Composition for surface protection, surface protection sheet, and method for producing electronic component device

By using surface protection compositions of hydrophilic group polymers and active compounds, the complex problem of protective layer removal in the prior art is solved, and simple removal under water contact is achieved, and the reliability and manufacturing efficiency of electronic components are improved. .

CN118922914APending Publication Date: 2024-11-08NITTO DENKO CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380029843.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-06
Filing Date
2023-04-03
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In the existing electronic component manufacturing methods, the removal process of the surface protective layer is complicated and not simple enough, especially when it comes into contact with water, which affects product reliability.

Method used

The protective layer formed is easily removed when water contacts are used to utilize a surface protection composition of a polymer containing a hydrophilic group and a compound that produces an acid or a base by heating or active energy rays.

Benefits of technology

The hydrophilicity of the protective layer is improved, making it easier to dissolve and remove after water contact, simplifying the process and enhancing the reliability and production efficiency of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118922914A_ABST
    Figure CN118922914A_ABST
Patent Text Reader

Abstract

Provided is a surface protection composition and the like that protects at least one surface of a substrate, the surface protection composition comprising a polymer having a hydrophilic group in the molecule and a compound that generates an acid or a base by heating or / and irradiation with an active energy ray.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims the priority of Japanese Patent Application No. 2022-063386, which is incorporated into the description of the present application specification by reference. Technical Field

[0003] The present invention relates to a surface protective composition and a surface protective sheet for use in manufacturing electronic components such as semiconductor integrated circuits, and also to a method for manufacturing an electronic component using the surface protective composition or the surface protective sheet. Background Art

[0004] Conventionally, there is known a method for manufacturing an electronic component device, for example, when manufacturing an electronic component device such as a semiconductor integrated circuit, etc. In such a method for manufacturing an electronic component device, for example, a substrate such as a silicon wafer is divided into small pieces to produce a large number of chips.

[0005] During such processing, sometimes when the substrate is divided into small pieces, a very small part of the substrate becomes a tiny piece, thereby generating tiny foreign matter. When a circuit structure element such as a circuit wiring or an electrode portion is arranged on one surface of the substrate, sometimes tiny foreign matter will adhere to the circuit wiring or the electrode portion. In addition, sometimes foreign matter will also adhere to the other surface where the circuit structure element such as the circuit wiring or the electrode portion is not arranged. If a large amount of foreign matter is attached to the surface of the substrate, the product reliability of the manufactured electronic component device may be reduced regardless of whether the circuit structure element is arranged on the surface to which the foreign matter is attached.

[0006] In contrast, a method for manufacturing an electronic component device is known in which a protective pressure-sensitive adhesive tape is attached to at least one surface of a substrate and then the above-mentioned processing is performed (for example, Patent Document 1).

[0007] In the manufacturing method of the electronic component device described in Patent Document 1, the following semiconductor protective adhesive tape is used as the protective adhesive tape, wherein the semiconductor protective adhesive tape has: a substrate and a photocurable adhesive layer (protective layer) superimposed on one side of the substrate. The substrate is designed to have a specific thickness and a specific heat shrinkage rate after heating at 150° C. for 30 minutes. In addition, the photocurable adhesive layer (protective layer) is designed to be formed of a composition composed of a specified formula, has a specified thickness, and has a small specified adhesive force after light irradiation.

[0008] In more detail, in the manufacturing method of the electronic component device described in Patent Document 1, first, the photocurable adhesive layer (protective layer) of the protective adhesive tape is superimposed on the circuit surface of the substrate (hereinafter referred to as the semiconductor package) on which the circuit is formed, and the protective adhesive tape is divided into small pieces while being superimposed on the semiconductor package. Next, the semiconductor package and the protective adhesive tape that have been cut into small pieces are attached to the temporary fixing tape in such a manner that the circuit surface of the semiconductor package that has been cut into small pieces is opposite to the temporary fixing tape, and in such a manner that the temporary fixing tape is in contact with the substrate of the protective adhesive tape. Next, a metal film is formed on a portion of the surface of the semiconductor package in a temporarily fixed state. Finally, the circuit surface of the semiconductor package and the photocurable adhesive layer are peeled off, and the semiconductor package is picked up.

[0009] According to the manufacturing method of the electronic component device described in Patent Document 1, when the semiconductor package and the protective adhesive tape are processed into small pieces, the circuit surface of the semiconductor package can be protected by covering the circuit surface of the semiconductor package with the protective adhesive tape. Afterwards, the circuit surface of the semiconductor package and the photocurable adhesive layer of the protective adhesive tape fixed to the temporary fixing tape are peeled off, and the protective adhesive tape can be removed. The peeling force when removing the photocurable adhesive layer (protective layer) of the protective adhesive tape is weakened because the photocurable adhesive layer is cured by light irradiation. In addition, the heat when the metal film is formed on a part of the surface of the semiconductor package causes shrinkage stress (residual deformation) to be generated inside the substrate, and the substrate is easily deformed due to the shrinkage stress (residual deformation), so the above-mentioned peeling is easy to occur.

[0010] Prior art literature

[0011] Patent Literature

[0012] Patent Document 1: Japanese Patent Application Publication No. 2021-147579 Summary of the invention

[0013] Problems to be solved by the invention

[0014] However, in the manufacturing method of the electronic component device described in Patent Document 1, in order to prevent the circuit surface from being damaged by the peeling force when peeling the circuit surface of the semiconductor package and the photocurable adhesive layer (protective layer), for example, it is necessary to adjust the peeling speed, etc., and the process of removing the protective layer may not be simple. In addition, a temporary fixing tape is used for the peeling as described above, and the process of removing the protective layer accordingly may become complicated. In addition, sometimes after peeling, a part of the photocurable adhesive layer (protective layer) remains on the circuit surface, and it may not be easy to remove the photocurable adhesive layer (protective layer). Even when the photocurable adhesive layer (protective layer) overlapping the non-circuit surface where the circuit surface is not formed is removed, the above-mentioned problems may also occur.

[0015] Therefore, there is a strong demand for a surface protective composition that can form a protective layer that can not only protect at least one surface of a substrate to be protected by covering the surface when the substrate is processed, etc., but also can be easily removed from the protected surface after the processing, etc. is completed.

[0016] In particular, there is a strong demand for a surface protective composition that can form a protective layer that can be removed relatively easily by at least partially dissolving when in contact with a solvent such as water.

[0017] However, it cannot be said that sufficient research has been conducted on surface protective compositions for forming a protective layer that can not only protect at least one surface of a substrate to be protected by covering the surface but can also be relatively easily removed by contact with a liquid containing water after protection.

[0018] Therefore, the problem of the present invention is to provide a surface protection composition for forming the following protective layer, which protects by covering at least one side of the substrate in the manufactured electronic component device, and then is easily removed when it comes into contact with a liquid containing water. In addition, the problem of the present invention is to provide a surface protection sheet having a protective layer formed by the surface protection composition. In addition, the problem of the present invention is to provide a method for manufacturing an electronic component device using the protective layer to manufacture the electronic component device.

[0019] Solutions for solving problems

[0020] To solve the above problems, the surface protective composition of the present invention protects at least one surface of a substrate, and comprises a polymer having a hydrophilic group in a molecule and a compound that generates an acid or a base by at least one of heating and irradiation with active energy rays.

[0021] The surface protection sheet of the present invention comprises a protective layer formed from the above-mentioned surface protection composition.

[0022] The manufacturing method of the electronic component device of the present invention comprises: a step of overlapping a protective layer formed of a surface protective composition on at least one of the two surfaces of a substrate to be protected, thereby protecting the protected surface; and a step of removing the protective layer overlapping the protected surface, wherein the surface protective composition comprises: a polymer having a hydrophilic group in a molecule, and a compound that generates an acid or a base by at least one of heating or irradiation with active energy rays, wherein in the removal step, the acid or the base is generated by the compound by heating or irradiation with active energy rays, thereby increasing the hydrophilicity of the protective layer, and the protective layer is removed by dissolving at least a portion of the protective layer in a liquid containing water. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is a schematic cross-sectional view of an example of the surface protection sheet according to the present embodiment cut along the thickness direction.

[0024] Figure 2A This is a schematic cross-sectional view showing an example of a situation of a wetting step in the method for manufacturing an electronic component device according to the present embodiment.

[0025] Figure 2B This is a schematic cross-sectional view showing an example of a protection step in the method for manufacturing an electronic component device according to the present embodiment.

[0026] Figure 2C This is a schematic cross-sectional view showing an example of a protection step in the method for manufacturing an electronic component device according to the present embodiment.

[0027] Figure 2D This is a schematic cross-sectional view showing an example of a state before a substrate is cut in the method for manufacturing an electronic component device according to the present embodiment.

[0028] Figure 2E This is a schematic cross-sectional view showing an example of a state after the substrate is cut in the method for manufacturing an electronic component device according to the present embodiment.

[0029] Figure 2F This is a schematic cross-sectional view showing an example of a state of a removal step in the method for manufacturing an electronic component device according to the present embodiment.

[0030] Figure 2G This is a schematic cross-sectional view showing an example of a state of a removal step in the method for manufacturing an electronic component device according to the present embodiment.

[0031] Figure 3A This is a cross-sectional view of an example of a dicing tape cut along the thickness direction.

[0032] Figure 3B This is a cross-sectional view obtained by cutting an example of a dicing die bonding film in the thickness direction.

[0033] Figure 4A This is a cross-sectional view schematically showing a state after the fixing (Mounting) step and the protecting step in the first embodiment are performed.

[0034] Figure 4B This is a cross-sectional view schematically showing a situation in the middle of a blade dicing process in the first embodiment.

[0035] Figure 4C It is a cross-sectional view schematically showing a state after the blade cutting process in the first embodiment is performed.

[0036] Figure 4D It is a cross-sectional view schematically showing the state of the removal step in the first embodiment.

[0037] Figure 4E It is a cross-sectional view schematically showing the state of the removal step in the first embodiment.

[0038] Figure 4F It is a cross-sectional view schematically showing the state of the pickup step in the first embodiment.

[0039] Figure 4G It is a cross-sectional view schematically showing the state of the joining step in the first embodiment.

[0040] Figure 4H This is a cross-sectional view schematically showing a state of half-cutting of a semiconductor wafer in another example of the first embodiment.

[0041] Fig. 4I This is a cross-sectional view schematically showing a state of half-cutting processing of a semiconductor wafer in another example of the first embodiment.

[0042] Figure 4J This is a cross-sectional view schematically showing a state of half-cutting processing of a semiconductor wafer in another example of the first embodiment.

[0043] Figure 4K It is a cross-sectional view schematically showing a state of the fixing step in another example of the first embodiment.

[0044] Figure 5A This is a cross-sectional view of an example of a semiconductor wafer cut along the thickness direction.

[0045] Figure 5B This is a cross-sectional view obtained by cutting an example of a semiconductor chip produced by dividing a semiconductor wafer in the thickness direction.

[0046] Fig. 6A It is a cross-sectional view schematically showing a state before the fixing step in the second embodiment.

[0047] Figure 6B It is a cross-sectional view schematically showing the state of the fixing step in the second embodiment.

[0048] Figure 6C It is a cross-sectional view schematically showing a state after the fixing step in the second embodiment.

[0049] Fig.6D It is a cross-sectional view schematically showing the state of the protection step in the second embodiment.

[0050] Fig. 6E It is a cross-sectional view schematically showing the state of the stealth processing step in the second embodiment.

[0051] Fig. 6F It is a cross-sectional view schematically showing the state of the expansion step in the second embodiment.

[0052] Figure 6G It is a cross-sectional view schematically showing the state of the removal step in the second embodiment.

[0053] Figure 6H It is a cross-sectional view schematically showing the state of the removal step in the second embodiment.

[0054] Fig.6I It is a cross-sectional view schematically showing the state of the pickup step in the second embodiment.

[0055] Figure 6J It is a cross-sectional view schematically showing the state of the joining step in the second embodiment.

[0056] Fig. 7A It is a cross-sectional view schematically showing a state of a semiconductor wafer and a backgrinding tape in the third embodiment.

[0057] Figure 7B It is a cross-sectional view schematically showing the state of the protection step in the third embodiment.

[0058] Figure 7C It is a cross-sectional view schematically showing a state before the fixing step in the third embodiment.

[0059] Fig.7D It is a cross-sectional view schematically showing the state of the fixing step in the third embodiment.

[0060] Fig. 8A It is a cross-sectional view schematically showing a state of a semiconductor wafer and a back grinding tape in a fourth embodiment.

[0061] Figure 8B It is a cross-sectional view schematically showing the state of the stealth processing step in the fourth embodiment.

[0062] Figure 8C It is a cross-sectional view schematically showing the state of the protection step in the fourth embodiment.

[0063] Fig.8DIt is a cross-sectional view schematically showing a state before the fixing step in the fourth embodiment.

[0064] Fig. 8E It is a cross-sectional view schematically showing the state of the fixing step in the fourth embodiment.

[0065] Fig.9A It is a cross-sectional view schematically showing a state of grinding processing after the protection step in the fifth embodiment.

[0066] Fig. 9B It is a cross-sectional view schematically showing the state after grinding in the fifth embodiment.

[0067] Fig. 9C It is a cross-sectional view schematically showing a state in a stealth processing step in the fifth embodiment.

[0068] Fig.9D It is a cross-sectional view schematically showing the state after the stealth processing step in the fifth embodiment. DETAILED DESCRIPTION

[0069] Hereinafter, each embodiment of the surface protective composition, the surface protective sheet, and the method for producing an electronic component device of the present invention will be described in sequence with reference to the drawings.

[0070] The surface protective composition of the present embodiment protects at least one surface of the substrate, and the surface protective composition comprises: a polymer having a hydrophilic group in the molecule, and a compound (hereinafter also referred to as an ion generating compound) that generates an acid or a base by at least one of heating or irradiation with active energy rays. The surface protective composition of the present embodiment is used, for example, to form a protective layer that protects at least one surface to be protected (hereinafter also referred to as a protected surface) of the substrate.

[0071] By overlapping the protective layer formed by the surface protective composition described above on at least one surface of the substrate, foreign matter can be prevented from adhering to the surface of the substrate to be protected (the protected surface) until the protective layer overlapping the surface is removed. For example, when the substrate and the protective layer are processed into small pieces while the protective layer formed by the surface protective composition and the substrate overlap each other, foreign matter such as fragments that may be generated by the small pieces can be prevented from adhering to the protected surface, thereby protecting the protected surface.

[0072] In addition, by subjecting the above-mentioned protective layer to a heat treatment or an irradiation treatment with active energy rays, an acid or a base is generated by the above-mentioned compound. As a result, the hydrophilicity of the protective layer formed by the surface protection composition is improved. At least a portion of the protective layer after the hydrophilicity is improved can be easily dissolved in the liquid by contacting with a liquid containing water. Therefore, all or a portion of the protective layer after the hydrophilicity is improved is dissolved in a liquid containing water, and the protective layer is easily detached from the protected surface. Therefore, for example, compared with the case where a peeling tape is attached to the protective layer and the protective layer is removed together with the peeling tape, the protective layer is more easily removed from the protected surface. In particular, in the case of removing the protective layer that is divided and cut into small pieces, multiple protective layers cut into small pieces can be easily removed from the protected surface compared with removing them using a peeling tape.

[0073] Thus, the protective layer formed of the surface protective composition can not only protect the protected surface of the substrate as a member of the manufactured electronic component device, but also can be relatively easily removed from the protected surface by a liquid containing water after protection.

[0074] In this embodiment, the hydrophilic group of the polymer is, for example, a hydroxyl group or a carboxyl group. The hydrophilic group may also be a polyoxyethylene chain. In this embodiment, the ion generating compound is, for example, an acid generator that generates an acid by at least one of heating or irradiation with active energy rays, or a base generator that generates a base by at least one of heating or irradiation with active energy rays. Examples of the ion generating compound include: a photoacid generator, a photobase generator, a thermal acid generator, or a thermal base generator.

[0075] The above-mentioned surface protective composition contains the above-mentioned ion-generating compound, and therefore has a physical property of improving hydrophilicity by at least one of heat treatment or irradiation treatment with active energy rays such as ultraviolet rays. The above-mentioned surface protective composition only needs to have a hydrophilicity above the prescribed level after the treatment as described above. Therefore, before the above-mentioned treatment, the above-mentioned surface protective composition may have a hydrophilicity less than the prescribed level, or may have a hydrophilicity above the prescribed level. When the above-mentioned surface protective composition has a hydrophilicity above the prescribed level, usually, at least a portion of the above-mentioned surface protective composition will dissolve in a liquid containing water. As the above-mentioned ion-generating compound, an ion-generating compound that generates an acid or a base by irradiation with active energy rays (especially ultraviolet rays) is preferred.

[0076] The surface protective composition after the hydrophilicity is improved by the above treatment preferably has a hydrophilicity above a predetermined value, that is, the water absorption rate of the above surface protective composition is preferably 1.5% by mass or more. Thus, the surface protective composition subjected to the heat treatment or the irradiation treatment with active energy rays is more easily dissolved in a liquid containing water. The above water absorption rate can be increased, for example, by increasing the content of the ion generating compound in the surface protective composition. The above water absorption rate can also be, for example, 10.0% by mass or less.

[0077] In the case where the hydrophilicity of the surface protective composition is increased by irradiation with active energy rays, the water absorption rate is the result of irradiation with a high-pressure mercury lamp at 500 mJ / cm 2 The value after the irradiation treatment.

[0078] It should be noted that the water absorption of the surface protective composition before the above-mentioned heat treatment or active energy ray irradiation treatment may be less than 1.5% by mass. Thus, even if the protective layer comes into contact with water before the removal step (described in detail later) of removing the protective layer formed from the surface protective composition, the protective layer can be prevented from being accidentally removed.

[0079] On the other hand, the water absorption of the surface protective composition before the above-mentioned heat treatment or active energy ray irradiation treatment may be 0.1 mass % or more. Thus, the surface protective composition subjected to the heat treatment or active energy ray irradiation treatment can have higher hydrophilicity.

[0080] The water absorption rate of the surface protective composition before the above-mentioned treatment can be improved by, for example, increasing the hydrophilic group of the above-mentioned polymer contained in the surface protective composition.

[0081] The water absorption of the above-mentioned surface protection composition is calculated based on the measured value using the Karl Fischer coulometric method. The surface protection composition before receiving the above-mentioned heat treatment or irradiation treatment with active energy rays and the surface protection composition after receiving the above-mentioned heat treatment or irradiation treatment with active energy rays are measured respectively. Specifically, a test sample that is in a steady state under an environment of temperature 23°C and humidity 50RH% is heated at 150°C for 3 minutes using a water vaporization device, and the vaporized water is measured. The above-mentioned water absorption is calculated based on the ratio of the measured water content to the mass of the above-mentioned heated test sample. It should be noted that when the above-mentioned surface protection composition contains a solvent, the water absorption of the surface protection composition is measured after the solvent is removed by volatilization treatment or the like.

[0082] For example, the surface protective composition of the present embodiment may contain a polymer having a main chain and a plurality of side chains in the molecule as the polymer, wherein each of the plurality of side chains has at least one of an ester group and a hydrophilic group, and the hydrophilic group is a hydroxyl group or a carboxyl group.

[0083] The polymer contains at least one of a hydroxyl group or a carboxyl group as a hydrophilic group in the molecule, and the protective layer formed by the surface protective composition can be more fully adhered to the protected surface due to the hydroxyl group or the carboxyl group. Therefore, until the protective layer is subjected to a treatment such as heating or irradiation with active energy rays, it can be fully adhered to the protected surface, and after the treatment, the protective layer can be removed from the protected surface relatively easily as described above.

[0084] The above-mentioned polymer has a main chain and a side chain in the molecule. The main chain is, for example, a covalent bond chain generated by a free radical polymerization reaction. For example, the main chain is a covalent bond chain generated by polymerization reaction of vinyl acetate (vinyl acetate), alkyl (meth) acrylate (alkyl (meth) acrylate), hydroxyalkyl (meth) acrylate (hydroxyalkyl (meth) acrylate), (meth) acrylic acid, etc.

[0085] Each of the plurality of side chains contains at least one of a hydrophilic group and an ester group. For example, among the many side chains contained in the above-mentioned polymer, a part of the side chains has a hydrophilic group, and another part has an ester group. The hydrophilic group is, for example, at least one of a hydroxyl group or a carboxyl group. The ester group is represented by -C(=O)-O-. In the ester group, the carbon atom can be arranged at a position closer to the main chain than the oxygen atom of the ether group, and the carbon atom can also be arranged at a position farther from the main chain than the oxygen atom of the ether group. In other words, from the main chain toward the end of the side chain, the side chain can have an atomic arrangement of an ester group such as -C(=O)-O-, or an atomic arrangement of an ester group such as -O-(C=O)-.

[0086] In each side chain containing a hydrophilic group, the hydrophilic group may be arranged at the end portion of the side chain or at the central portion of the side chain. The hydrophilic group in the side chain is preferably arranged at the end portion of the side chain. It should be noted that the hydrophilic group arranged at the end portion of the side chain may also be bonded to the main chain via an ester group. For example, each group may be arranged in the order of an ester group, an alkyl group, and a hydrophilic group from the main chain toward the end of the side chain.

[0087] In the side chain including an ester group, the ester group is preferably arranged in the center of the side chain. In the side chain, an alkyl group having 1 to 4 carbon atoms is preferably bonded to the main chain via the ester group.

[0088] Examples of the polymer include polyvinyl alcohol obtained by hydrolyzing a portion of ester bonds in a vinyl acetate polymer, copolymers of an alkyl (meth)acrylate and at least one of (meth)acrylic acid or a hydroxyalkyl (meth)acrylate, and polyethylene oxide (e.g., having a molecular weight of 50,000 or more).

[0089] In addition, in this specification, the expression "(meth)acrylate" includes both acrylate and methacrylate. Similarly, the expression "(meth)acrylic acid" includes both acrylic acid and methacrylic acid.

[0090] When the above-mentioned polymer is polyvinyl alcohol (PVA), the saponification degree (mol %) of the polyvinyl alcohol may be greater than 20 and less than 100 before the protective layer formed by the above-mentioned surface protective composition is subjected to a heat treatment or an active energy ray irradiation treatment (described in detail later).

[0091] The saponification degree of the polyvinyl alcohol is preferably 25 or more, more preferably 35 or more. By increasing the saponification degree of the polyvinyl alcohol, the protective layer formed from the surface protective composition has a higher hydrophilicity after being subjected to a heat treatment or an irradiation treatment with active energy rays. Therefore, the protective layer can be removed more easily with a liquid containing water.

[0092] On the other hand, the saponification degree of the polyvinyl alcohol is preferably 80 or less, and more preferably 60 or less. By making the saponification degree of the polyvinyl alcohol smaller, the adhesion to the substrate can be further improved.

[0093] <Saponification degree measurement method and measurement conditions>

[0094] The above saponification degree was determined by proton nuclear magnetic resonance spectroscopy under the following analytical conditions: 1 HMNR) was measured.

[0095] In addition, when the surface protective composition contains components other than PVA, in order to avoid overlapping peaks in the measurement chart, the measurement is performed after separation and extraction treatment of PVA by methanol extraction or the like.

[0096] Analytical apparatus: FT-NMR.

[0097] (For example, "AVANCEIII-400" manufactured by Bruker Biospin)

[0098] Observation frequency: 400MHz(1H).

[0099] Determination solvent: heavy water or deuterated dimethyl sulfoxide (dDMSO).

[0100] Measurement temperature: 80℃.

[0101] Chemical shift standard: external standard TSP-d4 (0.00ppm) (when measuring heavy water)

[0102] : Measurement solvent (2.50 ppm) (in the case of measurement with deuterated DMSO).

[0103] <Calculation of Saponification Degree>

[0104] The saponification degree was calculated according to the following calculation formula based on the peak derived from the methylene group of the vinyl alcohol unit (VOH) (heavy water; 2.0 ppm to 1.1 ppm, deuterated DMSO; 1.9 ppm to 1.0 ppm) and the peak derived from the acetyl group of the vinyl acetate unit (VAc) (heavy water; around 2.1 ppm, deuterated DMSO; around 2.0 ppm). It should be noted that in the following calculation formula, VOH (-CH2-) is the intensity of the peak derived from the methylene group of the vinyl alcohol unit (VOH), and VAc (CH3CO-) is the intensity of the peak derived from the acetyl group of the vinyl acetate unit (VAc).

[0105]

[0106] The average degree of polymerization of the polyvinyl alcohol is preferably 100 or more, and more preferably 200 or more. Furthermore, the average degree of polymerization is preferably 1000 or less, and more preferably 800 or less.

[0107] When the average degree of polymerization of polyvinyl alcohol is 200 or more, it is easier to form a protective layer from the surface protective composition. On the other hand, when the average degree of polymerization of polyvinyl alcohol is 1000 or less, the hydrophilicity of polyvinyl alcohol is further improved, and the protective layer formed from the surface protective composition is more easily dissolved in a liquid containing water.

[0108] The above-mentioned average degree of polymerization is determined by the following measurement method and measurement conditions.

[0109] <Method and conditions for measuring average degree of polymerization>

[0110] ·Analysis device: Gel permeation chromatography analysis device.

[0111] (For example, manufactured by Agilent, device name "1260 Infinity")

[0112] Column: TSKgel G6000PWXL and TSKgel G3000PWXL (manufactured by Tosoh Corporation, connected in series).

[0113] Column temperature: 40℃.

[0114] Eluent: 0.2 M sodium nitrate aqueous solution.

[0115] Flow rate: 0.8 mL / min.

[0116] Injection volume: 100 μL.

[0117] · Detector: Differential Refractometer (RI).

[0118] Standard samples: PEG standard samples and PVA standard samples.

[0119] By using the GPC measurement of the PEG standard sample, the mass average molecular weight Mw of the measured sample (PVA) and the PVA standard sample with a known average polymerization degree are calculated respectively. A calibration curve is prepared based on the average polymerization degree of the PVA standard sample and the calculated mass average molecular weight Mw of the PVA standard sample. Using this calibration curve, the average polymerization degree of the measured sample (PVA) is obtained based on the mass average molecular weight Mw of the measured sample (PVA).

[0120] The above-mentioned compound (ion-generating compound) contained in the surface protective composition of this embodiment is a compound that newly generates an acid or a base by at least one of a heat treatment and an irradiation treatment with active energy rays. From the perspective of simply improving the hydrophilicity of the surface protective composition by ionizing the hydrophilic group of the above-mentioned polymer with the generated acid, the above-mentioned ion-generating compound is preferably a compound that newly generates an acid.

[0121] The heating treatment and the active energy ray irradiation treatment will be described in detail later.

[0122] As the above-mentioned ion generating compound, there can be listed: photoion generators such as photoacid generators or photobase generators, or thermal ion generators such as thermal acid generators or thermal base generators, preferably the above-mentioned photoion generators. It should be noted that sometimes a compound has the functions of both a photoacid generator and a thermal acid generator. In other words, for example, sometimes a specific acid generator generates an acid by any treatment of heat treatment and irradiation treatment with active energy rays. The same is true for the base generator.

[0123] When the ion generating compound is a photoacid generator, a photobase generator, a thermal acid generator or a thermal base generator, the protective layer formed by the surface protective composition generates acid or base more fully by irradiation with active energy rays such as heat treatment or ultraviolet irradiation. Therefore, the hydrophilicity of the protective layer is further improved. Therefore, the protective layer can be more easily removed from the protected surface by a liquid containing water.

[0124] The photoacid generator as the acid generator is, for example, a photocationic polymerization initiator generally used for cationic polymerization, and the thermal acid generator as the acid generator is, for example, a thermal cationic polymerization initiator generally used for cationic polymerization.

[0125] The photobase generator as the base generator is, for example, a photoanionic polymerization initiator generally used for anionic polymerization, and the thermal base generator as the base generator is, for example, a thermal anionic polymerization initiator generally used for anionic polymerization.

[0126] As the above-mentioned photoacid generator, thermal acid generator, photobase generator or thermal base generator, commercially available products can be used respectively.

[0127] As the photoacid generator, there are ionic and nonionic types. The ionic photoacid generator has a cationic structure and an anionic structure. As the ionic photoacid generator, according to the type of cationic structure, for example, onium salt compounds, sulfonyl imide compounds, or disulfonyl diazomethane compounds can be listed.

[0128] Examples of the onium salt compound include onium salt compounds such as iodonium salt compounds, sulfonium salt compounds, oxime sulfonate compounds, and diazonium salt compounds. Among them, iodonium salt compounds and sulfonium salt compounds are preferred, and sulfonium salt compounds are more preferred.

[0129] Examples of the iodonium salt compound include diphenyliodonium hexafluorophosphate, diphenyliodonium hexafluoroarsenate, bis(4-tert-butylphenyl)iodonium hexafluorophosphate, diphenyliodonium trifluoromethanesulfonate, diphenyliodonium nonafluoro-n-butanesulfonate, diphenyliodonium perfluoro-n-octanesulfonate, benzyl-4-hydroxyphenylmethylsulfonium hexafluorophosphate, diphenyliodonium camphorsulfonate, bis(4-tert-butylphenyl)iodonium camphorsulfonate, bis(4-tert-butylphenyl)iodonium trifluoromethanesulfonate, bis(4-fluorophenyl)iodonium trifluoromethanesulfonate, and diphenyliodonium hexafluorophosphate. In addition, the iodonium salt compounds used in the following Examples can also be mentioned.

[0130] Examples of the sulfonium salt compound include diphenyl[4-(phenylthio)phenyl]sulfonium=trifluorotris(pentafluoroethyl)-λ 5 -phosphate, triphenylsulfonium hexafluoroantimonate, triphenylsulfonium nonafluoro-n-butanesulfonate, triphenylsulfonium camphorsulfonate, 4,7-di-n-butoxy-1-naphthyltetrahydrothiophenium trifluoromethanesulfonate, triphenylsulfonium trifluoromethanesulfonate, triphenylsulfonium adamantanecarboxylate trifluoroethanesulfonate, triphenylsulfonium p-toluenesulfonate, triphenylsulfonium methanesulfonate, triphenylsulfonium phenolsulfonate, triphenylsulfonium nitrate, triphenylsulfonium maleate, bis(triphenylsulfonium) maleate, triphenylsulfonium hydrochloride, triphenylsulfonium acetate, triphenylsulfonium trifluoroacetate, triphenylsulfonium salicylate, triphenylsulfonium benzoate, triphenylsulfonium hydroxide, etc. In addition, the sulfonium salt compounds used in the following Examples can also be mentioned.

[0131] Examples of the oxime sulfonate compound include (5-propylsulfonyloxyimino-5H-thiophen-2-ylidene)-(2-methylphenyl)acetonitrile, (5-octylsulfonyloxyimino-5H-thiophen-2-ylidene)-(2-methylphenyl)acetonitrile, (camphorsulfonyloxyimino-5H-thiophen-2-ylidene)-(2-methylphenyl)acetonitrile, (5-p-toluenesulfonyloxyimino-5H-thiophen-2-ylidene)-(2-methylphenyl)acetonitrile, and (5-octylsulfonyloxyimino)-(4-methoxyphenyl)acetonitrile.

[0132] Examples of the diazonium salt compound include 4-nitrobenzene diazonium tetrafluoroborate and the like.

[0133] Examples of commercially available products of onium salt compounds include OPTMER SP-150, OPTMER SP-170, OPTMER SP-171 (all manufactured by ADEKA), UVE-1014 (manufactured by General Electric), OMNICAT 250, OMNICAT 270 (all manufactured by IGM Resin), IRGACURE 290 (manufactured by BASF), SAN-AIDSI-60L, SAN-AID SI-80L, SAN-AID SI-100L (all manufactured by Sanshin Chemical Industry Co., Ltd.), CPI-100P, CPI-101A, CPI-200K (all manufactured by San-Apro), etc.

[0134] Examples of the sulfonyl imide compound as the photoacid generator include N-(trifluoromethanesulfonyloxy)succinimide, N-(nonafluoro-n-butanesulfonyloxy)succinimide, N-(camphorsulfonyloxy)succinimide, N-(trifluoromethanesulfonyloxy)naphthalimide, N-(camphorsulfonyloxy)succinimide, N-(4-methylphenylsulfonyloxy)succinimide, N-(2-trifluoromethylphenylsulfonyloxy)succinimide, N-(4 N-(trifluoromethylsulfonyloxy)phthalimide, N-(camphorsulfonyloxy)phthalimide, N-(2-trifluoromethylphenylsulfonyloxy)phthalimide, N-(2-fluorophenylsulfonyloxy)phthalimide, N-(trifluoromethylsulfonyloxy)diphenylmaleimide, N-(camphorsulfonyloxy)diphenylmaleimide, 4-methylphenylsulfonyloxy)diphenylmaleimide, etc.

[0135] Examples of the disulfonyldiazomethane compound as the photoacid generator include bis(trifluoromethylsulfonyl)diazomethane, bis(cyclohexylsulfonyl)diazomethane, bis(phenylsulfonyl)diazomethane, bis(p-toluenesulfonyl)diazomethane, bis(2,4-dimethylbenzenesulfonyl)diazomethane, and methylsulfonyl-p-toluenesulfonyldiazomethane.

[0136] Moreover, as a photoacid generator, 2,4-bis(trichloromethyl)-6-[2-(furan-2-yl)vinyl]-1,3,5-triazine etc. are mentioned, for example.

[0137] Examples of the thermal acid generator include aryldiazonium salts, diaryliodonium salts, triarylsulfonium salts, triarylsulfoxonium salts, pyridinium salts, quinolinium salts, isoquinolinium salts, sulfonic acid esters, and iron arene complexes.

[0138] The acid generator such as a photoacid generator or a thermal acid generator preferably has good compatibility with the above-mentioned polymer contained in the surface protection composition. As the acid generator, an ionic acid generator is preferred, and an ionic photoacid generator is more preferred. The acid generator is preferably a stronger acid.

[0139] As an index indicating the strength of the acid of the acid generator, gas phase acidity [ΔGacid] can be used. Gas phase acidity is an index indicating the acidity in the gas phase, excluding the solvent effect as much as possible. That is, gas phase acidity is an index indicating the acidity in the gas phase.

[0140] The reactivity of the acid generator is affected by the type of counter anion (conjugate acid) contained in the acid generator. The gas phase acidity of the anion contained in the acid generator is preferably 280 [kJ / mol] or less, and more preferably 260 [kJ / mol] or less. The smaller the value, the stronger the acid.

[0141] If we give an example of representative anions and their gas phase acidity, it is (CF3CF2)3PF3 - (Gas phase acidity: 256 [kJ / mol]), SbF6 - (Gas phase acidity: 256 [kJ / mol]), PF6 - (Gas phase acidity: 277 [kJ / mol]), BF4 - (Gas phase acidity: 288 [kJ / mol]) etc. As the acid generator, (CF3CF2)3PF3 is preferred. - or SbF6 - As anion acid generator.

[0142] Gas phase acidity is defined by IUPAC as the change in Gibbs energy accompanying acid dissociation. Gas phase acidity can be calculated by a known method described in, for example, "J. Am. Chem. Soc. 2000, 122, 5114-5124".

[0143] Examples of the photobase generator include radiation-sensitive base generators containing a heterocyclic group, such as 4-(methylthiobenzoyl)-1-methyl-1-morpholinoethane, (4-morpholinobenzoyl)-1-benzyl-1-dimethylaminopropane, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone, N-(2-nitrobenzyloxycarbonyl)pyrrolidine, and 1-(anthraquinone-2-yl)ethylimidazole carboxylate. Other examples include 2-nitrobenzylcyclohexylcarbamate, [[(2,6-dinitrobenzyl)oxy]carbonyl]cyclohexylamine, bis[[(2-nitrobenzyl)oxy]carbonyl]hexane-1,6-diamine, triphenylmethanol, o-carbamoylhydroxyamide, o-carbamoyloxime, hexaaminecobalt(III)tris(triphenylmethylborate), 1,2-dicyclohexyl-4,4,5,5-tetramethylbiguanide-n-butyltriphenylborate, acetophenone O-benzoyloxime, 2-(9-oxobenzofluoren-2-yl)propionic acid 1,5,7-triazabicyclo[4.4.0]dec-5-enyl, etc. Other examples include the photobase generator used in the following Examples.

[0144] Examples of the thermal base generator include carbamate derivatives such as 1-methyl-1-(4-biphenylyl)ethylcarbamate, 1,1-dimethyl-2-cyanoethylcarbamate, and benzoylcyclohexylcarbamate; urea derivatives such as urea and N,N-dimethyl-N'-methylurea; dihydropyridine derivatives such as 1,4-dihydronicotinamide; and quaternary ammonium salts of organosilanes or organoboranes.

[0145] In the surface protective composition, the amount of the ion generating compound is preferably 1 part by mass or more, more preferably 3 parts by mass or more, relative to 100 parts by mass of the polymer. Thus, the protective layer formed by the surface protective composition can have higher hydrophilicity after being subjected to a heat treatment or an active energy ray irradiation treatment.

[0146] The amount of the ion generating compound is preferably 10 parts by mass or less relative to 100 parts by mass of the polymer, thereby more sufficiently preventing the ion generating compound from remaining in the surface protecting composition.

[0147] The surface protective composition of the present embodiment may contain, in addition to the above-mentioned ingredients, a solvent, a surfactant, etc. Examples of the solvent include water and an organic solvent.

[0148] As the organic solvent, a relatively volatile organic solvent is preferred. Examples of such an organic solvent include ethanol and methanol.

[0149] The surface protective composition of the present embodiment may be a solid without fluidity or may have fluidity. When the surface protective composition contains a solvent, it may have fluidity.

[0150] The surface protective composition of the present embodiment can be produced by mixing the above-mentioned polymer, the above-mentioned plasma generating compound such as the photoacid generator, and the solvent etc. which are mixed as required by a common method. Alternatively, the surface protective composition of the present embodiment can be produced by volatilizing the solvent after the above-mentioned mixing.

[0151] The surface protective composition of the present embodiment is used, for example, to produce a surface protective sheet described below.

[0152] Next, the surface protection sheet 10 of the present embodiment will be described.

[0153] The surface protection sheet 10 of this embodiment is as follows Figure 1 The surface protection sheet 10 shown in the figure at least comprises a protective layer 11. The surface protection sheet 10 of the present embodiment may further comprise a release liner 15 overlapped on at least one surface of the protective layer 11. The release liner 15 may be overlapped on one surface or both surfaces of the protective layer 11.

[0154] It should be noted that each figure in the accompanying drawings is a schematic diagram, and the length ratio of the length to the width may not be the same as that of the actual object. The same applies to other drawings.

[0155] In this embodiment, the protective layer 11 of the surface protective sheet 10 is formed into a sheet from the surface protective composition. When the surface protective sheet 10 is used, for example, the release liner 15 is peeled off from the protective layer 11 and the protective layer 11 is attached to at least one surface (protected surface) of the substrate.

[0156] The protective layer 11 has flexibility that allows it to be deformed with a relatively weak force. In addition, the protective layer 11 has adhesiveness that allows it to adhere to the protected surface of the substrate, for example.

[0157] The protective layer 11 can be formed, for example, by applying the surface protective composition containing a solvent to one side of the substrate and then volatilizing the solvent. Alternatively, the protective layer 11 can also be formed by applying the surface protective composition containing a solvent to one side of the release liner 15 and then volatilizing the solvent. The protective layer 11 formed preferably does not contain a solvent for imparting fluidity to the surface protective composition.

[0158] It should be noted that the protective layer 11 may be formed, for example, from the surface protective composition not containing a solvent by a common molding method.

[0159] In the above-mentioned surface protection sheet, the thickness of the protective layer 11 is not particularly limited, for example, it is 1 μm or more and 100 μm or less. The thickness can be 3 μm or more, or 5 μm or more. In addition, the thickness can also be 40 μm or less. It should be noted that, when the protective layer 11 is a laminate, the above-mentioned thickness is the total thickness of the laminate.

[0160] The protective layer 11 may also have a property of being broken into small pieces by being stretched in the plane direction. The protective layer 11 having such a property is preferably used in the case where an electronic component device is manufactured through a stealth processing step using a stealth dicing device described later. Similarly, it is preferably used in the case where an electronic component device is manufactured through a DBG (Dicing Before Grinding) process (described in detail later).

[0161] It should be noted that the protective layer 11 described above may not have the above-mentioned physical properties because it can be preferably used in the case of manufacturing an electronic component device through a blade dicing process (described in detail later).

[0162] The adhesion of the protective layer 11 to the substrate is represented by, for example, the peeling force when the protective layer 11 is peeled off from a bare silicon wafer serving as the substrate. The peeling force of the protective layer 11 at 25°C may be 10.0 [N / 10mm] or less, or 8.0 [N / 10mm] or less. It should be noted that the peeling force may also be 0.01 [N / 10mm] or more. It should be noted that the value of the peeling force is a value before the protective layer 11 is subjected to at least one of a heat treatment and an irradiation treatment with active energy rays.

[0163] The above-mentioned peeling force is measured under the following measurement conditions.

[0164] In order to measure the peeling force of one surface of the above-mentioned protective layer 11 (the surface attached to the side of the silicon bare wafer), a sample for measurement is prepared as described below. First, a backing tape is attached to the surface of the protective layer 11 opposite to the above-mentioned one surface at 25°C using a hand roller. Next, the sample for measurement is processed in a manner to have a width of 100 mm, and a bare wafer is attached to the above-mentioned one surface of the protective layer 11. The attachment is carried out under the conditions of 90°C and 10 mm / sec. Then, under an environment of 23°C, the protective layer 11 is peeled off from the bare wafer together with the backing tape at a peeling angle of 180° and a peeling speed of 300 mm / min, and the peeling force is measured. Finally, the measured value is converted to be expressed in a unit value of [N / 10mm]. It should be noted that as a measuring device, for example, "Autograph (manufactured by SHIMADZU)" can be used.

[0165] The surface free energy of the protective layer 11 can be 70 [mJ / m 2 ] or less, or 65[mJ / m 2 It should be noted that the surface free energy can also be 20 [mJ / m 2 ]above.

[0166] When the surface free energy is within the above range, the wettability of the protective layer 11 to water becomes moderately good, so the protective layer 11 can be removed more easily in the removal step described later. It should be noted that the numerical value of the surface free energy is a value before the protective layer 11 is subjected to at least one of a heating treatment and an irradiation treatment with active energy rays.

[0167] The protective sheet 1 of this embodiment is used, for example, in the process of manufacturing an electronic component device. Specifically, the protective sheet 1 of this embodiment is used for the purpose of temporarily protecting the protected surface (protection target surface) of an electronic component (a type of substrate). More specifically, the protective sheet 1 of this embodiment is used, for example, by being attached to the protected surface of an electronic component (a type of substrate).

[0168] Examples of the electronic component include a semiconductor wafer, a semiconductor chip, a substrate such as a wiring circuit substrate, a connected wiring circuit substrate formed by connecting a plurality of wiring circuit substrates, and a dummy wafer.

[0169] The semiconductor chip mentioned above usually comprises: a semiconductor chip body; and an electrode portion, which is arranged on one side or both sides of the semiconductor chip body and is electrically connected to the electrode portion of other components. Other components include a wiring circuit substrate or other semiconductor chips. A circuit surface is formed on at least one side of the semiconductor chip, and a circuit is formed on the circuit surface.

[0170] Specifically, the semiconductor chip may be a semiconductor chip in the form of a TSV (Through Silicon Via) having: paired electrode portions disposed on both sides of the semiconductor chip body, and a conductive portion penetrating the semiconductor chip body in the thickness direction so that one side of the electrode portion is conductive to the other side. In a semiconductor chip in the form of a TSV, a circuit surface may be formed on only one side, or circuit surfaces may be formed on both sides.

[0171] In addition, a sensor element (for example, a light receiving element or a vibration element) may be provided as an element in the circuit of the semiconductor chip. Such a semiconductor chip is, for example, a sensor chip. Examples of sensor chips include CMOS (Complementary Metal-Oxide Semiconductor) chips and MEMS (Micro Electro Mechanical Systems) chips.

[0172] The above-mentioned dummy chip, for example, comprises: a supporting substrate, and a package in which a plurality of semiconductor chips arranged on the supporting substrate are resin-sealed together. The dummy chip may also be the above-mentioned package removed from the above-mentioned supporting substrate. A rewiring layer may also be formed on at least a portion of the surface of the dummy chip. The above-mentioned protective sheet 1 may also be used to cover the rewiring layer. It should be noted that the divided bodies formed by dividing the above-mentioned dummy chip into structural units each containing at least one semiconductor chip may also be electronic components.

[0173] As described above, there are various types of electronic components having a surface to be protected (surface to be protected), and various electronic components can serve as a substrate.

[0174] Next, a method for manufacturing the electronic component device according to the present embodiment will be described.

[0175] The manufacturing method of the electronic component device of the present embodiment includes: a process (protection process) of overlapping a protective layer 11 formed by a surface protection composition on at least one of the two surfaces of a substrate to be protected, thereby protecting the protected surface; and a process (removal process) of removing the protective layer 11 overlapping the protected surface, wherein the surface protection composition includes: a polymer having a hydrophilic group in the molecule, and a compound (the above-mentioned ion-generating compound) that generates an acid or a base by at least one of heating or irradiation with active energy rays, in the removal process, the acid or the base is generated by the compound (ion-generating compound) by heating or irradiation with active energy rays, thereby improving the hydrophilicity of the protective layer 11, and the protective layer 11 is removed by dissolving at least a portion of the protective layer 11 in a liquid containing water.

[0176] The method for manufacturing an electronic component device of the present embodiment may further include a step of increasing the humidity of the gas in contact with the protected surface Sa (wetting step) before the above-mentioned protecting step (see Figure 2A ) By performing the wetting step, the adhesion of the protective layer 11 to the protected surface Sa can be improved.

[0177] The wetting step can be performed, for example, by: bringing a gas containing water vapor into contact with the protected surface; spraying mist of water on the protected surface; or applying water to the protected surface.

[0178] In the above protection process, it is also possible to Figure 2B As shown, the surface protection sheet 10 having a release liner 15 on one side of the protective layer 11 is used to protect the protected surface Sa of the substrate S. For example, after the protective layer 11 of the surface protection sheet 10 is superimposed on the protected surface Sa of the substrate S, the release liner 15 may be peeled off from the protective layer 11 (see Figure 2C ).

[0179] The method for manufacturing the electronic component device of this embodiment can also be as follows Figure 2D and Figure 2E As shown, the method further includes: dividing the stack of the overlapping substrate S and the protective layer 11 into small pieces in a manner that they are spaced apart in the surface direction, thereby producing a plurality of small pieces of the stack of the chip S' formed by the substrate being divided into small pieces and the small pieces 11' of the protective layer overlapping each other. It should be noted that a fragile portion for the small pieces may also be formed inside the substrate S before being divided.

[0180] In the above-mentioned removal process, Figure 2FAs shown, by subjecting the plurality of small pieces 11' of the protective layer to, for example, heat treatment or irradiation with active energy rays such as ultraviolet rays, the ion generating compound contained in each small piece 11' newly generates acid or base, thereby improving the hydrophilicity of each small piece 11'.

[0181] Then, in the above-mentioned removal process, if Figure 2G As shown, each small piece 11 ′ of the protective layer overlapping the circuit surface of the chip S′ is removed by a liquid containing water.

[0182] It should be noted that the method for manufacturing an electronic component device of the present embodiment may further include the step of arranging the circuit surface of the chip S' toward the adherend and bonding the chip S' to the adherend.

[0183] The electronic component device manufactured by the manufacturing method of this embodiment has at least one of the various electronic components described above. As the electronic component device, for example, there can be listed: a semiconductor device such as a semiconductor integrated circuit having a semiconductor chip; a device having a system LSI (Large Scale Integration: large-scale integrated circuit) having a complementary MOS (CMOS); or a device having a device (MEMS, Micro ElectroMechanical Systems) in which mechanical elements, sensors, drivers or electronic circuits are integrated on a silicon substrate, a glass substrate or an organic material substrate through micro-machining technology, etc. It should be noted that the manufactured electronic component device can also be a device having a wiring circuit substrate.

[0184] In the manufacturing method of the electronic component device of the present embodiment, at least one surface of the substrate is protected by a protective layer. The protected surface (hereinafter, also referred to as the protected surface) may be only one side of the substrate or both sides. It should be noted that the circuit structure element may or may not be configured on the protected surface (described in detail later).

[0185] The material of the substrate is not particularly limited as long as it is in the form of a plate. Examples of the material of the substrate include glass, silicon, stainless steel (SUS), plastic, or ceramic. Examples of the substrate include semiconductor wafers, sensor wafers such as CMOS or MEMS, dummy wafers, or wiring circuit substrates.

[0186] In the above-mentioned protection step, the protection layer 11 may be overlapped on the surface of the side of the substrate where at least one of the circuit wiring, the sensor part, and the electrode part is configured as a circuit structure element. For example, the protection layer 11 may be overlapped on a single side (circuit surface) of the side of the substrate where the circuit wiring is configured, or the protection layer 11 may be overlapped on a single side of the substrate where the sensor part is configured, or the protection layer 11 may be overlapped on a single side of the substrate where the electrode part is configured. In the above-mentioned protection step, it is preferred to overlap the protection layer 11 on at least one side of the substrate in such a manner that the circuit wiring, the sensor part, or the electrode part is covered by the protection layer 11. Examples of the circuit structure element include: circuit wiring, electrode part or transistor, diode or sensor part (light receiving sensor or vibration sensor, etc.) and other elements.

[0187] Hereinafter, a case where a semiconductor integrated circuit (semiconductor device) is manufactured as an electronic component device will be described in detail.

[0188] Generally, the manufacturing method of a semiconductor device includes a front process of forming a circuit surface on one side of a wafer with a highly integrated electronic circuit, and a back process of cutting out chips from the wafer with the circuit surface formed thereon and assembling them.

[0189] In the post-process, for example, a weak portion is formed on the wafer for cutting a wafer (semiconductor wafer) as a substrate having a circuit surface into small semiconductor chips (die), and the adhesive layer of the dicing tape is attached to the surface opposite to the circuit surface. Then, the dicing tape is stretched in the surface direction while the semiconductor wafer is attached to the adhesive layer of the dicing tape, thereby cutting the semiconductor wafer into semiconductor chips with the above-mentioned weak portion as the boundary. After that, the semiconductor chips that have become small pieces are peeled off from the adhesive layer of the dicing tape.

[0190] The post-processes as described above include, for example, a stealth processing process, in which a fragile part for cutting the wafer into small chips (die) is formed on the wafer by using laser or the like; a fixing process, in which the surface of the semiconductor wafer opposite to the circuit surface is attached to the dicing tape to fix the semiconductor wafer; an expansion process, in which the dicing tape is stretched in the surface direction to cut the semiconductor wafer into small chips (die); a picking process, in which the semiconductor chip is peeled off from the adhesive layer and taken out; and a bonding process, in which the taken out semiconductor chip is bonded to the adherend. For example, a semiconductor integrated circuit (semiconductor device) is manufactured through these processes.

[0191] In the method for manufacturing a semiconductor device (electronic component device) of the present embodiment, for example, a semiconductor chip is cut out from a semiconductor wafer having a circuit surface formed thereon, and a semiconductor device having the cut semiconductor chip is assembled. In the method for manufacturing a semiconductor device of the present embodiment, at least the protective layer 11 of the surface protection sheet 10 and the dicing tape 20 (see Figure 3A ), a semiconductor device is manufactured as described below. The sheet and tape are used as auxiliary tools for manufacturing semiconductor devices. It should be noted that a dicing die bonding film (see Figure 3B ) As the dicing tape 20 and the dicing die-bonding film, commercially available products can be used respectively.

[0192] Hereinafter, specific embodiments of the method for manufacturing a semiconductor device will be described in detail from the first embodiment to the fifth embodiment.

[0193] In addition, the manufacturing method of the first embodiment is described as “I” in the drawings. Similarly, the second to fifth embodiments are described as “II” to “V” in the drawings, respectively.

[0194] "First Implementation Method"

[0195] The method for manufacturing a semiconductor device according to the first embodiment includes an assembling step of cutting out a semiconductor chip X from a semiconductor wafer W (substrate) having a circuit surface formed thereon, and assembling a semiconductor device having the semiconductor chip X.

[0196] The assembly process includes: a process of protecting the circuit surface (protected surface) by stacking a protective layer 11 for protecting the circuit structure element on the circuit surface of at least one surface of the semiconductor chip W on which any circuit structure element is formed (protection process); a process of dividing the stack of the overlapping semiconductor chip W and the protective layer 11 into small pieces in a manner spaced apart in the surface direction, thereby producing a plurality of small pieces of a stack of semiconductor chips X formed by the semiconductor chip W being sliced ​​and small pieces 11' of the protective layer overlapping each other; a process of subjecting each small piece 11' of the protective layer overlapping the circuit surface of the semiconductor chip X to a heat treatment or an irradiation treatment with active energy rays, etc., so that the above-mentioned ion-generating compound in each small piece 11' generates an acid or a base, thereby improving the hydrophilicity of each small piece 11', and then removing each small piece 11' of the protective layer by a liquid containing water (removal process); and a process of bonding the semiconductor chip X to an adherend.

[0197] The assembling process of the first embodiment includes, for example, the following steps.

[0198] Specifically, the assembly process of the first embodiment includes: a fixing process, in which a semiconductor wafer W having a circuit structure element formed on one side is attached to a dicing die bonding film (a die bonding sheet 30 overlapping a dicing tape 20), and the semiconductor wafer W is fixed to the dicing die bonding film; a protection process, in which a protection layer 11 is attached to the circuit surface of the semiconductor wafer W, thereby protecting the circuit surface; a blade cutting process, in which the die bonding sheet 30 and the semiconductor wafer W attached with the protection layer 11 are cut into small pieces using a dicing blade T, etc., to produce a semiconductor chip (die) formed by cutting the semiconductor wafer W into small pieces. ) (a process of making a plurality of small pieces of the above-mentioned laminate); a removal process of removing the plurality of small pieces 11' attached to the protective layer of the semiconductor chip X after the above-mentioned heating treatment or active energy ray irradiation treatment, etc. (the above-mentioned removal process); a picking process of peeling the semiconductor chip X and the small piece 30' of the chip bonding sheet, and taking out the semiconductor chip X in a state of being attached with the small piece 30' of the chip bonding sheet; and a bonding process of bonding the taken-out semiconductor chip X to the adherend through the small piece 30' of the chip bonding sheet (the above-mentioned bonding process). When implementing these processes, the above-mentioned protective layer 11 and the dicing die bonding film with the dicing tape 20 are used as manufacturing auxiliary tools.

[0199] The semiconductor wafer W is configured to obtain a plurality of semiconductor chips X. Specifically, the semiconductor wafer W is configured to be divided into small pieces in a manner of being spaced apart in a plurality of directions along the surface (for example, directions along the surface and orthogonal to each other), thereby being able to produce a plurality of semiconductor chips X. In addition, the semiconductor wafer W has a circuit surface on which at least one of the circuit structure elements is arranged on at least one surface. For example, the semiconductor wafer W used in the first embodiment has a circuit surface formed on any one surface.

[0200] In the semiconductor industry in recent years, with the further progress of integration technology, thinner semiconductor chips (e.g., thickness of 20 μm or more and 50 μm or less) are eagerly desired. When the semiconductor chip is viewed from one side in the thickness direction, the shape is, for example, a rectangle, and the length of one side is, for example, a predetermined length of 5 mm or more and 20 mm or less.

[0201] In the fixing process, Figure 4A As shown, a dicing ring R is attached to the adhesive layer 22 of the dicing tape 20 , and a semiconductor wafer W is attached and fixed to the die bonding sheet 30 superimposed on the dicing tape 20 .

[0202] In the protection process, for example Figure 4AAs shown, the protective layer 11 is laminated on the above-mentioned one circuit surface of the semiconductor wafer W. In the protection step, for example, the protective layer 11 may be directly pressed and adhered to the above-mentioned circuit surface, thereby laminating the protective layer 11 on the above-mentioned circuit surface. On the other hand, a surface protective composition including a solid component constituting the protective layer 11 and a solvent for dissolving the solid component may be prepared, and the prepared surface protective composition may be applied to the above-mentioned circuit surface and then the solvent is volatilized, thereby forming the protective layer 11 in contact with the above-mentioned circuit surface, thereby laminating the protective layer 11 on the above-mentioned circuit surface.

[0203] By stacking the protective layer 11 on the circuit surface of the semiconductor wafer W, the circuit surface can be protected by the protective layer 11 until the protective layer 11 is removed. Therefore, it is possible to prevent dirt and the like from being attached to the circuit surface of the semiconductor wafer W covered by the protective layer 11.

[0204] It should be noted that the protecting step may be performed after the fixing step, or the fixing step may be performed after the protecting step.

[0205] In the blade cutting process, for example Figure 4B and Figure 4C As shown, the semiconductor wafer W is cut. Specifically, the semiconductor wafer W is cut into a predetermined size together with the chip bonding sheet 30 to form a semiconductor chip with the chip bonding sheet 30. The blade cutting process is performed in accordance with a conventional method using, for example, a cutting blade T. In the blade cutting process, for example, a cutting method called a full cut can be adopted in which the chip bonding sheet 30 is cut into. There is no particular limitation on the cutting device used in the blade cutting process, and a conventionally known device can be used.

[0206] In the blade dicing process, foreign matter such as chips may be generated as the semiconductor wafer W is cut. At this time, the protected surface of the semiconductor wafer W is protected by the protective layer 11, so that foreign matter can be prevented from being attached to the protected surface.

[0207] It should be noted that, before the blade cutting process, the dicing ring R may be attached to the adhesive layer 22 of the dicing tape 20 and then fixed to the holder H of the expansion device.

[0208] In the removal process, Figure 4D As shown, the plurality of small pieces 11' of the protective layer are subjected to a treatment in which the ion generating compound generates an acid or a base. As the treatment, at least one of a heat treatment and an active energy ray irradiation treatment is adopted.

[0209] The heat treatment is performed, for example, by exposing the plurality of small pieces 11 ′ of the protective layer to an environment of 90° C. or higher and 250° C. or lower for 10 minutes or higher and 300 minutes or lower.

[0210] In the irradiation treatment with active energy rays, for example, 10 mW / cm 2 Above and 300mW / cm 2 The following intensity of ultraviolet rays is used as active energy rays, and the accumulated light amount is 50mJ / cm 2 Above and 1000mJ / cm 2 The plurality of small pieces 11 ′ of the protective layer are irradiated with ultraviolet rays in the following manner.

[0211] In the removal process, by subjecting the plurality of small pieces 11' of the protective layer to the above-mentioned treatment, the ion-generating compound contained in the small pieces 11' generates an acid or a base. The newly generated acid or base increases the hydrophilicity of the plurality of small pieces 11' of the protective layer accordingly. As a result, when the small pieces 11' are subsequently in contact with a liquid containing water, the small pieces 11' can be removed from the surface of the semiconductor chip X more easily.

[0212] In the removal process, Figure 4E As shown, by bringing a liquid containing water into contact with the plurality of small pieces 11' of the protective layer, at least a portion of each small piece 11' is dissolved in the liquid, and each small piece 11' of the protective layer is removed from the surface (protected surface) of the semiconductor chip X.

[0213] By removing the small pieces 11' of the protective layer in this way, all of the plurality of small pieces 11' of the protective layer can be removed relatively easily, and the amount of foreign matter attached to the surface of the semiconductor chip can be reduced relatively easily by the above-mentioned liquid. In addition, the surface (protected surface) of each semiconductor chip X overlapped by the small pieces 11' of the protective layer can also be cleaned by the liquid.

[0214] In the removal step, the protective layer (plural small pieces 11' of the protective layer) that have been cut into small pieces may be completely dissolved in the above-mentioned liquid to remove the small pieces 11' of the protective layer. On the other hand, the small pieces 11' of the protective layer that have weakened their adhesion to the semiconductor chip X may be peeled off from the semiconductor chip X to remove the small pieces 11' of the protective layer.

[0215] The liquid containing water is not particularly limited as long as it is a liquid substance containing water. The liquid may contain more than 30% by mass of water, more than 50% by mass of water, more than 70% by mass of water, more than 80% by mass of water, or more than 90% by mass of water.

[0216] The liquid may contain a component soluble in water in addition to water. Such a component may include, for example, a water-soluble organic solvent. Such a water-soluble organic solvent may include, for example, a monohydric alcohol having a carbon number of 4 or less, such as propanol such as methanol, ethanol, and isopropanol, or butanol such as tert-butyl alcohol.

[0217] In the removal step of the first embodiment, the small piece 11' of the protective layer may be immersed in the stirred liquid to make the liquid contact with the small piece 11' of the protective layer. Alternatively, the liquid ejected from a nozzle or the like may be made contact with the small piece 11' of the protective layer. The temperature of the liquid is not particularly limited, and may be set to, for example, 10° C. or higher and 90° C. or lower.

[0218] For example, in the removal process, a disk-shaped workbench supporting the dicing tape 20 from below is rotated in the circumferential direction, and the liquid is sprayed onto the semiconductor chips X of the small pieces 30' respectively attached to the chip bonding sheet. Thus, a plurality of small pieces 11' respectively overlapping the protective layer of the semiconductor chip X can be removed. The rotation speed of the workbench can be, for example, 500 rpm or more and 4000 rpm or less, the spraying amount of the liquid can be, for example, 0.05 L / min or more and 5.0 L / min or less, and the spraying time can be, for example, 5 seconds or more and 300 seconds or less.

[0219] According to the method for manufacturing a semiconductor device of the first embodiment, the protective layer 11 is overlapped on the surface (circuit surface) of the semiconductor wafer W on which the circuit structural elements are formed, so that the above-mentioned circuit surface can be protected until the protective layer 11 is removed. Specifically, the semiconductor wafer W is cut into small pieces to produce the semiconductor chip X in a state where the semiconductor wafer W and the protective layer 11 overlap each other, so that foreign matter such as fragments that may be generated due to the cutting of the semiconductor wafer W can be prevented from being attached to the circuit surface of the semiconductor chip X. Even if foreign matter is attached to the circuit surface of the semiconductor chip X before the protective layer 11 is overlapped, the foreign matter can be removed when the small piece 11' of the protective layer overlapping the circuit surface of the semiconductor chip X is removed. Therefore, it is possible to suppress the attachment of foreign matter to the circuit surface of the manufactured semiconductor chip X.

[0220] In the picking process, Figure 4F As shown, the semiconductor chip X is peeled off from the adhesive layer 22 of the dicing tape 20. Specifically, the pin member P is raised to push up the semiconductor chip X to be picked up through the dicing tape 20. The pushed-up semiconductor chip X is held by the suction jig J.

[0221] When the pickup process is performed in this way, the small pieces 30' of the die bond sheet attached to the semiconductor chip X need to be easily peeled off from the adhesive layer 22 of the dicing tape 20. In addition, when the above-mentioned expansion process is performed, the die bond sheet 30, the semiconductor wafer W, and the protective layer 11 need to be well divided into small pieces by stretching the dicing tape 20. The above-mentioned dicing tape 20 is designed to well demonstrate such performance.

[0222] For example, the dicing tape 20 is configured so that the adhesive layer 22 is cured by irradiating active energy rays (e.g., ultraviolet rays), thereby reducing the adhesive force of the adhesive layer 22. By curing the adhesive layer 22 after irradiation, the adhesive force of the adhesive layer 22 can be reduced, so that the semiconductor chip X and the small piece 30' of the die bonding sheet can be easily peeled off from the adhesive layer 22 after irradiation. Dicing tapes 20 having such a configuration are commercially available.

[0223] In the bonding process, the semiconductor chip X with the die bonding sheet small piece 30' attached thereto is bonded to the adherend Z. In other words, the semiconductor chip X is bonded to the adherend Z via the die bonding sheet small piece 30'. Figure 4G As shown, the semiconductor chip X with the die bonding sheet 30' attached thereto is stacked multiple times. In the first embodiment, the semiconductor chip X is bonded to an adherend such as a substrate or the semiconductor chip X via the die bonding sheet 30'.

[0224] When a plurality of semiconductor chips X are stacked in the bonding process as described above, since a plurality of semiconductor chips X are stacked to suppress adhesion of foreign matter to the circuit surface, the amount of foreign matter entering between one semiconductor chip X and another semiconductor chip X in the stack can be suppressed.

[0225] In addition, as a to-be-adhered body Z, an interposer, a wiring circuit board, or a small piece of a board|substrate (in the case of stacking small pieces of a board|substrate) etc. are mentioned, for example.

[0226] In the first embodiment, in order to protect the semiconductor chip X after the bonding step, a resin sealing step of sealing (covering) the semiconductor chip X with a thermosetting resin or the like may be performed.

[0227] In the above description of the first embodiment, an example of cutting the semiconductor wafer W into small pieces by a blade cutting process is cited, but the semiconductor wafer W can also be cut into small pieces through a so-called DBG process, which reduces the thickness of the semiconductor wafer W after half-cutting the semiconductor wafer W.

[0228] In the half-cutting process, for example, a groove is formed in a semiconductor wafer W that is to be processed into a chip (die) by a cutting process, and the semiconductor wafer W is further ground to reduce the thickness. Figure 4H to Figure 4KAs shown in FIG. 1 , a wafer processing tape E is attached to the surface of the semiconductor wafer W opposite to the circuit surface. A groove for dividing is formed with the wafer processing tape E attached. A back grinding tape B is attached to the surface with the groove formed, and the wafer processing tape E attached initially is peeled off. With the back grinding tape B attached, grinding is performed until the semiconductor wafer W reaches a predetermined thickness. Then, a fixing step is performed, and thereafter, a semiconductor device is manufactured in the same manner as described above.

[0229] Next, the second embodiment will be described in detail. It should be noted that the same description as the first embodiment will not be repeated for the second embodiment. In the second embodiment, unless otherwise specified, the same operation as the first embodiment can be performed.

[0230] "Second Implementation Method"

[0231] The method for manufacturing a semiconductor device according to the second embodiment includes, for example, a fixing step of attaching a semiconductor wafer W having circuit components formed on both sides thereof to a dicing tape 20 to fix the semiconductor wafer W to the dicing tape 20; a protecting step of attaching a protective layer 11 to the circuit surface of the exposed side of the semiconductor wafer W to protect the circuit surface; a stealth processing step of forming a fragile portion inside the semiconductor wafer W to which the protective layer 11 is attached by laser to prepare for cutting the semiconductor wafer W into small pieces into semiconductor chips (dies); an expanding step of stretching the dicing tape 20 to cut the semiconductor wafer W and the protective layer 11 into small pieces; a removing step of removing a plurality of small pieces 11' of the protective layer attached to the semiconductor chip X after the above-mentioned heating treatment or active energy ray irradiation treatment, etc.; a picking-up step of peeling the semiconductor chip X and the adhesive layer 22 to take out the semiconductor chip X; and a bonding step of bonding the taken-out semiconductor chip X to an adherend.

[0232] When performing these steps, the protective layer 11 and the dicing tape 20 described above are used as manufacturing aids.

[0233] As the dicing tape 20 described above, the dicing tape used in the first embodiment can be used.

[0234] The semiconductor wafer W (substrate) before being diced into semiconductor chips X can also be ground to a desired thickness by, for example, back grinding. Specifically, in the back grinding, the semiconductor wafer W with the back grinding tape B attached to the circuit surface can also be ground to reduce the thickness of the semiconductor wafer W to the thickness of the semiconductor chip X to be manufactured later.

[0235] The semiconductor wafer W used in the second embodiment has circuit surfaces formed on both sides. On the other hand, the semiconductor wafer W used in other embodiments has a circuit surface formed on either side. Figure 5A and Figure 5B As shown, the electrode portion D is arranged on one side where the circuit is formed, and the electrode portion D is also arranged on the other side where the circuit is formed. The electrode portion D on one side and the electrode portion D on the other side are electrically connected to each other.

[0236] Specifically, the semiconductor chip X produced by dividing the semiconductor wafer W has electrodes D disposed on both sides and connected to each other. Figure 5B As shown, electrodes D are arranged on both sides of the semiconductor chip X, and conductive through holes V are arranged to penetrate in the thickness direction of the semiconductor chip X. Through the through holes V, the electrodes D on both sides are electrically connected to each other.

[0237] In a second embodiment, if Fig. 6A As shown, a glass carrier G is attached to one circuit surface of the semiconductor wafer W. The glass carrier G overlaps the circuit surface of one circuit surface of the semiconductor wafer W to support the thin semiconductor wafer, making it easy to handle the semiconductor wafer. For example, the glass carrier G is used to further arrange circuit components on the other surface of the semiconductor wafer W in a state where the glass carrier G is attached to the circuit surface after forming the circuit surface on one side. The thickness of the glass carrier G is, for example, not less than 0.5 mm and not more than 5.0 mm.

[0238] In the fixing step, the dicing ring R is mounted on the adhesive layer 22 of the dicing tape 20, and a semiconductor wafer W is attached to the exposed surface of the adhesive layer 22 (see Figure 6B ). Next, the glass carrier G is peeled off from the semiconductor wafer W (refer to Figure 6C ).

[0239] In the subsequent protection process, a protection layer 11 is laminated on the circuit surface of the semiconductor wafer W (see Fig.6D ). In the protection step, for example, the protective layer 11 may be directly pressed and pasted on the circuit surface, thereby laminating the protective layer 11 on the circuit surface. On the other hand, a surface protective composition comprising a solid component constituting the protective layer 11 and a solvent for dissolving the solid component may be prepared, and the prepared surface protective composition may be applied to the circuit surface and then the solvent may be volatilized to form the protective layer 11 in contact with the circuit surface, thereby laminating the protective layer 11 on the circuit surface.

[0240] By stacking the protective layer 11 on the circuit surface of the semiconductor wafer W, the circuit surface can be protected by the protective layer 11 until the protective layer 11 is removed. Therefore, it is possible to prevent dirt and the like from being attached to the circuit surface of the semiconductor wafer W covered by the protective layer 11.

[0241] In the stealth process, a weak portion for cutting the semiconductor wafer W into semiconductor chips X is formed inside the semiconductor wafer W. By irradiating the semiconductor wafer W with laser light L, a weak portion is formed inside the semiconductor wafer W (see Fig. 6E ). The laser L is irradiated to the semiconductor wafer W from the dicing tape side, for example. It should be noted that the semiconductor wafer W is irradiated with the laser L in such a manner that each semiconductor chip X produced by dividing the semiconductor wafer W through the subsequent expansion process has the above-mentioned electrode portion D as designed in advance. The stealth processing step can be implemented using a commercially available stealth dicing device, for example.

[0242] In the expansion process, Fig. 6F As shown, in a state where the dicing tape 20 and the protective layer 11 are respectively arranged on both sides of the semiconductor wafer W, the dicing tape 20 is stretched in the surface direction to increase the surface area of ​​the dicing tape 20. As a result, the stack of the semiconductor wafer W and the protective layer 11 is divided into small pieces, and the interval between the adjacent semiconductor chips X formed by the small pieces is expanded in the surface direction. In detail, the upper supporting member U possessed by the expansion device is pushed up from the lower side of the dicing tape 20, thereby stretching the dicing tape 20 in a manner that expands in the surface direction. As a result, under specific temperature conditions, the semiconductor wafer W and the protective layer 11 are broken into small pieces. The above-mentioned temperature conditions are, for example, above -20°C and below 0°C. The expansion state is released by lowering the upper supporting member U (it is a low-temperature expansion process so far).

[0243] When the expansion process is performed at a low temperature, the protective layer 11 needs to be cut into small pieces. The protective layer 11 is designed to be well cut at this time.

[0244] Furthermore, in the expansion process, the dicing tape 20 is stretched under a higher temperature condition (e.g., 10° C. or higher and 25° C. or lower) to increase the surface area of ​​the dicing tape 20. Thus, the semiconductor chips X adjacent to each other are pulled apart in the surface direction of the dicing tape 20, and the cut (interval) is further increased (normal temperature expansion process).

[0245] In the expansion process, the dicing tape 20 is stretched in the surface direction to expand the area of ​​the dicing tape 20, thereby dividing the protective layer 11 into small pieces together with the semiconductor wafer W. Specifically, by stretching the dicing tape 20, the semiconductor wafer W can be divided into small pieces with the above-mentioned fragile portion inside the semiconductor wafer as a boundary. At this time, as the semiconductor wafer W is divided into small pieces into semiconductor chips X, the protective layer 11 is also divided into small pieces.

[0246] The removal process of the second embodiment is as follows Figure 6G and Figure 6H As shown, the removal process can be carried out in the same manner as in the first embodiment.

[0247] In the picking process of the second embodiment, as Fig.6I As shown, the semiconductor chip X is peeled off from the adhesive layer 22 of the dicing tape 20. When the pickup process is performed in this way, the semiconductor chip X is peeled off from the adhesive layer 22 of the dicing tape 20.

[0248] As described above, the two sides of the semiconductor chip X taken out by the pickup process are provided with mutually conductive electrode portions D. The surface layer portions of one side and the other side of the semiconductor chip X are provided with electrode portions D and non-electrode portions other than the electrode portions D. The non-electrode portions are made of, for example, insulating materials (silicon oxide). Figure 5B As shown, on one surface and the other surface of the semiconductor chip X, the surface of the electrode portion D and the surface of the non-electrode portion are flush. The electrode portion D is formed, for example, to have a thickness of more than 5 nm and less than 10 μm from the surface of the semiconductor chip X. It should be noted that the above-mentioned through hole V configured to penetrate the semiconductor chip X in the thickness direction is covered by the above-mentioned insulating material except for the portion connected to the electrode portion D. In other words, a portion of the surface of the through hole V extending in the thickness direction of the semiconductor chip X is covered by the insulating material, and the other portion is connected to the electrode portion D.

[0249] The bonding process is performed after the removal process and the picking process. Figure 6J As shown, the semiconductor chip X may be bonded to the adherend with the surface (circuit surface) of the small piece 11 ′ from which the protective layer of the semiconductor chip X is removed facing the adherend.

[0250] In the bonding step, for example, an adherend Z (wiring board or the like) is bonded to a semiconductor chip X. At this time, the adherend Z and the semiconductor chip X are bonded so that the electrode portion D of the adherend Z and the electrode portion D of the semiconductor chip X are electrically connected.

[0251] Furthermore, for example, in the bonding step, at least two semiconductor chips X are stacked, and the electrode portion D of one semiconductor chip X and the electrode portion D of another semiconductor chip X as adherends are directly connected to each other.

[0252] When a plurality of semiconductor chips X are stacked as described above in the bonding process, since a plurality of semiconductor chips X are stacked to suppress the attachment of foreign matter to the circuit surface, the number of foreign matter that enters between one stacked semiconductor chip X and another semiconductor chip X can be suppressed. Therefore, the electrode portions D of adjacent semiconductor chips X can be more reliably connected to each other. Therefore, the circuits of the plurality of semiconductor chips X are connected to each other with high reliability.

[0253] When directly connecting the electrode parts D to each other, for example, an atomic diffusion bonding method can be used. The atomic diffusion bonding method can be performed using, for example, a commercially available atomic diffusion bonding apparatus.

[0254] Next, the third to fifth embodiments are described in detail. It should be noted that the same description as the first or second embodiment is not repeated for the third to fifth embodiments. In the third to fifth embodiments, unless otherwise specified, the same operation as the first or second embodiment can be performed.

[0255] "Third Implementation Method"

[0256] The method for manufacturing a semiconductor device according to the third embodiment includes the above-mentioned steps similarly to the method for manufacturing a semiconductor device according to the second embodiment.

[0257] However, the manufacturing method of the semiconductor device of the third embodiment mainly differs from the second embodiment in the following aspects: a circuit structure element is arranged on one surface of the semiconductor chip W; in addition, in the fixing process, the semiconductor chip W overlapping the glass carrier G is not pasted on the adhesive layer 22 of the dicing tape 20, but the semiconductor chip W is pasted on the adhesive layer 22 in a state where the semiconductor chip W and the surface protection sheet 10 are stacked.

[0258] Specifically, in the method for manufacturing a semiconductor device according to the third embodiment, Fig. 7A As shown in FIG. 1 , a semiconductor wafer W to be attached to a back grinding tape B is prepared.

[0259] In the protection process, Figure 7B As shown, the protective layer 11 of the surface protective sheet 10 is attached to the semiconductor wafer W. At this time, the protective layer 11 of the surface protective sheet 10 is attached to one surface of the semiconductor wafer W, and the back grinding tape B is attached to the other surface. The circuit surface is formed on the above-mentioned one surface of the semiconductor wafer W.

[0260] Next, in the fixing process, Figure 7CAs shown, the back grinding tape B is peeled off from the semiconductor wafer W while the semiconductor wafer W and the surface protection sheet 10 are overlapped. Thus, the semiconductor wafer W and the surface protection sheet 10 are overlapped, and the other surface of the semiconductor wafer W (the surface without the circuit surface) is exposed.

[0261] In the fixing process of the third embodiment, Fig.7D As shown, the other surface of the semiconductor wafer W is attached to the adhesive layer 22 of the dicing tape 20 while the semiconductor wafer W is overlapped with the protective layer 11. At this time, the protective layer 11 is attached to one surface of the semiconductor wafer W, and the release liner 15 is also attached, so the semiconductor wafer W can be pressed to the adhesive layer 22 via the protective layer 11 and the release liner 15. Therefore, the circuit surface of the semiconductor wafer W can be protected, and the semiconductor wafer W can be attached to the adhesive layer 22.

[0262] In the fixing step, the protective layer 11 is preferably placed on the semiconductor wafer W in a state where the release liner 15 and the protective layer 11 are stacked, and the release liner 15 is preferably peeled from the protective layer 11 before the protective layer 11 is fragmented in the expanding step.

[0263] In the third embodiment, steps not particularly mentioned can be performed in the same manner as the steps in the first to fifth embodiments.

[0264] Next, the fourth embodiment will be described in detail. It should be noted that the same description as the above-mentioned embodiments will not be repeated for the fourth embodiment. In the fourth embodiment, unless otherwise specified, the same operations as those in the first to third embodiments can be performed.

[0265] "Fourth Implementation Method"

[0266] The method for manufacturing a semiconductor device according to the fourth embodiment mainly differs from the third embodiment in that, before the fixing step, the semiconductor wafer W is irradiated with laser light to form a weak portion inside the wafer.

[0267] Specifically, the method for manufacturing a semiconductor device according to the fourth embodiment includes a stealth processing step of forming a fragile portion inside a semiconductor wafer W on which a back grinding tape B is attached, using a laser, to prepare for cutting the semiconductor wafer W into small pieces.

[0268] In a fourth embodiment, the preparation Fig. 8A The semiconductor wafer W is shown in a state where it overlaps with the back grinding tape B. The semiconductor wafer W in such a state is thinned to a desired thickness by, for example, performing a back grinding process while the back grinding tape B is affixed thereto.

[0269] In the invisible processing step of the fourth embodiment, Figure 8B As shown, the semiconductor wafer W overlapped with the back grinding tape B is irradiated with laser light. The back grinding tape B is, for example, attached to the surface opposite to the circuit surface of the semiconductor wafer W. The laser light is irradiated from the circuit surface side of the semiconductor wafer W, for example.

[0270] In the protection process of the fourth embodiment, similarly to the third embodiment, Figure 8C As shown in FIG. 1 , the protective layer 11 of the surface protective sheet 10 is attached to the semiconductor wafer W. Thus, the protective layer 11 is overlapped on one side (circuit side) of the semiconductor wafer W, and the back grinding tape B is overlapped on the other side. Thereafter, the back grinding tape B is peeled off from the semiconductor wafer W. It should be noted that the semiconductor wafer W may also be overlapped with the back grinding tape B. Figure 8C As shown, a release liner 15 is overlapped on the protective layer 11 .

[0271] Afterwards, if Fig.8D and Fig. 8E As shown, the fixing step can be performed in the same manner as in the third embodiment.

[0272] In the fourth embodiment, steps not particularly mentioned can be performed in the same manner as the steps in the first to third embodiments.

[0273] Finally, the fifth embodiment is described in detail. It should be noted that the same description as the first to fourth embodiments is not repeated for the fifth embodiment. In the fifth embodiment, unless otherwise specified, the same operations as those in the first to fourth embodiments can be performed.

[0274] "Fifth Implementation Method"

[0275] The method for manufacturing a semiconductor device according to the fifth embodiment mainly differs from the other embodiments in that the semiconductor wafer W is attached to the adhesive layer 22 of the dicing tape 20 with the protective layer 11 disposed between the semiconductor wafer W and the back grinding tape B.

[0276] Specifically, in the method for manufacturing a semiconductor device according to the fifth embodiment, Fig.9A As shown, the protective layer 11 is laminated on the circuit surface of the semiconductor wafer W, and the back grinding tape B is laminated on the protective layer 11. It should be noted that the semiconductor wafer W can be laminated on the other surface of the protective layer 11 after the back grinding tape B is laminated on one surface of the protective layer 11, or the semiconductor wafer W can be laminated on the other surface of the protective layer 11 before the back grinding tape B is laminated on one surface of the protective layer 11.

[0277] In the state where the semiconductor wafer W, the protective layer 11 and the back grinding tape B are stacked, the surface of the semiconductor wafer W where no circuit components are arranged is ground. Fig.9A As shown in FIG. 1 , a grinding process (back grinding process) using a grinding pad K is performed until the semiconductor wafer W reaches a predetermined thickness. By the grinding process, the thickness of the semiconductor wafer W is reduced to a predetermined thickness (see FIG. 1 ). Fig. 9B ).

[0278] Next, in the fixing step, the surface of the semiconductor wafer W that has been ground (the surface on which the circuit components are not arranged) is superimposed on the adhesive layer 22 of the dicing tape 20. Fig. 9C As shown, a protective layer 11 is attached to the circuit surface of the semiconductor wafer W, and a back grinding tape B is attached to the protective layer 11 .

[0279] After the semiconductor wafer W is laminated on the adhesive layer 22 of the dicing tape 20, the stealth processing step can be performed in the same manner as described above. Then, the protective layer 11 attached to the semiconductor wafer W and the back grinding tape B are peeled off, and the back grinding tape B is removed (see Fig.9D ) It should be noted that the stealth processing step may be performed after the back grinding tape B is removed.

[0280] Thereafter, the expansion step of dividing the semiconductor wafer W and the protective layer 11 into small pieces, the removal step of removing the small pieces 11' of the protective layer adhered to the semiconductor chip X, the pickup step of taking out the semiconductor chip X, and the bonding step of bonding the semiconductor chip X to the adherend can be performed in the same manner as the above-mentioned method.

[0281] Although the method for manufacturing an electronic component device according to the embodiment of the present invention is as exemplified above, the present invention is not limited to the method for manufacturing an electronic component device exemplified above.

[0282] That is, various modes used in a general method for manufacturing an electronic component device may be adopted within a range that does not impair the effects of the present invention.

[0283] For example, as described above, the semiconductor wafer used in the manufacturing method of the present invention may be a semiconductor wafer having circuit surfaces formed on both sides as described in the first embodiment, or may be a semiconductor wafer having a circuit surface formed on only one side as described in other embodiments. In other words, of the two sides of the semiconductor chip manufactured in the manufacturing method of the present invention, circuit structure elements may be arranged only on one side, or circuit structure elements may be arranged on both sides.

[0284] Matters disclosed by this specification include the following. (1)

[0286] A surface protective composition for protecting at least one surface of a substrate, the surface protective composition comprising: a polymer having a hydrophilic group in a molecule; and a compound that generates an acid or a base by at least one of heating and irradiation with active energy rays.

[0287] The surface protective composition can form a protective layer that can be relatively easily removed when it comes into contact with a liquid containing water after covering at least one surface of a substrate in a manufactured electronic component. (2)

[0289] The surface protective composition according to the above (1), wherein the compound is a compound that generates an acid or a base upon irradiation with the active energy ray. (3)

[0291] The surface protective composition according to (1) or (2) above, wherein the hydrophilic group of the polymer is a hydroxyl group or a carboxyl group. (4)

[0293] The surface protective composition according to any one of (1) to (3), wherein the water absorption of the surface protective composition before the heating or before the irradiation with the active energy ray is 0.1% by mass or more and less than 1.5% by mass, and the water absorption of the surface protective composition after the heating or after the irradiation with the active energy ray using a high pressure mercury lamp at 500 mJ / cm 2 The water absorption after the irradiation was performed was 1.5% by mass or more. (5)

[0295] The surface protecting composition according to any one of (1) to (4) above, wherein the polymer is polyvinyl alcohol or polyethylene oxide. (6)

[0297] A surface protection sheet comprising a protective layer formed from the surface protection composition according to any one of (1) to (5) above. (7)

[0299] The surface protection sheet according to the above (6), further comprising a release liner superimposed on at least one surface of the protection layer. (8)

[0301] A method for manufacturing an electronic component device, comprising: a step of overlapping a protective layer formed of a surface protective composition on at least one of the two surfaces of a substrate to be protected, thereby protecting the protected surface; and a step of removing the protective layer overlapping the protected surface, wherein the surface protective composition comprises: a polymer having a hydrophilic group in a molecule, and a compound that generates an acid or a base by at least one of heating or irradiation with active energy rays, wherein in the removal step, the acid or the base is generated by the compound by heating or irradiation with active energy rays, thereby increasing the hydrophilicity of the protective layer, and the protective layer is removed by dissolving at least a portion of the protective layer in a liquid containing water.

[0302] This method of manufacturing an electronic component device can suppress adhesion of foreign matter to at least one surface of a substrate in the manufactured electronic component device by the protective layer, and can subsequently remove the protective layer relatively easily by bringing the protective layer into contact with a liquid containing water. (9)

[0304] The method for manufacturing an electronic component device according to (8) above, wherein a circuit component is arranged on the protected surface of the substrate.

[0305] Example

[0306] Next, the present invention will be described in further detail using experimental examples, but the present invention is not limited thereto.

[0307] A commercially available product (product name "V-12SR", manufactured by Nitto Denko Corporation) was prepared as a dicing tape. In addition, a silicon bare wafer (disk-shaped with a thickness of 50 μm and a diameter of 300 mm) was used instead of a semiconductor wafer.

[0308] A surface protection sheet was prepared as follows. Specifically, a surface protection composition containing a solvent was applied to one surface of a release liner, and the solvent was volatilized, thereby laminating the protective layer and the release liner. Furthermore, the release liner was attached to the protective layer to prepare a surface protection sheet in which the protective layer was arranged between two release liners.

[0309] [Examples 1 to 10, Comparative Examples]

[0310] (Production of Surface Protection Sheet a)

[0311] The following polyvinyl alcohol (commercially available product) was prepared. The polyvinyl alcohol (PVA) was dissolved in any of the following alcohol aqueous solutions to prepare a PVA solution. The following photoacid generator or photobase generator was added and mixed to the prepared PVA solution in an amount shown in Table 1 relative to 100 parts by mass of PVA. Each PVA solution was applied to a release liner a (PET film, thickness 50 μm). Each release liner a has a surface treated with silicone release, and the above-mentioned PVA solution is applied to the surface using an applicator. Moreover, a drying treatment was performed at 110°C for 2 minutes to form a protective layer with a thickness of 10 μm overlapping one surface of the release liner a. Thereafter, a release liner b (PET film, thickness 25 μm) was superimposed on the exposed surface of each protective layer. It should be noted that each release liner b has a surface treated with silicone release, and the surface is adhered to the protective layer. In this way, a surface protection sheet a sandwiched between two release liners was produced.

[0312] Polyvinyl alcohol

[0313] Saponification degree: 35 (mol%), average polymerization degree: 200.

[0314] Alcohol aqueous solution

[0315] 50% ethanol aqueous solution (Examples 1 to 3, 9, 10, Comparative Example).

[0316] 60% aqueous solution of isopropanol (Examples 4 to 8).

[0317] Photoacid generator

[0318] Sulfonium salt type, product name "CPI-200K", manufactured by San-Apro Co., Ltd. (gas phase acidity: 256).

[0319] Chemical name: diphenyl[4-(phenylthio)phenyl]sulfonium=trifluorotris(pentafluoroethyl)-λ 5 -Phosphate [Alias: Diphenyl [4- (phenylthio) phenyl] sulfonium trifluorotris (1,1,2,2,2-pentafluoroethyl) phosphate (1-) (1:1), its English is Diphenyl [4- (phenylthio) phenyl] sulfonium, trifluorotris (1,1,2,2,2-pentafluoroethyl) phosphate (1-) (1:1)].

[0320] Sulfonium salt type, product name "CPI-310FG", manufactured by San-Apro (gas phase acidity: 259).

[0321] Ionium salt type, product name "IK-1", manufactured by San-Apro Co., Ltd. (gas phase acidity: 256).

[0322] Chemical name: (4-isopropylphenyl)(4-methylphenyl)iodonium=trifluoro[tris(pentafluoroethyl)]-λ 5 -Phosphate [Alias: [4-(1-methylethyl)phenyl](4-methylphenyl)iodonium trifluorotris(1,1,2,2,2-pentafluoroethyl)phosphate (1-)(1:1), its English is [4-(1-Methylethyl)phenyl](4-methylphenyl)iodonium,trifluorotris(1,1,2,2,2-pentafluoroethyl)phosphate (1-)(1:1)].

[0323] Photobase generator

[0324] Product name: "WPBG-266", manufactured by Fujifilm Corporation.

[0325] Chemical name: 2-(3-Benzoylphenyl)propionic acid 1,2-diisopropyl-3[bis(dimethylamino)methylene]guanidine, its English is 2-(3-Benzoylphenyl)propionic acid 1,2-diisopropyl-3[bis(dimethylamino)methylene]guanidine [Alias: Benzeneacetic acid, 3-benzoyl-α-methyl-, compd. with N, N, N', N'-tetramethyl-N"-[[(1-methylethyl)amino][(1-methylethyl)imino]methyl]guanidine (1:1)].

[0326] (Fixing process and protection process)

[0327] The release liner b was peeled off from the produced surface protection sheet a to expose one surface of the protection layer, and the exposed surface was bonded to a silicon bare wafer (substrate) superposed on a dicing tape.

[0328] The exposed surface of the wafer (the surface opposite to the contact surface of the dicing tape) was bonded to the exposed surface of the protective layer after the release liner b was peeled off. During bonding, a MV3000 vacuum mounter (mounter) manufactured by Nitto Seiki Co., Ltd. was used with the workbench temperature heated to 90°C. In this way, the dicing tape, the silicon bare wafer, and the protective layer were stacked in sequence.

[0329] (Removal process)

[0330] The protective layer was subjected to a high pressure mercury lamp at 500 mJ / cm 2 The irradiation treatment (including ultraviolet light irradiation treatment) performed increased the hydrophilicity of the protective layer. Afterwards, in order to remove the protective layer, a cleaning unit (product name DFD6361) manufactured by DISCO was used to implement the removal process as described below. The disc-shaped workbench supporting the dicing tape from below was rotated in the circumferential direction, and 25°C water was sprayed onto the semiconductor chips of the small pieces attached to the chip bonding sheet. The rotation speed of the workbench was 1000 rpm, and the water spraying time was shown in Table 1.

[0331] [Comparative Example]

[0332] Surface protection sheet b was prepared in the same manner as in Example 1 except that no photoacid generator was added to the PVA aqueous solution when preparing the protective layer of the surface protection sheet; ultraviolet rays were not irradiated on the fragmented protective layer in the removal step; and the water spraying time in the removal step was changed.

[0333] <Water absorption rate of protective layer before and after UV irradiation>

[0334] The water absorption rate of the protective layer was measured by Karl Fischer Coulometry using a moisture measuring device (product name "CA-07") and a moisture vaporization device (product name "VA-07") manufactured by Mitsubishi Chemical Analytical Co., Ltd. Specifically, a test sample of the protective layer weighed to about 4 mg was placed in a steady state at 23°C and 50 RH%. Thereafter, the test sample was heated at 150°C for 3 minutes using a moisture vaporization device to evaporate the moisture in the test sample, and the amount of vaporized moisture was measured.

[0335] The water absorption rate was calculated from the ratio of the measured water content to the mass of the test sample before heating.

[0336] <Evaluation: Adhesion to substrate (before ultraviolet irradiation)>

[0337] The adhesion of the protective layer to the silicon bare wafer was evaluated according to the following evaluation criteria.

[0338] (Good) The adhesion of the protective layer to the silicon bare wafer is 0.2 N / 100 mm or more.

[0339] (Poor) The adhesion of the protective layer to the silicon bare wafer is less than 0.2N / 100mm.

[0340] <Evaluation: Ease of removing the protective layer (after UV irradiation)>

[0341] After the removal process is performed as described above, the water used to remove the protective layer is removed. In addition, the surface of the silicon bare wafer is analyzed using a Fourier transform infrared spectrophotometer (FT-IR). The presence or absence of residual organic matter is confirmed by this analysis. It should be noted that the evaluation criteria related to the ease of removing the protective layer are as follows.

[0342] (Good) No residue of protective layer can be visually confirmed (800-4000cm -1 The maximum absorption under is below 0.05).

[0343] (Slightly better) No residue of the protective layer can be visually confirmed (however, 800-4000cm -1 The maximum absorption under the condition is greater than 0.05).

[0344] (Poor) Residues of the protective layer were visually observed.

[0345] As described above, each production method of Examples and Comparative Examples was carried out. Table 1 shows the details of the protective layer of the surface protection sheet used in each production method and the evaluation results.

[0346] [Table 1]

[0347]

[0348] As can be understood from the above evaluation results, by manufacturing a semiconductor device using the manufacturing method of the semiconductor device of the embodiment, foreign matter can be prevented from adhering to the circuit surface of the semiconductor chip (die), thereby protecting the circuit surface. In addition, in the removal process, the plurality of protective layers that have been cut into small pieces can be removed more easily using water, so the semiconductor device can be manufactured efficiently. It should be noted that in the removal process, no matter how much or how little energy is irradiated to the protective layer (no matter how long or short the ultraviolet irradiation time is), there is no big difference in the removability of the protective layer.

[0349] By implementing the method for manufacturing a semiconductor device according to the above-described embodiment, a semiconductor device or the like in which a plurality of semiconductor chips to which foreign matter and the like are hardly attached are stacked can be efficiently manufactured.

[0350] Industrial Applicability

[0351] The method for manufacturing an electronic component device of the present invention is preferably used for manufacturing a semiconductor device including a semiconductor integrated circuit or the like, for example.

[0352] Description of Reference Numerals

[0353] 10: surface protection sheet; 11: protection layer; 11': small piece of protection layer; 15: release liner; 20: dicing tape; 21: substrate layer; 22: adhesive layer; 30: chip bonding sheet; G: glass carrier; W: semiconductor wafer; X: semiconductor chip; V: through hole; D: electrode part; B: back grinding tape.

Claims

1. A surface protective composition for protecting at least one surface of a substrate. The surface protective composition includes a polymer having a hydrophilic group in its molecule and a compound that generates an acid or a base by at least one of heating and irradiation with active energy rays.

2. The surface protecting composition according to claim 1, wherein The compound is a compound that generates an acid or a base upon irradiation with the active energy rays.

3. The surface protective composition according to claim 1 or 2, wherein The hydrophilic group of the polymer is a hydroxyl group or a carboxyl group.

4. The surface protective composition according to claim 1 or 2, wherein The surface protective composition has a water absorption rate of 0.1% by mass or more and less than 1.5% by mass before being heated or irradiated with active energy rays. The water absorption rate of the surface protective composition after the heating, or after the irradiation of the active energy ray with a high pressure mercury lamp at 500 mJ / cm 2 The water absorption after the irradiation was performed was 1.5% by mass or more. 5 . A surface protection sheet comprising a protective layer formed from the surface protection composition according to claim 1 .

6. The surface protection sheet according to claim 5, wherein The invention further comprises a release liner superposed on at least one surface of the protective layer.

7. A method for manufacturing an electronic component device, comprising: a step of overlaying a protective layer formed of a surface protective composition on at least one of the two surfaces of the substrate to be protected, thereby protecting the protected surface; as well as The step of removing the protective layer overlapping the protected surface, The surface protective composition comprises: a polymer having a hydrophilic group in its molecule; and a compound that generates an acid or a base by at least one of heating and irradiation with active energy rays. In the removal step, the acid or base is generated from the compound by heating or irradiation with active energy rays, thereby increasing the hydrophilicity of the protective layer, and the protective layer is removed by dissolving at least a portion of the protective layer in a liquid containing water.

8. The method for manufacturing an electronic component device according to claim 7, wherein: Circuit components are arranged on the protected surface of the substrate.