Method for manufacturing polycrystalline silicon wafer
By forming a film on a silicon single crystal substrate by using the CVD method and controlling the inner-plane film thickness distribution of the first polysilicon layer in the polysilicon wafer manufacturing, the problems of tiny shape adjustment and deviation in the prior art are solved, and high reproduction is achieved polysilicon wafer manufacturing is suitable for mass production of RF devices.
Patent Information
- Application Number
- CN202380033330.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-15
- Filing Date
- 2023-03-08
- Publication Date
- 2024-11-08
AI Technical Summary
The existing polysilicon wafer manufacturing method is difficult to adjust the tiny shape, and the deviation between the film forming device or chamber is difficult to reduce, resulting in poor reproducibility.
The CVD method is used to form a film on a silicon single crystal substrate. The first polysilicon layer is formed at a temperature below 1000°C, and the second polysilicon layer is formed at a temperature above 1000°C, and the inner film thickness is distributed on the first layer. The difference between the maximum value and the minimum value is within 5.2%, ensuring the stability of the wafer shape.
Even if the film forming device or chamber is different, the deviation of the tiny wafer shape can be reduced, and polysilicon wafer manufacturing with good reproducibility can be achieved, which is particularly suitable for mass production of RF devices.
Smart Images

Figure CN118922913A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for manufacturing a polycrystalline silicon wafer, and in particular to a method for manufacturing a polycrystalline silicon wafer capable of controlling the wafer shape of the polycrystalline silicon wafer with good reproducibility. Background Art
[0002] Since the noise characteristics of RF devices vary depending on the shape (Bow) of polycrystalline silicon (Poly-Si) wafers, it is necessary to control its tiny shape. As a polycrystalline silicon film formation process, a two-layer growth process (first layer: low temperature deposition + second layer: high temperature deposition) for improving productivity is well known, and the wafer shape can be adjusted by its film formation temperature or film thickness.
[0003] As a method for controlling the shape of a substrate, Patent Document 1 discloses a method for manufacturing by measuring the curved surface of a wafer, determining the curvature direction of the curved surface, and mounting polysilicon on any one surface to reduce the warping. Patent Document 2 describes a manufacturing method for suppressing the warping by making the shape of the front and back surfaces the same when growing a SiC film by CVD on a carbon substrate.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Publication No. 2009-295889
[0007] Patent Document 2: Japanese Patent Application Laid-Open No. 11-016991 Summary of the invention
[0008] 1. Technical issues to be resolved
[0009] However, it is difficult to adjust minute shapes using existing methods, and it is necessary to reduce the deviation between film forming devices or chambers.
[0010] The present invention has been made to solve the above-mentioned problems, and an object of the present invention is to provide a method for manufacturing a polycrystalline silicon wafer that can reduce minute wafer shape deviations and manufacture polycrystalline silicon wafers with good reproducibility even if film forming apparatuses or chambers are different.
[0011] (II) Technical solution
[0012] In order to solve the above technical problems, the present invention provides a method for manufacturing a polycrystalline silicon wafer, which is a method for manufacturing a polycrystalline silicon wafer having a polycrystalline silicon layer formed on a silicon single crystal substrate, and has the following steps:
[0013] (1) forming a first polycrystalline silicon layer on a silicon single crystal substrate at a temperature of 1000° C. or less by CVD;
[0014] (2) forming a second polysilicon layer on the first polysilicon layer at a temperature higher than 1000° C. by using a CVD method, and
[0015] In the step (1), the value (%) of the in-plane film thickness distribution of the formed first polysilicon layer is controlled within a predetermined range, and the difference between the maximum value (%) and the minimum value (%) of the predetermined range is within 5.2 (%).
[0016] According to such a method for manufacturing a polycrystalline silicon wafer, even if a film forming apparatus or a chamber is different, it is possible to reduce minute variations in wafer shape and manufacture a polycrystalline silicon wafer with good reproducibility.
[0017] Furthermore, in the step (1), it is preferred that the maximum value (%) of the predetermined range be controlled to be 1.5% or less.
[0018] By controlling the in-plane film thickness distribution in this manner, it is possible to more stably reduce minute variations in wafer shape and manufacture polycrystalline silicon wafers with good reproducibility.
[0019] Furthermore, in the step (1), preferably, the in-plane temperature distribution of the silicon single crystal substrate is controlled to control the in-plane film thickness distribution of the first polycrystalline silicon layer to be formed.
[0020] In this manner, the in-plane film thickness distribution of the first polycrystalline silicon layer can be easily controlled.
[0021] In addition, the present invention provides a method for manufacturing a polycrystalline silicon wafer, which is a method for manufacturing a polycrystalline silicon wafer using two or more different manufacturing equipments, wherein:
[0022] In the two or more different manufacturing equipments, the polycrystalline silicon wafers are manufactured using the above-mentioned method for manufacturing a polycrystalline silicon wafer.
[0023] The method for manufacturing a polycrystalline silicon wafer of the present invention is extremely useful for mass production of polycrystalline silicon wafers using two or more different manufacturing equipments.
[0024] (III) Beneficial effects
[0025] As described above, the method for manufacturing polycrystalline silicon wafers of the present invention can reduce small deviations in wafer shape and manufacture polycrystalline silicon wafers with good reproducibility even if the film forming apparatus or chamber is different. In particular, the present invention is extremely useful in mass production of Si wafers for RF devices in which wafer shape is controlled with high precision. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1Graph showing the relationship between the in-plane film thickness distribution of the first polysilicon layer in Example 1 and Comparative Example 1 and the Bow value of the obtained wafer.
[0027] Figure 2 This is an example of a schematic diagram showing the CVD temperature in each step in the method for manufacturing a polycrystalline silicon wafer of the present invention.
[0028] Figure 3 The diagram is an example of a schematic diagram showing a film forming process of a polycrystalline silicon layer in each step in the method for manufacturing a polycrystalline silicon wafer of the present invention.
[0029] Figure 4 Schematic diagram of the polysilicon growth reactor used in the embodiment. DETAILED DESCRIPTION
[0030] In the two-layer growth process (first layer: low temperature deposition + second layer: high temperature deposition), the wafer shape can be adjusted by the film formation temperature or film thickness. However, these methods are difficult to adjust the fine shape and make fine adjustments to the deviation between film formation devices or chambers.
[0031] The inventors of the present application have repeatedly conducted in-depth studies on the above-mentioned technical problems, and as a result, have found that by controlling the in-plane film thickness distribution of the first layer of the polysilicon layer within a specified range, even if the film forming device or chamber is different, the tiny shape can be adjusted, and polysilicon wafers of the same level of wafer shape can be manufactured with good reproducibility, thereby completing the present invention.
[0032] That is, the present invention is a method for manufacturing a polycrystalline silicon wafer, which is a method for manufacturing a polycrystalline silicon wafer having a polycrystalline silicon layer formed on a silicon single crystal substrate, and comprises: (1) a process of forming a first polycrystalline silicon layer on a silicon single crystal substrate at a temperature below 1000°C by a CVD method; (2) a process of forming a second polycrystalline silicon layer on the first polycrystalline silicon layer at a temperature above 1000°C by a CVD method, and in the process (1), the value (%) of the in-plane film thickness distribution of the formed first polycrystalline silicon layer is controlled within a predetermined range, and the difference between the maximum value (%) and the minimum value (%) of the predetermined range is within 5.2 (%).
[0033] Hereinafter, the present invention will be described in detail, but the present invention is not limited thereto.
[0034] [Manufacturing method of polycrystalline silicon wafer]
[0035] The method for manufacturing a polycrystalline silicon wafer of the present invention comprises steps (1) and (2). Figure 2 , 3 Provide detailed explanation.
[0036] <Process (1)>
[0037] Process (1) is a process of forming a first polycrystalline silicon layer on a silicon single crystal substrate at a temperature below 1000°C using a CVD method. In this process, the value (%) of the in-plane film thickness distribution of the formed first polycrystalline silicon layer is controlled within a predetermined range, and the difference between the maximum value (%) and the minimum value (%) of the predetermined range is within 5.2 (%).
[0038] There is no particular limitation on the silicon single crystal substrate. For example, it can be a CZ single crystal or a FZ single crystal, and it can be doped or undoped. In addition, in the case of doping, the type and concentration of the dopant are not particularly limited, and for example, P, Sb or As doping in n-type, B, Al or Ga doping in p-type, etc. can be listed. The diameter of the substrate is not particularly limited, and for example, the diameter can be set to 100~300mm. The resistivity of the substrate is also not particularly limited, and for example, the resistivity can be set to a high resistance of more than 5000Ω·cm.
[0039] like Figure 2 As shown, in this process, the film is formed by a CVD method at a low temperature of 1000°C or less. The film forming temperature at this time is not particularly limited as long as it is 1000°C or less, and can be preferably set to less than 980°C. In addition, the lower limit of the film forming temperature is not particularly limited, and can be set to 800°C or more, for example. Figure 3 As shown, in this step, a first polysilicon layer 2 is formed as a seed layer on a silicon single crystal substrate 1 by film formation at a low temperature.
[0040] At this time, by controlling the value (%) of the in-plane film thickness distribution of the first polysilicon layer 2 within the above-predetermined range, a polysilicon wafer having a desired warpage shape can be obtained after forming the second polysilicon layer in the later-described step (2). On the other hand, if the value (%) of the in-plane film thickness distribution of the first polysilicon layer is not controlled within the above-predetermined range, even if the value (%) of the in-plane film thickness distribution of the second polysilicon layer is accurately controlled in the later-described step (2), wafers of the same level of shape cannot be manufactured with good reproducibility.
[0041] There is no particular limitation on the method for controlling the in-plane film thickness distribution of the formed first polycrystalline silicon layer, and a conventionally known method may be used. For example, it is preferred to control the in-plane film thickness distribution of the formed first polycrystalline silicon layer by controlling the in-plane temperature distribution of the silicon single crystal substrate. There is no particular limitation on the method for controlling the in-plane temperature distribution of the silicon single crystal substrate, and a function of a commonly used film forming apparatus may be used.
[0042] In the present invention, as the value (%) of the in-plane film thickness distribution, a value calculated by a known method may be used, and for example, a value calculated by the following mathematical formula may be used.
[0043] In-plane film thickness distribution (%) = (maximum film thickness - minimum film thickness) / (maximum film thickness + minimum film thickness) × 100
[0044] The predetermined range is not particularly limited as long as the difference between the maximum value (%) and the minimum value (%) of the range is within 5.2 (%). That is, the value (%) of the in-plane film thickness distribution of the first polysilicon layer itself can be higher or lower, as long as the value (%) of the in-plane film thickness distribution can be controlled with high precision. That is, the in-plane film thickness distribution (%) can be controlled with high precision at a higher value, or it can be controlled with high precision at a lower value. It can be said that regardless of whether the in-plane film thickness distribution (%) of the first polysilicon layer is in a uniform direction or a deteriorated direction, as long as the film thickness distribution is of the same level, the wafer shape can be adjusted to the same level. The difference between the maximum value (%) and the minimum value (%) of a predetermined range can be set to greater than 0 (%), but from the perspective of more reproducible wafer manufacturing, the difference between the maximum value (%) and the minimum value (%) of the predetermined range is preferably controlled to within 3%, more preferably to within 1.5%, further preferably to within 1.0%, extremely preferably to within 0.5%, and particularly preferably to 0% (constant each time).
[0045] In addition, the value (%) of the in-plane film thickness distribution of the formed first polysilicon layer can be controlled, for example, so that the maximum value (%) of the predetermined range is less than 10%, and from the perspective of being able to more stably adjust the wafer shape to the same level, it is preferably controlled so that the maximum value (%) is less than 1.5%. In addition, the maximum value (%) of the predetermined range can be set to more than 0%.
[0046] The predetermined range will be described below with more specific examples.
[0047] (Specific example 1)
[0048] When the in-plane film thickness distribution value (%) of the first polysilicon layer is controlled to be a constant value of 1.5%, since the maximum value of the predetermined range is 1.5 (%) and the minimum value is also 1.5 (%), the difference between the maximum value (%) and the minimum value (%) of the predetermined range is 0 (%).
[0049] (Specific example 2)
[0050] When the in-plane film thickness distribution value (%) of the first polysilicon layer is controlled to be 1.5%±0.5%, since the maximum value of the predetermined range is 2.0 (%) and the minimum value is 1.0 (%), the difference between the maximum value (%) and the minimum value (%) of the predetermined range is 1 (%).
[0051] (Concrete example 3)
[0052] When the in-plane film thickness distribution value (%) of the first polysilicon layer is controlled to be a constant value of 6.8%, since the maximum value of the predetermined range is 6.8 (%) and the minimum value is also 6.8 (%), the difference between the maximum value (%) and the minimum value (%) of the predetermined range is 0 (%).
[0053] (Concrete example 4)
[0054] When the in-plane film thickness distribution value (%) of the first polysilicon layer is controlled to be 6.8%±0.5%, since the maximum value of the predetermined range is 7.3 (%) and the minimum value is 6.3 (%), the difference between the maximum value (%) and the minimum value (%) of the predetermined range is 1 (%).
[0055] <Process (2)>
[0056] Step (2) is a step of forming a second polysilicon layer on the first polysilicon layer at a temperature higher than 1000° C. by using a CVD method.
[0057] like Figure 2 As shown, in this process, in order to increase the growth rate and thus the productivity, a CVD method at a high temperature higher than 1000°C is used to form a film to a desired film thickness. The film forming temperature at this time is not particularly limited as long as it is higher than 1000°C, and can be preferably set to 1050°C or higher. In addition, the upper limit of the film forming temperature is not particularly limited, and can be set to 1200°C or lower, for example. Figure 3 As shown, in this process, the second polysilicon layer 3 can be formed on the first polysilicon layer 2 by film formation at a high temperature, thereby obtaining a polysilicon wafer 4.
[0058] For the second polysilicon layer, it is also preferred to control the in-plane film thickness distribution (%) within a predetermined range similarly to the first polysilicon layer. By accurately controlling the in-plane film thickness distribution of the second polysilicon layer, wafers of the same shape can be manufactured with better reproducibility.
[0059] In addition, the ratio of the thickness of the first polysilicon layer formed in step (1) to the thickness of the second polysilicon layer formed in step (2) is arbitrarily set. However, since the growth rate of the polysilicon layer increases under high temperature conditions, from the perspective of improving productivity, it is preferred to design the process so that the film formed in step (2) is thicker than that in step (1).
[0060] As described above, according to the present invention, even if the film forming apparatus or the chamber is different, it is possible to reduce minute variations in wafer shape and manufacture polycrystalline silicon wafers with good reproducibility.
[0061] [Method for manufacturing a polycrystalline silicon wafer using two or more different manufacturing equipments]
[0062] In addition, the present invention provides a method for manufacturing polycrystalline silicon wafers, which is a method for manufacturing polycrystalline silicon wafers using more than two different manufacturing equipment to manufacture polycrystalline silicon wafers, wherein the polycrystalline silicon wafers are manufactured using the above-mentioned method for manufacturing polycrystalline silicon wafers in the more than two different manufacturing equipments respectively.
[0063] As described above, the method for manufacturing polycrystalline silicon wafers of the present invention can reduce the deviation of the tiny wafer shape and manufacture polycrystalline silicon wafers with good reproducibility even if the film forming device or chamber is different. That is, regardless of the type of manufacturing equipment, polycrystalline silicon wafers of the same quality can be manufactured with good reproducibility. Therefore, the method for manufacturing polycrystalline silicon wafers of the present invention is particularly suitable for using multiple manufacturing equipment to mass-produce polycrystalline silicon wafers in parallel.
[0064] Example
[0065] Hereinafter, the present invention will be specifically described using Examples and Comparative Examples, but the present invention is not limited thereto.
[0066] In the following Examples 1 to 3 and Comparative Example 1, the film thickness distribution is adjusted by adjusting the temperature distribution of the silicon single crystal substrate during polycrystalline silicon growth. However, the film thickness distribution adjustment method in the present invention is not limited thereto.
[0067] A schematic diagram showing a single-wafer vapor phase growth apparatus (reactor) for growing polycrystalline silicon used in the following Examples 1 to 3 and Comparative Example 1 is shown in FIG. Figure 4. The chamber (reaction container) 12 of the vapor phase growth device 10 is formed by a chamber base 11 and transparent quartz components 13 and 14 that clamp the chamber base 11 from the top and bottom. A susceptor 17 that supports the silicon single crystal substrate W using a wafer loading surface (countersunk portion) 19 on the upper surface is arranged in the chamber 12. The susceptor 17 is provided with, for example, three or more through holes 16, and is provided with wafer lifting pins 15. The wafer lifting pins 15 are inserted into the through holes 16 and move up and down to load and separate the silicon single crystal substrate W. The susceptor 17 is connected to a wafer rotating mechanism 18. By rotating the susceptor 17 during epitaxial growth, the mounted silicon single crystal substrate W is rotated, so that the polycrystalline silicon layer grows on the silicon single crystal substrate W with a uniform film thickness. The chamber 12 is connected to a gas introduction pipe 20, which introduces a gas phase growth gas including a raw material gas and a carrier gas (e.g., hydrogen) into the chamber 12, thereby supplying the raw material gas and the carrier gas to the surface of the silicon single crystal substrate W placed on the susceptor 17. In addition, a gas exhaust pipe 21 for exhausting gas from the chamber 12 is connected to the side of the chamber 12 opposite to the side connected to the gas introduction pipe 20.
[0068] (Example 1)
[0069] The following experiment was conducted using two different reactors (RCT-A and RCT-B). A silicon single crystal substrate with a resistivity of 5000 Ω·cm or more and a diameter of 200 mm containing boron as an impurity was prepared. A polycrystalline silicon wafer as a sample was manufactured by performing a CVD method on the silicon single crystal substrate. In the CVD method, a non-doped polycrystalline silicon film (first polycrystalline silicon layer) with a polycrystalline silicon film thickness of 0.3 μm (first layer) was grown at a growth temperature of 870°C using trichlorosilane (TCS) as a film-forming gas. Then, the growth temperature was changed to 1070°C, and a non-doped polycrystalline silicon film (second polycrystalline silicon layer) with a polycrystalline silicon film thickness of 1.9 μm (second layer) was continuously formed.
[0070] At this time, in the film forming process of the first layer of RCT-A and B, the film thickness distribution is adjusted to 1.5% (the difference between the maximum value (%) and the minimum value (%) in the predetermined range is controlled to 0 (%), and at the same time, the film thickness distribution of the second layer of RCT-A and B is also adjusted to 1.5%.
[0071] The wafer shape (Bow) of the polycrystalline silicon wafer manufactured at this time was measured. Figure 1 The result at this time is shown in FIG. Figure 1 It was confirmed that the Bow values of the wafers manufactured in RCT-A and B were both about 4.35 μm, and that by making the film thickness distribution of the first layer of RCT-A and B the same level, the same level of wafer shape could be reproduced.
[0072] Figure 1 The left figure in the figure is a graph obtained by plotting the film thickness on the wafer surface after the first layer is formed thicker than the original 0.3μm (the film is formed to be about 2.5μm) in order to confirm the film thickness distribution of the first layer. In addition, the horizontal axis of the above left figure represents the film thickness measurement position, CTR: wafer center, R / 2: 50mm from the wafer center, 10mm: 90mm from the wafer center (10mm from the periphery). Figure 1 The right figure in the figure shows the Bow value of the wafer when the film is formed according to the designed film thickness (0.3μm for the first layer and 1.9μm for the second layer). In addition, whether the first layer is formed to the original 0.3μm or the film is formed to be thicker than the original 0.3μm, the calculated value of the in-plane film thickness distribution (%) is theoretically the same value.
[0073] (Example 2)
[0074] The polycrystalline silicon wafer was manufactured in the same manner as in Example 1, except that the film thickness distribution was adjusted to 1.5% in the film forming process of the first layer of RCT-A and the film thickness distribution was adjusted to 6.7% in the film forming process of the first layer of RCT-B (the difference between the maximum value (%) and the minimum value (%) in the predetermined range was controlled to 5.2 (%)). In addition, the film thickness distribution of the second layer of RCT-A and B was also adjusted to 1.5% as in Example 1.
[0075] The wafer shape (Bow) of the polycrystalline silicon wafer manufactured in Example 2 was measured. The results showed that the Bow values of the wafers manufactured in RCT-A and B were both about 4.35 μm. Wafers with the same level of shape (Bow) were obtained in RCT-A and RCT-B.
[0076] (Example 3)
[0077] The polycrystalline silicon wafer was manufactured in the same manner as in Example 1, except that the film thickness distribution was adjusted to 6.8% in the film forming process of the first layer of RCT-A and the film thickness distribution was adjusted to 6.8% in the film forming process of the first layer of RCT-B (the difference between the maximum value (%) and the minimum value (%) in the predetermined range was controlled to 0 (%)). In addition, the film thickness distribution of the second layer of RCT-A and B was also adjusted to 1.5% as in Example 1.
[0078] The wafer shape (Bow) of the polycrystalline silicon wafer manufactured in Example 3 was measured. The results showed that the Bow values of the wafers manufactured in RCT-A and B were both about 3.20 μm. Wafers with the same level of shape (Bow) were obtained in RCT-A and RCT-B.
[0079] (Comparative Example 1)
[0080] The polycrystalline silicon wafer was manufactured in the same manner as in Example 1, except that the film thickness distribution was adjusted to 1.5% in the film forming process of the first layer of RCT-A and 6.8% in the film forming process of the first layer of RCT-B (the difference between the maximum value (%) and the minimum value (%) in the predetermined range was controlled to 5.3 (%)). In addition, the film thickness distribution of the second layer of RCT-A and B was also adjusted to 1.5% as in Example 1.
[0081] The wafer shape (Bow) of the polycrystalline silicon wafer manufactured at this time was measured. Figure 1 The result at this time is shown in FIG. Figure 1 It was confirmed that the Bow of the wafer manufactured in RCT-A was about 4.35μm, while the Bow of the wafer manufactured in RCT-B was about 3.20μm. Since the in-plane film thickness distribution of the first polysilicon layer was not controlled to within the range of 5.2(%) between the maximum value (%) and the minimum value (%), the wafer shapes were different.
[0082] This specification includes the following inventions.
[0083] [1]: A method for manufacturing a polycrystalline silicon wafer, which is a method for manufacturing a polycrystalline silicon wafer having a polycrystalline silicon layer formed on a silicon single crystal substrate, characterized in that it comprises: (1) a step of forming a first polycrystalline silicon layer on a silicon single crystal substrate at a temperature below 1000°C by a CVD method; (2) a step of forming a second polycrystalline silicon layer on the first polycrystalline silicon layer at a temperature above 1000°C by a CVD method, and in the step (1), the value (%) of the in-plane film thickness distribution of the formed first polycrystalline silicon layer is controlled within a predetermined range, and the difference between the maximum value (%) and the minimum value (%) of the predetermined range is within 5.2 (%).
[0084] [2]: The method for manufacturing a polycrystalline silicon wafer according to [1] above, characterized in that, in the step (1), the maximum value (%) of the predetermined range is controlled to be less than 1.5%.
[0085] [3]: The method for manufacturing a polycrystalline silicon wafer according to the above-mentioned [1] is characterized in that, in the step (1), the in-plane temperature distribution of the silicon single crystal substrate is controlled to control the in-plane film thickness distribution of the first polycrystalline silicon layer formed.
[0086] [4]: The method for manufacturing a polycrystalline silicon wafer according to the above-mentioned [2] is characterized in that, in the step (1), the in-plane temperature distribution of the silicon single crystal substrate is controlled to control the in-plane film thickness distribution of the first polycrystalline silicon layer formed.
[0087] [5]: A method for manufacturing polycrystalline silicon wafers, which is a method for manufacturing polycrystalline silicon wafers using two or more different manufacturing equipment to manufacture polycrystalline silicon wafers, characterized in that the polycrystalline silicon wafers are manufactured using the method for manufacturing polycrystalline silicon wafers described in [1], [2], [3] or [4] above in the two or more different manufacturing equipments, respectively.
[0088] The present invention is not limited to the above-mentioned embodiments. The above-mentioned embodiments are merely examples, and any technical solution having substantially the same configuration as the technical concept described in the claims of the present invention and having the same function and effect is included in the technical scope of the present invention.
Claims
1. A method for manufacturing a polycrystalline silicon wafer, which is a method for manufacturing a polycrystalline silicon wafer by forming a polycrystalline silicon layer on a silicon single crystal substrate, characterized in that: have: (1) forming a first polycrystalline silicon layer on a silicon single crystal substrate at a temperature of 1000° C. or less by CVD; (2) forming a second polysilicon layer on the first polysilicon layer at a temperature higher than 1000° C. by using a CVD method, and In the step (1), the value (%) of the in-plane film thickness distribution of the formed first polysilicon layer is controlled within a predetermined range, and the difference between the maximum value (%) and the minimum value (%) of the predetermined range is within 5.2 (%).
2. The method for manufacturing a polycrystalline silicon wafer according to claim 1, wherein: In the step (1), the maximum value (%) of the predetermined range is controlled to be 1.5% or less.
3. The method for manufacturing a polycrystalline silicon wafer according to claim 1, characterized in that: In the step (1), the in-plane temperature distribution of the silicon single crystal substrate is controlled to control the in-plane film thickness distribution of the formed first polycrystalline silicon layer.
4. The method for manufacturing a polycrystalline silicon wafer according to claim 2, characterized in that: In the step (1), the in-plane temperature distribution of the silicon single crystal substrate is controlled to control the in-plane film thickness distribution of the formed first polycrystalline silicon layer.
5. A method for manufacturing a polycrystalline silicon wafer, which is a method for manufacturing a polycrystalline silicon wafer using two or more different manufacturing equipments, characterized in that: In the two or more different manufacturing equipments, the polycrystalline silicon wafer is manufactured using the method for manufacturing a polycrystalline silicon wafer according to any one of claims 1 to 4.