High zirconia electrocast refractory
By adjusting the chemical composition of high zirconia electromelting cast refractories, inhibiting the formation of ZrO2 crystal phase and zircon crystals, the problems of joint openings and zircon crystals in glass melting kilns are solved, and the corrosion resistance and resistance of refractories are improved Thermal properties enable stable operation and high-quality production of glass melting kilns.
Patent Information
- Application Number
- CN202380029308.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-25
- Filing Date
- 2023-03-10
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2043-03-10
Smart Images

Figure CN118922394A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a high zirconia electric fused casting refractory suitable for use in a glass melting furnace. Background Art
[0002] As refractory for glass melting furnace, electric casting refractory (hereinafter, sometimes simply described as "refractory") has been widely used.
[0003] The so-called electric fused cast refractory is a refractory that is dense and has excellent corrosion resistance to molten glass. It is manufactured by melting a raw material prepared by mixing main components such as alumina, silica, and zirconia with trace components such as sodium carbonate and boric acid in a given amount in an electric arc furnace, casting the melt in a refractory mold, cooling it together with the mold in an annealing material, and solidifying it into the shape of the mold.
[0004] Since the electrocast refractory is manufactured through the process of casting the molten material in a mold, it is different from the manufacturing method of the sintered refractory manufactured by sintering and bonding the crystal particles. In addition, the technical development means and methods, and the solution means and methods of the sintered refractory cannot be used for the electrocast refractory, and vice versa.
[0005] As one of such electric cast refractory materials, a high zirconia electric cast refractory containing 85 mass % or more of ZrO 2 is generally used.
[0006] High zirconia electric fused casting refractory has low solubility in glass, and ZrO2 with high melting point is the main component. It has high ZrO2 content and dense structure, so it has great corrosion resistance to all types of molten glass.
[0007] Furthermore, the high zirconia electric fused casting refractory has the property of not generating a reaction layer at the interface with the molten glass, and therefore has an excellent feature that defects such as nodules and streaks are unlikely to be generated in the molten glass.
[0008] Therefore, high zirconia electric fused casting refractory is a refractory particularly suitable for producing high-quality glass.
[0009] The mineral structure of the high zirconia electric fused casting refractory is composed of a monoclinic ZrO2 crystal that occupies most of the body and a small amount of glass phase filling the grain boundaries of the ZrO2 crystals.
[0010] This small amount of glass phase has a composition very different from that of the glass used in the glass industry. It is a glass that is very rich in SiO2. It is melted simultaneously with a high content of ZrO2 and cast in a mold. Therefore, the technical development means and methods, and solution means and methods of the glass industry cannot be used for electric cast refractory materials, and vice versa.
[0011] The glass phase of high zirconia electric cast refractory is generally composed of oxides such as Al2O3, SiO2, Na2O, B2O3, and P2O5.
[0012] Furthermore, ZrO2 crystals, which account for most of the high zirconia electric cast refractory, undergo a rapid volume change from 1000°C (when cooling) to around 1150°C (when heating), and a reversible crystal phase transition between monoclinic and tetragonal occurs.
[0013] By adopting the flow of the glass phase filling the grain boundaries of the ZrO2 crystals to alleviate the stress generated by the volume change accompanying the phase transformation of the ZrO2 crystals, it is possible to manufacture and sell high zirconia electrocast refractory with a ZrO2 content of 93 to 94 mass% that is free of cracks (cracks) during manufacturing and during heating at the production level.
[0014] However, the rapid volume change of the ZrO2 crystal from 1000°C (when cooling) to 1150°C (when heating) and the reversible phase transition between monoclinic and tetragonal crystals have a great impact on the glass melting furnace when high zirconia electrocast refractory is used in the glass industry.
[0015] That is, the high zirconium oxide electric casting refractory expands when heated, but changes from monoclinic to tetragonal in the ZrO2 crystal phase transition temperature region, accompanied by a sharp volume contraction. With further heating thereafter, the refractory expands, but in the operating temperature region of the glass melting furnace, its expansion does not exceed the maximum expansion of the monoclinic in the ZrO2 crystal phase transition temperature region.
[0016] Therefore, for general high zirconia electric cast refractory, in an operating glass melting furnace, a temperature distribution is generated between the surface on the inner side of the furnace that contacts the molten glass and reaches the maximum temperature (generally 1300°C to 1700°C) and the surface on the outer side of the glass melting furnace that contacts the atmosphere (or insulating material), with maximum expansion between these two surfaces.
[0017] That is, when the temperature rises, the ZrO2 crystal shrinks due to the phase transition from monoclinic to tetragonal, which means that the refractory has an expansion coefficient smaller than the maximum expansion at the part inside the furnace in contact with the molten glass.
[0018] If the refractory has an expansion coefficient smaller than the maximum expansion at the portion inside the furnace in contact with the molten glass, a portion called a "joint" serving as the contact portion between the refractory materials in a glass melting furnace using a combination of refractory materials will be slightly open.
[0019] If the contact portion between the refractories, that is, the joint, is opened, the flow rate of the glass near the joint changes, thereby accelerating the erosion of the refractories by the glass.
[0020] In addition, with respect to high zirconia electrocast refractory, if the refractory is heated alone or subjected to a heat cycle in a temperature region where a reversible crystalline phase transition between monoclinic and tetragonal crystals occurs, accompanied by a rapid volume change of ZrO2 crystals from 1000°C (when cooling) to 1150°C (when heating), sometimes the main component of the glass phase of the refractory, namely silicon dioxide (SiO2), reacts with zirconium oxide (ZrO2) crystals to form zircon (ZrO2·SiO2) crystals.
[0021] When subjected to heating and thermal cycles, zircon crystals are generated at the interface or glass phase between ZrO2 crystals and the glass phase filling the crystal grain boundaries, so the generation of zircon crystals leads to a relative reduction in the glass phase. Furthermore, if the reduction of the glass phase progresses due to the growth and increase of zircon crystals, it becomes difficult for the glass phase to absorb the rapid volume change of ZrO2 crystals at around 1000°C to 1150°C, the strength of the refractory is reduced, and cracks are easily generated.
[0022] At this time, corrosion selectively occurs from the cracked portion, and if corrosion progresses, crystals constituting the high zirconia electric cast refractory are mixed into the molten glass, which may cause a decrease in the quality of the glass.
[0023] Therefore, in order to perform long-term stable operation and maintain stable glass quality in the operation of a glass melting furnace, it is very important to suppress the generation of zircon crystals in the high zirconia electric cast refractory.
[0024] Therefore, research has been conducted so far on refractory materials that suppress the opening of joints at contact portions between refractory materials, namely, portions called "joints", by adding Y2O3 to the refractory materials.
[0025] Furthermore, high zirconia electro-fused casting refractory materials that suppress the formation of zircon crystals have been studied so far.
[0026] Patent Document 1 proposes a fused-cast zirconia heat-resistant mechanical material characterized by comprising single crystals and / or polycrystals having a composition of 89≦ZrO2≦99, 1≦Y2O3≦11 expressed in mol %.
[0027] As for the refractory of document 1, although zircon crystals are not generated because it does not contain SiO2, it cannot absorb the rapid volume change during the phase transition between monoclinic and tetragonal ZrO2 crystals, making it difficult to mass-produce refractory materials industrially.
[0028] Patent Document 2 proposes a fused zirconia refractory material, which is characterized by containing 1 to 30 wt% of calcium oxide and 0.05 to 2 wt% of yttrium oxide or a rare earth mineral containing yttrium oxide as stabilizers.
[0029] As for the refractory of document 2, although zircon crystals are not generated because it does not contain SiO2, it cannot absorb the rapid volume change during the phase transition between monoclinic and tetragonal ZrO2 crystals, making it difficult to mass-produce refractory materials industrially.
[0030] A product is proposed in patent document 3, which is a refractory product containing more than 85% zirconium oxide (ZrO2), characterized in that, based on the weight percentage of oxides, it includes ZrO2>92%, SiO2: 2~8%, Na2O: 0.12~1%, Al2O3: 0.2~2%, 0.5%≤Y2O3+CaO≤2.6%, wherein Y2O3: 0.3~2%, or CaO: 0.5~1.93%.
[0031] The refractory of Document 3 was cracked during production and was difficult to manufacture at a production level. As described below, this is believed to be due to the relatively low Y2O3 content.
[0032] Patent document 4 proposes a refractory material which is melted and then cast, wherein, expressed in weight % based on oxides, the total being 100%, comprises ZrO2: 100% balance, Hf2O: <5%, SiO2: 2% to 10%, 0.9 < Y2O3 + CeO2 + CaO + MgO ≤ 4.0%, B2O3: ≤ 4.5%, B2O3: ≥ 0.09 × (Y 2O3+1 / 3(CeO2+CaO+MgO))×SiO2, Al2O3: 0.3%~2.0%, Na2O+K2O: ≦0.5%, P2O5: <0.05%, Fe2O3+TiO2: <0.55%, other species: <1.0%, among which the Y2O3 content is more than 0.5% or the CeO2+CaO+MgO content is more than 2%.
[0033] The refractory of Document 4 contains a large amount of CaO and MgO which significantly promote the formation of zircon crystals. The increase in residual volume expansion after heating due to the formation of zircon crystals may cause cracks in the refractory, which may reduce the strength of the refractory structure.
[0034] In patent document 5, a fused cast refractory is proposed, which is expressed by weight percentage based on oxides and, relative to a total of 100%, includes ZrO2: balance up to 100%, Hf2O: <5%, SiO2: 2% to 10%, Y2O3: 0.4 to 2.0%, CaO: 4.0% to 8.0%, B2O3+Na2O+K2O: 0.4 to 3.0%, Al2O3: 0.3% to 2.0%, P2O5: <0.05%, Fe2O3+TiO2: <0.55%, and other species: <1.5%.
[0035] In Document 5, a large amount of CaO is contained which significantly promotes the formation of zircon crystals. The increase in residual volume expansion after heating caused by the formation of zircon crystals and anorthite crystals (CaAl2Si2O8) becomes the cause of cracks in the refractory, which may reduce the strength of the refractory structure.
[0036] Patent document 6 proposes a refractory material which is melted and then cast, wherein, expressed in terms of weight % based on oxides, the total being 100%, comprises ZrO2: 100% balance, SiO2: 2% to 10%, 0.9<Y2O3+CeO2+CaO+MgO≦4.0%, B2O3: ≦4.5%, B2O3: ≧0.09×(Y2O3+1 / 3(CeO2+CaO+MgO))×SiO2, Al2O3: 0.3% to 2.0%, and Y2O3: ≧0.8 %, and satisfies the following characteristics: HfO2: <5%, CeO2: <0.7%, MgO: <0.7%, CaO: <0.7%, Na2O+K2O: ≦0.5%, P2O5: <0.05%, Fe2O3+TiO2: <0.55%, and the respective amounts of species other than ZrO2, HfO2, SiO2, Y2O3, CeO2, CaO, MgO, B2O3, Al2O3, Na2O, K2O, P2O5, Fe2O3, and TiO2: <0.2%.
[0037] The refractory of Document 6 cracks during production, making it difficult to mass-produce the refractory industrially. As described below, this is thought to be because the Y2O3 content is 4% or less.
[0038] Patent Document 7 proposes a high zirconia electric casting refractory, wherein ZrO2 is 85 to 95% by weight, Al2O3 is 0.4 to 2.5% by weight, SiO2 is 3.5 to 10% by weight, the total of Na2O and K2O is 0.05 to 1% by weight, B2O3 is more than 0.04% by weight and less than 1% by weight, P2O5 is less than 0.02% by weight, MgO is less than 0.05% by weight, and CaO is less than 1% by weight. It is 0.01~0.2 weight%. For SrO and BaO, when they are contained alone, SrO is 0.3~3 weight% or BaO is more than 0.5 weight% and less than 3 weight%. When both are contained, SrO is more than 0.3 weight%, and the total of SrO and BaO is 0.3~3 weight%. SnO2 is 0.01~0.7 weight%, and the total of Fe2O3 and TiO2 is less than 0.3 weight%.
[0039] Since the refractory of Document 7 has an extremely low content of Y2O3, it cannot suppress the opening of the joint and the corrosion resistance of the joint is insufficient.
[0040] Patent document 8 proposes a molten cast refractory product, which is expressed as a mass percentage based on oxides and relative to the total of 100% of the oxides, includes ZrO2+HfO2: up to 100% balance, wherein Hf2O≦5%, SiO2: 1.5%~7.5%, Al2O3: 1.0%~3.0%, CaO+SrO: 1.2~3.0%, Y2O3: 1.5~3.0%, Na2O+K2O: <0.15%, B2O3: <1.0%, P2O5: <0.15%, Fe2O3+TiO2: <0.55%, oxide species other than ZrO2, HfO2, SiO2, Al2O3, Na2O, K2O, B2O3, CaO, SrO, Y2O3, P2O5, Fe2O3, and TiO2: <1.5%.
[0041] The refractory of Document 8 sometimes cracks and is difficult to manufacture at a production level. As described below, this is believed to be because the Y2O3 content is 4% or less.
[0042] Prior art literature
[0043] Patent Literature
[0044] Patent Document 1: Japanese Patent Application Laid-Open No. 59-131585
[0045] Patent Document 2: Japanese Patent Application Laid-Open No. 4-42813
[0046] Patent Document 3: Japanese Patent Application No. 2005-526683
[0047] Patent Document 4: Japanese Patent Application No. 2013-514254
[0048] Patent Document 5: Japanese Patent Application No. 2015-506898
[0049] Patent Document 6: Japanese Patent Application Publication No. 2015-212223
[0050] Patent Document 7: Japanese Patent Application Publication No. 2015-40144
[0051] Patent Document 8: Japanese Patent Application No. 2018-509363 Summary of the invention
[0052] Problems to be solved by the invention
[0053] Generally, if high zirconium oxide electro-cast refractory contains Y2O3, most of Y2O3 is dissolved in ZrO2 crystal, and part of it is contained in the glass phase of refractory. At this time, through the solid solution of Y2O3 in ZrO2 crystal, part of it becomes tetragonal ZrO2, and the characteristics of ZrO2 crystal change. That is, the phase transition temperature of the reversible crystal phase of monoclinic crystal and tetragonal crystal accompanied by the rapid volume change of ZrO2 crystal from 1000℃ (when cooling) to 1150℃ (when heating), so the maximum expansion temperature is moved to the low temperature side.
[0054] On the other hand, as described above, in terms of the refractory during operation, a temperature distribution is generated between the surface of the furnace inside the glass melting furnace that contacts the molten glass and the surface of the outside of the glass melting furnace that contacts the atmosphere (or insulating material), and the general high zirconia electric casting refractory has the maximum expansion between these two surfaces. If the phase change temperature of the ZrO2 crystal migrates to the low temperature side, the maximum expansion of the refractory moves in the direction of the surface outside the glass melting furnace that contacts the atmosphere (or insulating material), and compared with the general refractory, the ZrO2 crystal changes into a tetragonal crystal at a low temperature and then expands, so the expansion of the part of the furnace inside the glass melting furnace that contacts the molten glass is the same as the maximum expansion of the refractory or becomes a slightly smaller state, so that the joint part as the contact part between the refractory is closed, or the opening of the joint part is suppressed.
[0055] However, if the phase transition temperature of the ZrO2 crystal phase migrates to the low temperature side, the viscosity of the glass phase is high on the low temperature side, and further, the low temperature side is the temperature region where the glass phase solidifies. Therefore, the glass phase cannot alleviate the stress generated by the volume change accompanying the phase transition of the ZrO2 crystal, and cracking is likely to occur, which may make it difficult to mass-produce refractory materials industrially.
[0056] In addition, if the phase transition temperature of the ZrO2 crystal phase migrates to a greater extent toward the low temperature side, the stress generated by the volume change accompanying the phase transition of the ZrO2 crystal can no longer be further alleviated during the manufacture of the refractory, which may also promote the occurrence of cracks.
[0057] Therefore, it is considered difficult to increase the Y2O3 content and increase the degree of migration of the phase transformation temperature of the ZrO2 crystal phase to the low temperature side, thereby producing a high-zirconia electric cast refractory with good quality.
[0058] In addition, when using refractory materials in which the phase change temperature of the ZrO2 crystal phase migrates to the low temperature side in the glass melting furnace, if zircon crystals are generated during operation, the glass phase will be relatively reduced, and the viscosity of the glass phase is high at low temperatures. Furthermore, on the low temperature side, the glass phase solidifies. Therefore, if a thermal cycle occurs due to changes in the operating temperature during the glass melting furnace operation, it becomes difficult to absorb the rapid volume change of the ZrO2 crystals compared to general high zirconia electric cast refractory materials, and cracking may occur easily.
[0059] Therefore, it is considered that high zirconia electric cast refractory with relatively increased Y2O3 content is not suitable for use in a portion where thermal cycles occur due to changes in operating temperature in a glass melting furnace.
[0060] In addition, if Y2O3 content is increased, ZrO2 content is reduced relatively. ZrO2 content has a great influence on the corrosion resistance of refractory relative to glass, because the corrosion resistance of refractory is proportional to ZrO2 content, therefore think that the corrosion resistance of refractory with relatively low ZrO2 content is insufficient.
[0061] Therefore, it is considered that high zirconia electric cast refractory with increased Y2O3 content may have insufficient corrosion resistance in a glass melting furnace.
[0062] In such a background, the object of the present invention is to provide an improved high zirconia electrocast refractory, and in particular, to provide a high zirconia electrocast refractory which is easy to mass-produce industrially, suppresses the opening of the joints at the contact portions between the refractories, namely the portions called "joints", and also suppresses the formation of zircon crystals. Even if some zircon crystals are formed, the residual volume expansion coefficient does not increase extremely, and no cracks are generated in the refractory when heated and thermally cycled, and has high corrosion resistance to glass.
[0063] Means for solving problems
[0064] The solving means of the present invention is exemplified as follows: a high zirconia electric cast refractory.
[0065] <Option 1>
[0066] High zirconia electric cast refractory, wherein, as chemical components, the total of ZrO2 and HfO2 is more than 80 mass% and less than 92 mass%, Al2O3 is 0.2-3.0 mass%, SiO2 is 1.5-10 mass%, Na2O is 0.05-2.0 mass%, K2O is less than 1.0 mass%, B2O3 is 0-1.5 mass%, Y2O3 is more than 4.0 mass% and less than 9.0 mass%, the total of MgO and CaO is 0.02-0.4 mass%, CaO is more than 0.01 mass%, the total of Fe2O3 and TiO2 is less than 0.5 mass%, and the content of P2O5 is less than 0.04 mass%.
[0067] <Option 2>
[0068] The high zirconia electric cast refractory according to Scheme 1, wherein, as chemical components, the total of ZrO2 and HfO2 is more than 80 mass% and less than 92 mass%, Al2O3 is 0.4-2.5 mass%, SiO2 is 1.5-7.0 mass%, Na2O is 0.3-1.8 mass%, K2O is less than 1.0 mass%, B2O3 is 0-1.0 mass%, Y2O3 is more than 4.0 mass% and less than 7.5 mass%, the total of MgO and CaO is 0.02-0.4 mass%, CaO is more than 0.01 mass%, the total of Fe2O3 and TiO2 is less than 0.5 mass%, and the content of P2O5 is less than 0.04 mass%.
[0069] <Option 3>
[0070] The high zirconia electric cast refractory according to claim 1 or 2, wherein the mass content of Y2O3 is 4.5 to 7.5 mass%.
[0071] <Option 4>
[0072] The high zirconia electric cast refractory according to claim 3, wherein the mass content of Y2O3 is more than 4.5 mass % and less than 6.0 mass %.
[0073] <Option 5>
[0074] The high zirconia electric cast refractory according to any one of claims 1 to 4, wherein the mass content of SiO2 is 4.0 to 6.5 mass%.
[0075] <Option 6>
[0076] The high zirconia electric fused cast refractory according to any one of claims 1 to 5, wherein the mass content of Al 2 O 3 is 0.5 to 1.2 mass %.
[0077] <Option 7>
[0078] The high zirconia electric fused cast refractory according to any one of claims 1 to 6, wherein the mass content of Na2O is 0.5 to 1.2 mass%.
[0079] <Option 8>
[0080] The high zirconia electric fused cast refractory according to any one of claims 1 to 7, wherein the mass content of B2O3 is 0.01 to 0.6 mass %.
[0081] <Option 9>
[0082] The high zirconia electric cast refractory according to any one of claims 1 to 8, wherein in the process of heating from 200°C to 1500°C, the temperature at which the expansion coefficient of the refractory becomes maximum exists in the range of 1300°C to 1500°C.
[0083] <Option 10>
[0084] The high zirconia electric cast refractory according to any one of claims 1 to 9, wherein during cooling from 1500° C., ZrO 2 crystals shrink without changing from a tetragonal phase to a monoclinic phase.
[0085] <Plan 11>
[0086] The high zirconia electric fused casting refractory according to any one of aspects 1 to 10, which is used in a glass melting furnace.
[0087] Effects of the Invention
[0088] According to the present invention, an improved high-zirconia electric fused-cast refractory can be provided. In particular, if the high-zirconia electric fused-cast refractory of the present invention, which is easy to mass-produce industrially, is used in a glass melting furnace, the opening of the joints at the contact portion between the refractory materials is suppressed, and the generation of zircon crystals is suppressed. Even if zircon crystals are generated, the residual volume expansion coefficient does not become extremely large, and cracks do not occur in the refractory, so a refractory with high corrosion resistance to glass can be provided. Therefore, long-term operation can be achieved, which is very beneficial in industry. BRIEF DESCRIPTION OF THE DRAWINGS
[0089] Figure 1 This is a graph showing the thermal expansion coefficient measurement of a high zirconia electric cast refractory containing 93 mass % of zirconia (Y2O3 content 0.24 mass %) and Examples 2 and 8.
[0090] Figure 2 This is a graph showing the thermal expansion coefficient measurement of a high zirconia electric cast refractory containing 93 mass % of zirconia (Y2O3 content: 0.24 mass %) and Comparative Example 16.
[0091] Figure 3 A diagram showing an apparatus used for evaluating corrosion resistance.
[0092] Figure 4 This is a photograph of the appearance of the sample after the corrosion resistance evaluation.
[0093] Figure 5A This is a photograph of the internal structure of a high zirconia electric cast refractory containing 93 mass % zirconia (0.24 mass % Y2O3 content) after corrosion resistance evaluation.
[0094] Figure 5B This is a photograph of the internal structure of the high zirconia electric cast refractory according to Example 1 after evaluation of corrosion resistance. DETAILED DESCRIPTION
[0095] The inventor of the present application has conducted in-depth research and found that: at ZrO and HfO, the content of the total is to exceed 80% by mass and in the refractory below 92% by mass, by making AlO, SiO, NaO, KO, BO, MgO, CaO, PO, FeO, and TiO, the content of each component is a specific range, and then YO content is to exceed 4% by mass and below 9% by mass, thereby can solve the problem of the present invention. Specifically, it is found that according to such composition, ZrO can be made that the crystalline phase is not a part but all or almost all becomes tetragonal, as a result, makes ZrO, the phase transition of the reversible crystalline phase of the monoclinic crystal and tetragonal crystal almost disappears, and also makes the rapid volume change disappear. It was also discovered that, during the temperature increase from 200°C to 1500°C, if the temperature at which the expansion coefficient of the refractory becomes maximum is between 1300°C and 1500°C, the maximum expansion portion that previously existed between the outer side surface of the high zirconia electric cast refractory and the inner side surface of the furnace can be moved to the inner side of the furnace in contact with the molten glass, thereby completely or substantially completely suppressing the opening of the joint at the contact portion between the refractory materials.
[0096] That is, by making Y2O3 content be more than 4 mass % and less than 9 mass %, the phase change of the reversible crystalline phase of monoclinic and tetragonal of ZrO2 disappears, or substantially disappears, so even if the phase change temperature of ZrO2 crystalline phase migrates to the low temperature side, the stress generated by the volume change accompanying the phase change of ZrO2 crystal is also small, or substantially disappears, so the generation of cracks can be suppressed during the manufacture of refractory, industrial batch production becomes easy, and the joint opening when the refractory in the glass melting furnace is used can also be suppressed, and the corrosion resistance of glass is increased. In addition, for such refractory, in the cooling process from 1500 ℃, ZrO2 crystal does not shrink from tetragonal phase change to monoclinic. Therefore, it was found that when heated and heat-cycled during glass melting furnace operation, even if zircon crystals are generated, the reversible phase transformation of the monoclinic and tetragonal crystals of ZrO2 disappears or substantially disappears during the heating and cooling processes. Therefore, it is possible to provide high-zirconia electric-cast refractory refractory that does not produce cracks in the refractory.
[0097] In addition, it was found that if the Y2O3 content is increased, the ZrO2 concentration is relatively reduced, and Y2O3 plays a role substantially equivalent to that of ZrO2 through solid solution in ZrO2, and has the same corrosion resistance as the conventional high zirconia electric cast refractory with a ZrO2 content of 93 to 94% by mass, or through nodules formed by crystallization of a portion of Y2O3 contained in the glass phase during heating and holding, or high-concentration Y2O3 nodules formed by dissolution of Y2O3 in the ZrO2 in the glass phase, ZrO2 particles are easily three-dimensionally networked, thereby improving corrosion resistance (refer to Figure 5B ).
[0098] 《Contains ingredients》
[0099] The following is an explanation of each component of the refractory according to the present invention. The term "substantially free" means less than 0.01 mass %.
[0100] <ZrO2>
[0101] The content of ZrO2 contained in the high zirconia electric casting refractory can be relatively determined according to the content of other components. However, if the content of ZrO2 is too high, the content of other components will be relatively reduced.
[0102] In addition, ZrO2 raw materials and zircon raw materials used as raw materials for high zirconium oxide electric casting refractory inevitably contain 1 to 2 mass % of HfO2. HfO2 does not volatilize during manufacturing, so it is also included in high zirconium oxide electric casting refractory. Furthermore, it is a stable oxide like ZrO2 and has the same effect as ZrO2, so the ZrO2+HfO2 content can also be treated as the ZrO2 content.
[0103] Therefore, the total content of ZrO2 and HfO2 in the present invention is more than 80 mass% and less than 92 mass%, preferably 81-92 mass%, 82-92 mass%, 83-92 mass%, 84-92 mass%, 85-92 mass%, 86-92 mass%, and more preferably 86-91 mass%, 86-90 mass%, 86-89 mass%.
[0104] <SiO2>
[0105] SiO2 is the main component of the glass phase in the refractory of the present invention.
[0106] The content of SiO2 is 1.5 to 10% by mass, more preferably 1.5 to 9.0% by mass, 1.5 to 8.0% by mass, or 1.5 to 7.0% by mass, and further preferably 2.0 to 7.0% by mass, 3.0 to 7.0% by mass, 4.0 to 7.0% by mass, 4.0 to 6.5% by mass, or 4.0 to 6.0% by mass.
[0107] Even though the solid solution of Y2O3 in ZrO2 crystals causes almost no shrinkage during the phase transition from monoclinic to tetragonal crystals, and the shrinkage rate is small, the ZrO2 crystals sometimes shrink during the phase transition from monoclinic to tetragonal crystals. At this time, if the content of SiO2 is less than 1.5% by mass, the amount of glass phase formed is reduced, and the stress caused by the volume change accompanying the phase transition of ZrO2 crystals cannot be completely suppressed, and cracking is easy to occur. If the content of SiO2 exceeds 10% by mass, the ZrO2 content is relatively reduced, so the corrosion resistance is sometimes reduced.
[0108] <Al2O3>
[0109] With regard to Al2O3, in the present invention, even if this raw material is not directly added, industrial batch production is also hardly affected.But Al2O3 has the effect of suppressing the generation of zircon crystals, so preferably contains.But, if it exceeds 2.5 quality %, then during manufacturing, during heating, the crystal of corundum and mullite in the glass phase is easily separated out, but even if the crystal is separated out, by Y2O3 solid solution in ZrO2 crystal, the phase transition from monoclinic to tetragonal crystalline phase disappears or disappears substantially, even if these resultants that become the cause of cracking when manufacturing high zirconium oxide electric casting refractory exist, industrial batch production is also hardly affected.
[0110] In the present invention, the content of Al2O3 is 0.2 to 3.0 mass%. Since Al2O3 exists as an impurity of ZrO2 raw material and SiO2 raw material, even if it is not newly added, it generally contains more than 0.2 mass%. In addition, if it exceeds 3.0 mass%, the ZrO2 content is relatively reduced, and the corrosion resistance is sometimes reduced.
[0111] Therefore, the Al2O3 content is 0.2 to 3.0 mass%, more preferably 0.3 to 3.0 mass%, 0.3 to 2.50 mass%, 0.4 to 3.0 mass%, or 0.4 to 2.5 mass%, and further preferably 0.4 to 2.0 mass%, 0.4 to 1.5 mass%, 0.5 to 1.5 mass%, or 0.5 to 1.2 mass%.
[0112] <Na2O>
[0113] Na2O functions as a modified oxide in the glass phase. It is also a necessary component in order to reduce the viscosity of the glass phase, reduce the occurrence of cracks during the manufacture of high zirconium oxide electric casting refractory, and facilitate industrial batch production. In addition, Na2O has the effect of significantly inhibiting the formation of zircon crystals in the glass phase of the refractory, but if the content exceeds 2.0% by mass, the softening point of the glass phase is significantly reduced, so the refractory is easily deformed and sometimes the corrosion resistance is reduced.
[0114] Therefore, the content of Na2O is 0.05 to 2.0 mass%, more preferably 0.2 to 2.0 mass%, 0.2 to 1.8 mass%, 0.3 to 1.8 mass%, 0.4 to 1.8 mass%, further preferably 0.5 to 1.7 mass%, 0.6 to 1.7 mass%, 0.7 to 1.7 mass%, or 0.5 to 1.4 mass%, 0.5 to 1.2 mass%, 0.5 to 1.0 mass%.
[0115] <K2O>
[0116] The K2O content is 1.0 mass % or less, preferably 0.5 mass % or less, more preferably 0.1 mass % or less, and particularly preferably substantially free of K2O. Substantially free of K2O means less than 0.01 mass %. The lower limit of the K2O content is not particularly limited, and may be 0.001 mass % or 0.0001 mass %.
[0117] <B2O3>
[0118] As for B2O3, even if it is not contained in the present invention, it will hardly have an impact on industrial batch production. However, even if B2O3 has a low content, it has the effect of suppressing cracking during manufacturing, and sometimes makes industrial batch production easy. On the other hand, if it exceeds 1.5% by mass, relatively, ZrO2 content decreases, so sometimes the corrosion resistance of high zirconium oxide electric casting refractory decreases. In addition, if the content is too high, sometimes the generation of zircon crystals is easy.
[0119] Therefore, the content of B2O3 is 0 to 1.5 mass%, more preferably 0 to 1.2 mass%, 0 to 1.0 mass%, further preferably 0.01 to 0.8 mass%, 0.01 to 0.6 mass%, 0.01 mass% or more and less than 0.58 mass%, 0.01 to 0.5 mass%, or 0.01 to 0.4 mass%, 0.01 to 0.2 mass%.
[0120] <Y2O3>
[0121] Y2O3 is the most important component in the present invention.Think that by making Y2O3 content exceed 4 mass % and be below 9 mass %, so that ZrO2 crystalline phase is not a part but all or substantially all become tetragonal, so that ZrO2 the phase transition of the reversible crystalline phase of monoclinic crystal and tetragonal crystal disappears substantially, so ZrO2 the rapid volume change during the phase transition of monoclinic crystal and tetragonal crystal also disappears substantially, and the effect of cracking during manifestation suppression manufacturing can be made to make industrial batch production easy.If Y2O3 content is too much, then to cubic ZrO2 stabilization, can become the reason for cracking during manufacturing.When Y2O3 content is too little, compared with tetragonal crystal, the ZrO2 of monoclinic crystal The ratio rises, ZrO2 the rapid volume change during the phase transition of monoclinic crystal and tetragonal crystal becomes large, so can become the reason for cracking during manufacturing.
[0122] Therefore, the content of Y2O3 is greater than 4.0 mass% and less than 9.0 mass%, more preferably greater than 4.0 mass% and less than 8.5 mass%, greater than 4.0 mass% and less than 8.0 mass%, greater than 4.0 mass% and less than 7.5 mass%, further preferably 4.5-7.5 mass%, 4.5-7.0 mass%, 4.5-6.5 mass%, 4.5-6.0 mass%, greater than 4.5 mass% and less than 6.0 mass%, or 5.0-6.0 mass%.
[0123] <MgO>
[0124] MgO exists as an impurity of ZrO2 raw material, so it is necessary to pay attention to the selection of raw materials. In addition, if the content is high, the formation of zircon crystals is sometimes made easy. In the present invention, it is not necessary to newly add, preferably 0.1% by mass or less, and more preferably substantially free of MgO.
[0125] <CaO>
[0126] As for CaO, by containing a certain amount, the viscosity of the melt of the high zirconium oxide electric casting refractory can be reduced to form a stable glass phase. In the case of basically not containing it, it becomes a very unstable glass phase, and cracks occur during manufacturing. That is, due to the occurrence of cracks, it is impossible to achieve mass production in manufacturing. Therefore, CaO must be contained.
[0127] In addition, CaO exists as ZrO2 raw material and as impurities of zircon raw material of ZrO2 source, so when making the content in refractory less than 0.01%, it is necessary to use high-purity reagent as raw material, which is not suitable for batch production due to its very high price. Therefore, the content is more than 0.01% by mass, preferably more than 0.02% by mass. But, if it exceeds a certain amount, it is necessary to pay attention to the generation of zircon crystals due to the promotion of the generation of zircon crystals. Due to the phase transition of the reversible crystalline phase of the monoclinic crystal and tetragonal crystal of ZrO2 crystal almost disappears, so even if zircon crystal is generated, it can be said that cracks will not be generated in refractory, but in the present invention, although the shrinkage is small, due to the shrinkage refractory during the crystalline phase transition of the monoclinic crystal to tetragonal crystal of ZrO2 crystal, it is necessary to suppress the generation of zircon crystals.
[0128] Therefore, the CaO content is preferably 0.02 to 0.3 mass%, more preferably 0.02 to 0.2 mass%, or 0.02 to 0.1 mass%, particularly preferably 0.03 to 0.2 mass%, or 0.03 to 0.1 mass%.
[0129] The total content of MgO and CaO is 0.02 to 0.4% by mass, preferably 0.02 to 0.35% by mass.
[0130] <Fe2O3 and TiO2>
[0131] Fe2O3 and TiO2 are impurities of ZrO2 raw materials and zircon raw materials. These oxides are the cause of coloring and foaming of molten glass, so it is necessary to limit the content. The total content of Fe2O3 and TiO2 is 0.5 mass% or less, preferably 0.3 mass% or less, and more preferably 0.2 mass% or less. There is no particular limitation on the lower limit, and the total content of Fe2O3 and TiO2 can be 0.01 mass% or more.
[0132] <P2O5>
[0133] P2O5 is one of the components constituting glass, and has the effect of making low-melting-point glass and adjusting the viscosity of the melt when manufacturing high-zirconia electric casting refractory. If P2O5 is contained, the formation of zircon crystals is significantly promoted, so the refractory of the present invention is preferably substantially free of P2O5. Therefore, the content of P2O5 is preferably 0.04% by mass or less, and more preferably 0.02% by mass or less.
[0134] 《Expansion coefficient of refractory materials (thermal expansion coefficient)》
[0135] The expansion rate of the refractory can be evaluated, for example, by the expansion rate of the temperature rise process at each temperature of 100° C. in the temperature range of 200° C. to 1500° C. In addition, the expansion rate of the refractory can be evaluated, for example, by the expansion rate of the temperature drop process at each temperature of 300° C. in the temperature range of 1500° C. to 300° C.
[0136] In the process of heating from 200°C to 1500°C, if the temperature at which the expansion rate of the refractory becomes the maximum is in the range of 1300°C to 1500°C, the maximum expansion portion between the surface on the outside side and the surface on the inside of the furnace of the high zirconia electric casting refractory in the prior art can be located on the inside of the furnace in contact with the molten glass, so that the joint opening can be completely or substantially completely suppressed at the contact portion between the refractory. Therefore, in the process of heating from 200°C to 1500°C, it is preferred that the temperature at which the expansion rate of the refractory becomes the maximum exists in the range of 1300°C to 1500°C.
[0137] In addition, about the expansion coefficient of the cooling process of refractory, it is preferred that ZrO2 crystal does not change to monoclinic and shrinks. When ZrO2 crystal changes from tetragonal phase to monoclinic, due to the rapid volume expansion, when zircon crystal is generated, due to the reduction of relative glass phase, the glass phase is difficult to absorb the rapid volume expansion, so the strength of refractory is reduced, which becomes the cause of cracking. Therefore, in the cooling process from 1500 ℃ to 300 ℃, it is preferred that the temperature at which the expansion coefficient of refractory becomes the maximum exists at 1200 ℃~1500 ℃. It is believed that in this case, the phase change of ZrO2 crystal from tetragonal to monoclinic does not occur or is suppressed.
[0138] According to the preferred embodiment of the refractory material to which the present invention relates, in the cooling process (cooling process) from 1500° C., ZrO2 crystal does not shrink from tetragonal phase change to monoclinic. This can be confirmed by measuring the expansion rate of the refractory material in the cooling process (cooling process) from 1500° C. at every 300° C. without the increase of the expansion rate corresponding to the phase change from tetragonal to monoclinic.
[0139] The expansion coefficient (linear expansion coefficient) of the refractory during the heating process and the cooling process can be measured using a thermomechanical analyzer (eg, TMA4000SA manufactured by NETZSCH) on a sample taken out of the refractory using a diamond drill according to JIS R 2207-3.
[0140] Example
[0141] The high zirconia electric cast refractory according to the preferred embodiment of the present invention will be described. However, the present invention is not limited to these embodiments.
[0142] 《Examples 1 to 14, Comparative Examples 15 to 24》
[0143] Refractories according to Examples 1 to 14 and Comparative Examples 15 to 24 were produced, respectively, and their physical properties and the like were evaluated.
[0144] <Manufacturing of refractory materials>
[0145] The ZrO2 raw material obtained by desiliconizing zircon sand is mixed with oxide raw materials such as SiO2, Al2O3, Na2O, B2O3, and Y2O3, and nitrate raw materials to achieve a predetermined ratio in terms of oxide conversion, and then melted in an electric arc furnace. After melting for a predetermined time, it is cast in a mold, buried in a slowly cooling material together with the mold, and slowly cooled to room temperature.
[0146] The casting mold used was made of graphite, with the product portion having dimensions of 100 mm×300 mm×300 mm, and the upper portion thereof being integrally connected to a riser portion having inner dimensions of 140 mm×235 mm×350 mm.
[0147] After slow cooling, the mold and the casting are taken out from the silica sand of the slow cooling material, and the mold is separated from the casting. As for the casting, the product part is cut off from the riser part to obtain the desired high zirconia electric casting refractory.
[0148] <Evaluation>
[0149] The physical properties of the refractory materials of Examples 1 to 14 and Comparative Examples 15 to 24 were evaluated as follows. The composition and properties of the high zirconia electric cast refractory materials of Examples 1 to 14 are shown in Table 1, and the expansion coefficients during the heating process and the cooling process are shown in Table 2. In addition, the composition and properties of the high zirconia electric cast refractory materials of Comparative Examples 15 to 24 are shown in Table 3, and the expansion coefficients during the heating process and the cooling process are shown in Table 4. The amounts of the components in Tables 1 and 3 are in mass %.
[0150] <Ingredient Analysis>
[0151] The analysis of each component was performed by wavelength dispersive fluorescent X-ray analysis. It should be noted that the B2O3 content was analyzed by high-frequency inductively coupled plasma emission spectrometry. However, the present invention is not limited to these analysis methods, and other analysis methods can also be used.
[0152] <Cracks>
[0153] Regarding cracks during manufacturing, first observe the state of the product after it is taken out from the slowly cooled material. Then, cut the product in half, observe the state of the inside, and evaluate it according to the following criteria.
[0154] +++: Refractory with no cracks on the surface or inside the block, or with no cracks on the surface and the length of the internal cracks is less than 50mm
[0155] ++: Refractory with no cracks on the surface of the block, but with cracks of 50 mm or more in length inside
[0156] +: The block has cracks on both sides and has cracks with a length of 50 mm or more inside.
[0157] -: Refractory with cracks on more than 3 sides of the block surface, or refractory that breaks due to cracks when taken out from slowly cooled material
[0158] <Bulk density and porosity>
[0159] As for the bulk density and porosity, a 23mm diameter drill core was taken out from the part 50mm away from the bottom of the mold contact part and 50mm away from the side of the mold contact part of the 300mm×300mm surface, and the bulk density and apparent porosity of the sample with a length of 90mm and an internal length of 5mm from the casting surface were calculated using the Archimedean method.
[0160] The bulk density of the refractory is preferably 5.10 g / cm 3 ~5.70g / cm 3 In addition, the porosity of the refractory is preferably 5.00% or less or 3.00% or less (the lower limit of the porosity is not particularly limited, and may be 0.80%).
[0161] <Expansion coefficient (thermal expansion coefficient)>
[0162] The expansion coefficient (linear expansion coefficient) of the refractory is measured in accordance with JIS R 2207-3. For the samples used to evaluate the expansion coefficient of the refractory, a drill core with a diameter of 5 mm is cut from a position 20 mm from the bottom of the mold contact portion of the 300 mm × 300 mm surface and 130 mm from the side of the mold contact portion, and 40 mm is cut from the surface of each casting to prepare a sample with a central length of 20 mm. In the samples taken out of the refractory, the expansion coefficient is measured using a thermomechanical analyzer. The results related to Examples 1 to 14 and Comparative Examples 15 to 24 are shown in Table 2 and Table 4, respectively. In addition, Figure 1 The results of thermal expansion coefficient measurements of high zirconium oxide electric casting refractory containing 93 mass % zirconium oxide (0.24 mass % Y2O3 content) and Examples 2 and 8 are shown in FIG. Figure 2 The results of thermal expansion coefficient measurement of a high zirconia electric cast refractory containing 93 mass % of zirconia (Y2O3 content: 0.24 mass %) and Comparative Example 16 are shown.
[0163] <Corrosion resistance>
[0164] A drill core with a diameter of 22 mm was cut out from the bottom and side surfaces of the mold contact portion of the 300 mm × 300 mm surface at a distance of 50 mm, and 5 mm was cut from the surface of the casting. The 90 mm long portion in the center was used as a sample for evaluating corrosion resistance.
[0165] exist Figure 3 2 shows a diagram of an apparatus used in the evaluation of corrosion resistance. The evaluation of corrosion resistance was performed using alkali-free glass as follows. The composition of the alkali-free glass used in this test was SiO2 62 mass%, Al2O3 16 mass%, B2O3 2 mass%, CaO 9 mass%, SrO2 mass%, and BaO 9 mass%.
[0166] <Corrosion resistance test using alkali-free glass>
[0167] Holes were processed in the sample to be evaluated and the alumina conduit for fixing the sample, and the pins of the refractory were inserted to fix the sample to be evaluated to the alumina conduit. The pins of the refractory and the alumina conduit were fixed using a heat-resistant adhesive. One end of the alumina conduit was connected to the sample to be evaluated, and the other end was connected to the test device.
[0168] Will be filled with alkali-free glass ( Figure 3 A crucible of a high zirconia electrocasting refractory material ( Figure 3 After the temperature of the sample was raised to 1700°C, the test device connected to the alumina conduit was started, and the sample to be evaluated was rotated at 40 rpm. Figure 3 1) and the alkali-free glass ( Figure 3 The alkali-free glass was brought into contact with the sample to be evaluated at a temperature of 1700° C. for 168 hours, and then the sample was lifted out of the refractory crucible to remove the glass attached to the sample to be evaluated.
[0169] Use a vernier caliper to measure the amount of corrosion at the most corroded part of the lifted sample. Figure 4 The sample with a ZrO2 content of 93 mass % (Y2O3 content of 0.24 mass %) is shown in ( Figure 4 4) and the sample involved in Example 1 ( Figure 4 Appearance after the corrosion resistance test of the reference numeral 5).
[0170] For comparison, the erosion amount of a high zirconia electrocast refractory having a ZrO2 content of 93 mass % (Y2O3 content of 0.24 mass %) was taken as a standard erosion amount and evaluated using the following criteria.
[0171] ++: Less erosion compared to standard
[0172] +: Erosion amount is the same as standard
[0173] -: More erosion than standard
[0174] For the refractory with a ZrO2 content of 93 mass% (Y2O3 content of 0.24 mass%) and the refractory involved in Example 1, photos of the internal structure after corrosion resistance evaluation were taken. Figure 5A and Figure 5B The respective photos are shown in .
[0175] <Residual volume expansion ratio after thermal cycle test>
[0176] A drill core with a diameter of 45 mm was cut from the bottom surface of the mold contact part and the mold contact part side of the 300 mm×300 mm surface at a distance of 50 mm, and a 25 mm portion was cut from each casting surface, and the central length of 50 mm was used as an evaluation sample.
[0177] The sample was heated to 600°C at a heating rate of 3°C / min and kept for 1 hour. Then, the sample was heated to 1450°C at a heating rate of 3°C / min and kept at 1450°C for 1 hour. After being kept for 1 hour, the sample was cooled to 600°C at a cooling rate of 3°C / min and kept for 1 hour. The thermal cycle was repeated 20 times, with 1 hour at 600°C and 1 hour at 1450°C being considered as one cycle. After 20 repeated thermal cycles, the residual volume expansion rate was calculated based on the volume difference of the evaluation sample obtained from the dimensions measured before and after heating.
[0178] The residual volume expansion rate calculated in this way is preferably 2% or less, and more preferably 1% or less. If the residual volume expansion rate exceeds 5%, part of the sample begins to powderize, which is not preferred, and if it exceeds 10%, the entire sample begins to powderize, which is even less preferred.
[0179] 《Evaluation Results》
[0180] Examples 1 to 14 are refractory materials with a Y2O3 content exceeding 4 mass%. Figure 1 ), in the heating process of 200°C to 1500°C, the temperature at which the expansion coefficient of the refractory becomes the maximum is in the range of 1300°C to 1500°C in Examples 1 to 14. In addition, in the cooling process of 300°C to 1500°C, the temperature at which the expansion coefficient of the refractory becomes the maximum is in the range of 1200°C or more in Examples 1 to 14. In Examples 1 to 14, no rapid volume change near the phase transition temperature of the ZrO2 crystal phase was observed. That is, in the refractory of Examples 1 to 14, the phase transition of the reversible crystal phase of the monoclinic crystal and the tetragonal crystal of ZrO2 disappears or substantially disappears, so the rapid volume change is relaxed or disappears.
[0181] Embodiment 7, 8 is the main component of glass phase, i.e., SiO2 content is relatively low refractory. Without intending to be limited by theory, it is shown that due to the effect of Y2O3, the phase transition of the reversible crystalline phase of the monoclinic crystal and tetragonal crystal of ZrO2 disappears or substantially disappears, so the phase transition of the crystalline phase accompanied by a sharp volume change is relaxed, and even if the SiO2 content is relatively low, the resistance to thermal cycling is also good.
[0182] Figure 5A This is a photograph of the internal structure of a high zirconium oxide electro-fused casting refractory containing 93 mass% zirconium oxide after corrosion resistance evaluation. The refractory contains 0.24 mass% Y2O3. Figure 5B The internal structure photos of the high zirconium oxide electric casting refractory involved in Example 1 after the evaluation of corrosion resistance (Y2O3 content = 5.67 mass%). As these photos suggest, it is believed that in refractory with Y2O3 content exceeding 4 mass%, it is easy to form a network between ZrO2 particles through the nodules formed by crystallization of a part of Y2O3 contained in the glass phase or the high concentration of Y2O3 nodules formed by dissolution of Y2O3 dissolved in ZrO2. Therefore, as in Examples 7, 8, and 11, even if the porosity becomes relatively high, it has the same or higher corrosion resistance as the high zirconium oxide electric casting refractory with a ZrO2 content of 93 mass%.
[0183] In Examples 5 and 11, it is shown that the component (CaO or B2O3) that promotes the formation of zircon crystals is increased, but if the Y2O3 content exceeds 4 mass %, even if zircon crystals are generated, the phase transition of the ZrO2 crystal from monoclinic to tetragonal accompanied by a sharp volume change is slowed down, so if the residual expansion rate is less than 2%, the resistance to thermal cycles is good.
[0184] It can also be seen from Table 1 that after the high zirconia electric cast refractory of Examples 1 to 14 is taken out from the slowly cooled material, the crack length is short or there is no crack in appearance. Therefore, even if cracks occur, mass production can be achieved industrially by partially cutting them off, the opening of the joints can be suppressed, the residual expansion coefficient to the thermal cycle can be suppressed, and they can be used as long-life refractory with high corrosion resistance to glass.
[0185] Table 3 shows refractory materials not belonging to the present invention as comparative examples. All refractory materials involved in comparative examples 15 to 24 show poor quality in terms of cracking during manufacturing. In addition, some comparative examples also show poor quality in terms of corrosion resistance and / or residual volume expansion rate after thermal cycling.
[0186] Among the comparative examples, comparative examples 15 to 17 are refractory materials with relatively low Y2O3 content, and comparative example 15 is a composition corresponding to patent document 4 (Japanese publication No. 2013-514254). Without intending to be limited by theory, it is believed that in these comparative examples, a relatively small amount of Y2O3 is contained, and as a result, the phase transition temperature of the ZrO2 crystal from the monoclinic crystal to the tetragonal crystal migrates to the low temperature side, and at the low temperature side, the viscosity of the glass phase is high, so the rapid volume change of ZrO2 cannot be alleviated, and the refractory material breaks when taken out from the slowly cooled material.
[0187] On the contrary, Comparative Example 19 is a refractory with a relatively high content of Y2O3. In this comparative example, Y2O3 is dissolved in ZrO2 crystals and a part of it is stabilized as cubic ZrO2, so cracks may be easily generated.
[0188] In the refractory materials involved in Comparative Examples 18 and 20 to 24, it is considered that although the Y2O3 content is in the range of more than 4.0 mass % to 9.0 mass %, at least one component among SiO2, Al2O3, B2O3, Fe2O3, TiO2, MgO, CaO, K2O, and P2O5 is excessive or insufficient, so cracks occur.
[0189] The refractories according to these comparative examples are difficult to mass-produce industrially and may not be suitable for stable production.
[0190] Based on the above results, the high zirconia electric cast refractory of the present invention suppresses erosion by glass due to seam opening, has high corrosion resistance, and exhibits good resistance to thermal cycles, and is very useful as a refractory for a glass melting furnace.
[0191] In addition, the high zirconia electric cast refractory of the present invention is very useful when used in a glass melting furnace, but is not limited to the use in a glass melting furnace.
[0192] [Table 1]
[0193]
[0194] [Table 2]
[0195]
[0196] [Table 3]
[0197]
[0198] [Table 4]
[0199]
[0200] Description of Reference Numerals
[0201] 1 Samples for evaluation of corrosion resistance
[0202] 2 Molten Glass
[0203] 3 Crucible for high zirconia electric casting refractory
[0204] 4 High zirconia electric casting refractory with 93% zirconium oxide by mass after corrosion resistance test
[0205] 5 Refractory of Example 1 after Corrosion Resistance Test
Claims
1. High zirconia electro-cast refractory, including: As chemical components, the total of ZrO2 and HfO2 is more than 80 mass% and less than 92 mass%, Al2O3 is 0.2~3.0 mass%, SiO2 is 1.5~10 mass%, Na2O is 0.05~2.0 mass%, K2O is less than 1.0 mass%, B2O3 is 0~1.5 mass%, Y2O3 is more than 4.0 mass% and less than 9.0 mass%, the total of MgO and CaO is 0.02~0.4 mass%, CaO is more than 0.01 mass%, the total of Fe2O3 and TiO2 is less than 0.5 mass%, and the content of P2O5 is less than 0.04 mass%.
2. The high zirconia electric cast refractory according to claim 1, wherein: As chemical components, the total of ZrO2 and HfO2 is more than 80 mass% and less than 92 mass%, Al2O3 is 0.4~2.5 mass%, SiO2 is 1.5~7.0 mass%, Na2O is 0.3~1.8 mass%, K2O is less than 1.0 mass%, B2O3 is 0~1.0 mass%, Y2O3 is more than 4.0 mass% and less than 7.5 mass%, the total of MgO and CaO is 0.02~0.4 mass%, CaO is more than 0.01 mass%, the total of Fe2O3 and TiO2 is less than 0.5 mass%, and the content of P2O5 is less than 0.04 mass%.
3. The high zirconia electric cast refractory according to claim 1 or 2, wherein: The mass content of Y2O3 is 4.5 to 7.5 mass%.
4. The high zirconia electric cast refractory according to claim 3, wherein: The mass content of Y2O3 is more than 4.5 mass% and less than 6.0 mass%.
5. The high zirconia electric cast refractory according to any one of claims 1 to 4, wherein The mass content of SiO2 is 4.0 to 6.5 mass%.
6. The high zirconia electric cast refractory according to any one of claims 1 to 5, wherein The mass content of Al2O3 is 0.5 to 1.2 mass%.
7. The high zirconia electric cast refractory according to any one of claims 1 to 6, wherein The mass content of Na2O is 0.5 to 1.2 mass%.
8. The high zirconia electric cast refractory according to any one of claims 1 to 7, wherein The mass content of B2O3 is 0.01 to 0.6 mass%.
9. The high zirconia electric cast refractory according to any one of claims 1 to 8, wherein In the process of heating from 200°C to 1500°C, the temperature at which the expansion coefficient of the refractory reaches a maximum exists in the range of 1300°C to 1500°C.
10. The high zirconia electric cast refractory according to any one of claims 1 to 9, wherein During the cooling process from 1500℃, the ZrO2 crystals do not change from tetragonal to monoclinic phase but shrink.
11. The high zirconia electric fused cast refractory according to any one of claims 1 to 10, which is used in a glass melting furnace.
Citation Information
Patent Citations
Fused cast refractory products with high zirconia content
JP2005526683A
Refractories with a high zirconia content
JP2013514254A
High zirconia electrically melted cast refractory
JP2015040144A
Refractory having high zirconia content
JP2015212223A
Refractory products with a high zirconia content
JP2015506898A