middle part MP2 of the side end surface ESS is shallower than the maximum depth of the median crack MC in the upper part UP2 of the side end surface ESS. It should be noted that the side end surface ESS may also have a portion where the depth becomes the maximum at multiple locations in the middle part MP2. The depth of the median crack MC gradually decreases as it goes downward from the position where it becomes the maximum in the middle part MP2. The depth of the median crack MC becomes the smallest at the lower end SMb of the scratch SM located at the lower part BP2 of the side end surface ESS.
[0085] In other words, if Fig. 9 As shown in FIG. 1 , the depth of the median crack MC formed on the scribed line SL2 of the first glass sheet G1 in the second cutting step S3 becomes maximum at the starting end portion SL2a (D MAX ), in the middle part MP1 becomes the maximum (D LM ), becomes minimum at the terminal SL2b (D MIN The scribe line SL2 is formed to have a maximum depth D in the middle portion MP1. LM The maximum depth D of the upper UP1 MAX shallow.
[0086] In the second glass sheet G2 of the first and second embodiments, when the thickness is 200 μm or more, the maximum depth of the median crack MC in the lower portion BP2 of the side end surface ESS can be set to, for example, 90 μm or less, and preferably 80 μm or less from the viewpoint of preventing breakage. On the other hand, from the viewpoint of stabilizing breakage, the minimum depth of the median crack MC in the lower portion BP2 of the side end surface ESS is preferably 30 μm or more, and more preferably 50 μm or more.
[0087] In the second glass sheet G2 of the first embodiment, when the thickness is 200 μm or more, the maximum depth of the median crack MC in the upper portion UP2 or the middle portion MP2 of the side end surface ESS is preferably 100 μm or more, and more preferably 110 μm or more, from the viewpoint of making the bending stress given to the glass sheet in the breaking step as small as possible by making the maximum depth of the median crack MC in the upper portion UP2 or the middle portion MP2 of the side end surface ESS deeper than the maximum depth of the median crack MC in the lower portion BP2 of the side end surface ESS. On the other hand, the maximum depth of the median crack MC in the upper portion UP2 or the middle portion MP2 of the side end surface ESS can be set to 180 μm or less, for example.
[0088] In the second glass sheet G2 of the second embodiment, when the thickness is 200 μm or more, the maximum depth of the median crack MC in the middle portion MP2 of the side end surface ESS is preferably 100 μm or more, and more preferably 110 μm or more, from the viewpoint of making the bending stress applied to the glass sheet as small as possible by making the maximum depth of the median crack MC in the middle portion MP2 of the side end surface ESS deeper than the maximum depth of the median crack MC in the breaking process of the lower portion BP2 of the side end surface ESS. On the other hand, the maximum depth of the median crack MC in the middle portion MP2 of the side end surface ESS can be set to, for example, 200 μm or less. From the viewpoint of preventing breakage, the maximum depth of the median crack MC in the upper portion UP2 of the side end surface ESS is preferably 90 μm or less, and more preferably 80 μm or less. On the other hand, from the viewpoint of stabilizing breaking, the minimum depth of the median crack MC in the upper portion UP2 of the side end surface ESS is preferably 30 μm or more, and more preferably 50 μm or more.
[0089] The packing step S4 is a step of manufacturing a glass plate package by placing a plurality of second glass plates G2 on a pallet. After the second cutting step S3 is completed, the second glass plate G2 is conveyed to the pallet by the conveying device 7 .
[0090] like Fig.10 As shown, in the packing step S4, the second glass plates G2 cut out in the second cutting step S3 are alternately loaded on the tray 11 with the protective sheets 10 while being suspended and supported in a vertical posture. The protective sheet 10 is a foamed resin sheet, but may be a non-foaming resin sheet, a backing paper, or the like.
[0091] The second glass plate G2 to be loaded on the tray 11 is in a posture along the vertical plane. In contrast, the back support surface 12a of the back support portion 12 of the tray 11 is an inclined surface that is inclined toward the rear side as it approaches the upper side. The inclination angle of the back support surface 12a relative to the horizontal plane is, for example, 60° to 85°. Therefore, the glass plate laminate 13 composed of the second glass plate G2 loaded on the tray 11 and the protective sheet 10 is in a vertical posture, but is inclined to imitate the back support surface 12a.
[0092] The second glass plate G2 is loaded on the pallet 11 while being suspended and supported in a vertical posture by the conveying device 7. In this case, the second glass plate G2 is loaded on the pallet 11 so that the second main surface 3 as a securing surface faces the back support surface 12a of the pallet 11.
[0093] like Fig.11As shown, the glass plate package GPB manufactured by performing the packaging step S4 includes: a glass plate stack 13 formed by alternately stacking the rectangular second glass plate G2 and the rectangular protection sheet 10 in a vertical posture (strictly speaking, the above-mentioned inclined posture); and a tray 11 on which the glass plate stack 13 is loaded. In addition, the glass plate package GPB also includes a packaging member such as a bundling band Ba for preventing the glass plate stack 13 from collapsing.
[0094] The tray 11 includes, in addition to the back support portion 12 having the inclined back support surface 12a described above, a bottom support portion 14 for supporting the bottom surface of the glass plate laminate 13. The bottom receiving surface 14a of the bottom support portion 14 is an inclined surface that inclines upward as it approaches the front side.
[0095] According to the present embodiment described above, in the second cutting step S3, by making the depth of the median crack MC formed in the lower part BP1 of the scribe line SL2 of the first glass sheet G1 shallower than the median crack MC in the upper part UP1 or the middle part MP1, the depth of the median crack MC in the scribe mark SM in the lower part BP2 of the side end surface ESS of the cut second glass sheet G2 can be made as shallow as possible. When the glass sheet package GPB is in a state, there is a possibility that the lower part BP2 of the side end surface ESS may be damaged due to the load or impact acting on the second glass sheet G2 during transportation. In particular, the deeper the depth of the median crack MC in the scribe mark SM, the easier it is to damage the lower part BP2 of the side end surface ESS. In the present embodiment, by making the depth of the median crack MC in the scribe mark SM in the lower part BP2 of the side end surface ESS of the second glass sheet G2 shallow, it is possible to prevent the lower part of the second glass sheet G2 from being damaged.
[0096] Moreover, by making the depth of the median crack MC of the upper part UP1 or the middle part MP1 of the scribe line SL2 in the second cutting process S3 deeper than the depth of the median crack MC of the lower part BP1 of the scribe line SL2, the amount of glass powder generated from the upper part UP1 or the middle part MP1 can be minimized in the breaking process of the second cutting process S3.
[0097] It should be noted that the present invention is not limited to the configuration of the above-described embodiment, nor is it limited to the above-described effects. The present invention can be modified in various ways without departing from the gist of the present invention.
[0098] In the above-mentioned embodiment, an example is shown in which the depth of the median crack MC of the scribe mark SM on the fracture surface (side end surface ESS) of the second glass sheet G2 is measured, but the present invention is not limited to this structure. For example, the depth of the median crack MC of the scribe line SL2 may be measured by measuring the depth of the median crack of the scribe mark remaining on the fracture surface of the width direction end Ga cut off from the first glass sheet G1 in the second cutting step S3.
[0099] Description of Reference Numerals
[0100] 8 Scratching wheel (scratching tool)
[0101] 11 Pallet
[0102] BP1 Lower part of the score line
[0103] BP2 Lower portion of the side surface of the second glass plate
[0104] ESS Side surface of the second glass plate
[0105] G1 First Glass Plate
[0106] G2 Second glass plate
[0107] Ga End of the first glass plate in the width direction
[0108] GPB Glass Plate Package
[0109] MC median crack
[0110] MP1 Middle of the score line
[0111] MP2 The middle part of the side surface of the second glass plate
[0112] S3 Second cutting process
[0113] SL2 Score Line
[0114] SM Scratches
[0115] UP1 Upper part of the score line
[0116] UP2 Upper part of the side surface of the second glass plate
[0117] X width direction
[0118] Y pull direction.
Claims
1. A method for manufacturing a glass plate, comprising a cutting step of removing the end portions in the width direction of the glass plate while the glass plate is supported in a vertical posture, The method for manufacturing the glass plate is characterized in that: The cutting process comprises: a scoring step of forming a scoring line including a median crack on the glass sheet along a vertical direction using a scoring tool; and a breaking step of applying bending stress to the glass sheet having the scoring line formed thereon to break the glass sheet. In the scribing step, the scribe line is formed such that the maximum depth of the median crack at a lower portion of the scribe line is shallower than the maximum depth of the median crack at an upper portion or a middle portion of the scribe line.
2. The method for manufacturing a glass plate according to claim 1, wherein: The maximum depth of the median crack in the middle portion of the score line is shallower than the maximum depth of the median crack in the upper portion of the score line.
3. The method for manufacturing a glass plate according to claim 1, wherein: The maximum depth of the median crack in the upper portion of the score line is shallower than the maximum depth of the median crack in the middle portion of the score line.
4. A glass plate package, comprising rectangular glass plates and a tray on which the glass plates are stacked in a vertical position, The glass plate package is characterized in that: The glass plate has an end surface extending in the up-down direction at an end in the width direction. The end surface is a fracture surface having a scratch mark including a median crack, The maximum depth of the median crack at the lower portion of the end surface is shallower than the maximum depth of the median crack at the upper portion or the middle portion of the end surface.
5. The glass plate package according to claim 4, wherein: The maximum depth of the median crack in the middle portion of the end surface is shallower than the maximum depth of the median crack in the upper portion of the end surface.
6. The glass plate package according to claim 4, wherein: The maximum depth of the median crack in the upper portion of the end surface is shallower than the maximum depth of the median crack in the middle portion of the end surface.
7. A glass plate, rectangular in shape, The glass sheet is characterized in that The glass plate has an end surface extending along the pulling direction. The end face is a fracture surface having a median crack, The maximum depth of the median crack at one end of the end surface in the plate pulling direction is shallower than the maximum depth of the median crack at the other end or middle portion of the end surface in the plate pulling direction.