Infrared heating source and preparation method thereof
By designing infrared heat source of ceramic base and electric heat radiation elements, the problems of nerve inhibition, smoke and uncertain efficacy in moxibustion are solved, and radiation characteristics similar to moxibustion are achieved, which promotes blood circulation and nervous system balance and provides effective health care effects.
Patent Information
- Application Number
- CN202411119254.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-12
AI Technical Summary
During the use of moxibustion, there are problems of nerve inhibition, smoke generation, release of toxic substances and uncertain efficacy. The existing infrared moxibustion therapy devices cannot fully reproduce the radiation spectrum and power of traditional moxibustion.
An infrared heat source was designed, using a ceramic base and an electric heating radiation element, including a far-infrared ceramic sintered body and embedded carbon fiber, and a full-band infrared light with a central wavelength of 3.5μm, combining the thermal insulation effect of the ceramic base and The high temperature stability of carbon fiber simulates the radiation characteristics of moxibustion.
The radiation spectrum and power similar to moxibustion are achieved, which promotes blood circulation, improves microcirculation, balances the autonomic nervous system, provides acupuncture-like health care effects, and effectively prevents and improves diseases.
Smart Images

Figure CN118924618A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of health care products, and in particular to an infrared heating source and a preparation method thereof. Background Art
[0002] Moxibustion, also known as moxibustion therapy or moxibustion method, is a treatment method that uses moxa sticks or moxa cones made of mugwort leaves. The heat generated by the moxa stimulates the acupuncture points or specific parts of the human body, and then adjusts the disordered physiological and biochemical functions of the human body by stimulating the activity of meridian qi, thereby achieving the purpose of preventing and curing diseases.
[0003] Moxibustion is an effective treatment method that has been verified for thousands of years. However, there are also some common disadvantages in the specific treatment process: (1) Long-term use of moxibustion and excessive use of volatile oils in moxa can have an inhibitory effect on nerves and can damage the patient's central nervous system; (2) The smoke produced by moxa sticks during moxibustion may cause dry mouth, inflammation, and even nausea and vomiting when the patient breathes for a long time; (3) The smoke produced during moxibustion has complex components and contains some toxic substances. The extract of moxa smoke may have a mutagenic effect and is a chromosome breaking agent; (4) In the actual treatment process, the origin of the moxa sticks, the storage year, the moxa ratio, and the production process all have an uncertain impact on the final efficacy.
[0004] To overcome the drawbacks of moxibustion, recreating traditional Chinese medicine moxibustion with modern technology is an attractive research topic. Currently developed infrared moxibustion heating devices primarily utilize the human body's characteristic absorption of infrared light of specific wavelengths. When the body absorbs far-infrared light, not only does it produce a thermal effect on the skin's surface, but it also resonates within cellular tissue, causing biomolecules to reach a higher vibrational energy level, mobilizing the body's disease resistance, thereby exerting a therapeutic effect and improving local symptoms. Using modern engineering methods, if a heat source with the same emission spectrum, power, and irradiation area as moxibustion can be produced, it will be possible to better replicate traditional Chinese medicine moxibustion, leading to even better therapeutic results. Summary of the Invention
[0005] Based on the technical problems existing in the background technology, the present invention proposes an infrared heating source and a preparation method thereof. The infrared heating source has the function of radiating near, middle and far full-band infrared light with a central wavelength of 3.5μm (the same as the thermal radiation wavelength of moxa sticks in the spontaneous combustion state), thereby achieving the basic reproduction of the moxibustion radiation spectrum, thereby achieving the purpose of better therapeutic effect.
[0006] The infrared heat source proposed by the present invention comprises a ceramic base and an electric heat radiation element placed in a groove on the surface of the ceramic base;
[0007] The electrothermal radiation element includes a far-infrared ceramic sintered body and carbon fibers embedded in the far-infrared ceramic sintered body.
[0008] In the present invention, the ceramic base has an excellent thermal insulation effect, which is used to reduce unnecessary heat loss of the electric heating radiation element placed therein; the electric heating radiation element includes carbon fiber as a heating element and a far-infrared ceramic sintered body as a radiation element, which is used to generate heat and provide far-infrared rays, thereby promoting blood circulation and improving microcirculation; compared with the existing technology, the carbon fiber embedded in the far-infrared ceramic sintered body can provide high-temperature heat of 500-800°C for the far-infrared ceramic sintered body while avoiding oxidation (carbon fiber will oxidize at high temperatures exceeding 200°C, while embedding it in the far-infrared ceramic sintered body can avoid oxidation at high temperatures exceeding 1000°C), thereby enabling the far-infrared ceramic sintered body to efficiently radiate full-band infrared light with a central wavelength of 3.5μm.
[0009] Preferably, the infrared heat source further includes positive and negative metal electrodes; the positive and negative metal electrodes pass through the surface of the ceramic base to open holes and are connected to the carbon fibers in the electric heat radiation element, so as to electrically connect the electric heat radiation element to an external power supply.
[0010] Preferably, the infrared heat source further includes a temperature sensor; the temperature sensor passes through a cavity on the surface of the ceramic base and is connected to the far-infrared ceramic sintered body in the electric heat radiation element, for measuring the temperature of the electric heat radiation element.
[0011] The present invention also proposes a method for preparing the above-mentioned infrared heat source, comprising: forming a groove on the surface of a ceramic base, adding carbon fiber into the groove, then filling the groove with far-infrared ceramic powder, compacting it to form an electric heating radiation element embryo, and then placing it in a kiln for sintering to obtain the infrared heat source.
[0012] Preferably, the far-infrared ceramic powder is infrared ceramic powder modified by an aminosilane coupling agent.
[0013] Preferably, the aminosilane coupling agent is γ-aminopropyltrimethoxysilane or γ-aminopropyltriethoxysilane.
[0014] Preferably, the far-infrared ceramic powder further includes a sintering aid;
[0015] Preferably, the sintering aid is yttrium trioxide or aluminum trioxide.
[0016] Preferably, the carbon fiber is surface oxidized carbon fiber;
[0017] Preferably, the specification of the carbon fiber is 1-12K, and the fiber diameter is 5-9 μm.
[0018] In the present invention, there is electrostatic attraction between the amino groups contained in the infrared ceramic powder modified with the aminosilane coupling agent and the carboxyl groups contained in the surface oxidized carbon fibers. After the two are compositely sintered, a cross-linked network structure can be formed, thereby making the carbon fibers heat evenly and the heat can be effectively transferred to the far-infrared ceramic sintered body, thereby exerting a good far-infrared radiation effect.
[0019] Preferably, the volume content of the carbon fiber in the far-infrared ceramic powder is 5-50 vol%.
[0020] Preferably, the sintering temperature is 1000-1400° C., and the sintering time is 1-3 hours.
[0021] Preferably, the preparation method further comprises: reserving channels in the electrothermal radiation element embryo for installing positive and negative metal electrodes and / or temperature sensors, and opening a cavity on the surface of the ceramic base extending to the channels.
[0022] The infrared heat source of the present invention has a reasonable structure. By arranging an electric heating radiation element to generate heat and provide far infrared rays, it promotes blood circulation, improves microcirculation, balances the human autonomic nervous system, promotes the body's metabolism, and unblocks blocked meridians, thus forming a health-care effect similar to acupuncture, and effectively preventing and improving diseases. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is a schematic structural diagram of the infrared heat source described in Example 1 of the present invention;
[0024] Figure 2 This is a thermal radiation curve diagram of the infrared heating source of Example 3 of the present invention. DETAILED DESCRIPTION
[0025] Hereinafter, the technical solutions of the present invention will be described in detail through specific embodiments. However, it should be clearly stated that these embodiments are provided for illustration only and are not to be construed as limiting the scope of the present invention.
[0026] Example 1
[0027] Reference Figure 1, this embodiment proposes an infrared heat source, including a ceramic base 2, the ceramic base is made of zirconia, the thermal conductivity is between 2-3W / m·k, and it has excellent heat insulation effect; a groove is opened on the surface of the ceramic base 2, and an electric heat radiation element is formed in the groove, the electric heat radiation element includes a far-infrared ceramic sintered body 6 and carbon fiber 7 embedded in the far-infrared ceramic sintered body. The carbon fiber serves as a heating element to provide heat for the far-infrared ceramic sintered body. The far-infrared ceramic sintered body can not only provide a high temperature of 500-800°C, but also can excite the far-infrared ceramic sintered body 6 to radiate full-band infrared light with a central wavelength of 3.5μm at this temperature; in addition, the infrared heat source also includes a positive metal electrode 3 and a negative metal electrode 4, which pass through the surface of the ceramic base 2. A cavity is provided and connected to the carbon fiber 7 in the electric heat radiation element. During operation, the positive and negative metal electrodes can be electrically connected to an external power supply to energize the carbon fiber 7 and convert electrical energy into thermal energy, thereby causing the electric heat radiation element to heat up and stimulate the far-infrared ceramic sintered body 6 to radiate far-infrared rays of a specific wavelength; further, the infrared heat source also includes a temperature sensor 5, and a high-temperature thermocouple can be selected as the temperature sensor. The temperature sensor 5 also passes through the surface of the ceramic base 2 to provide a cavity and is connected to the far-infrared ceramic sintered body 6 in the electric heat radiation element. During operation, the control system adjusts the current supplied by the external power supply to the carbon fiber 7 according to the temperature of the electric heat radiation element measured by the temperature sensor 5, so that the temperature of the electric heat radiation element is maintained at a constant value with an upper and lower deviation of no more than 2%.
[0028] In actual use, the infrared heating source of this embodiment can be placed in an outer cover 1 made of a heat-insulating ceramic material. The heating source is 3 cm away from the port of the outer cover 1 to ensure that the patient's skin is not burned while ensuring the effects of hot compress and infrared radiation, thereby achieving hot moxibustion for the user.
[0029] The infrared heat source preparation method proposed in this embodiment includes: forming a groove on the surface of a ceramic base, adding carbon fiber into the groove, and then adding far-infrared ceramic powder and a sintering aid to fill the groove. The carbon fiber accounts for 5-50% by volume of the far-infrared ceramic powder, and the sintering aid accounts for 1-5% by weight of the far-infrared ceramic powder. After vibrating and mixing, the mixture is die-cast and compacted to form an electric heating radiation element embryo. The embryo is then sintered in a kiln under inert atmosphere conditions at a temperature of 1000-1400°C for 1-3 hours to obtain the infrared heat source. Furthermore, the method includes reserving channels in the electric heating radiation element embryo for mounting positive and negative metal electrodes and a temperature sensor, and forming a cavity on the surface of the ceramic base extending to the channel. During the actual preparation process, the positive and negative metal electrodes and the temperature sensor pass through the cavity on the surface of the ceramic base and into the channel. The gap between the channels is sealed with high-temperature resistant ceramic glue that can withstand temperatures up to 1800°C, ensuring that the carbon fiber is completely sealed.
[0030] Example 2
[0031] This embodiment proposes an infrared heat source and a preparation method thereof. The structure of the infrared heat source is the same as that of Example 1, except that it specifically selects carbon fiber (specification 3K, fiber diameter 6.9 μm), far-infrared ceramic powder (composed of MgO-Al2O3-TiO2-ZrO2, average particle size 0.02 μm) and Al2O3 (average particle size 0.5 μm) sintering aids. The volume content of the carbon fiber in the far-infrared ceramic powder is 20 vol%, and the mass content of the sintering aid in the far-infrared ceramic powder is 3 wt%. The sintering temperature is 1200°C and the time is 2 h.
[0032] Example 3
[0033] This embodiment provides an infrared heat source and a preparation method thereof. The structure of the infrared heat source is the same as that of Example 1, except that surface-oxidized carbon fibers, infrared ceramic powder modified with an aminosilane coupling agent, and a sintering aid of Al2O3 (average particle size of 0.5 μm) are specifically selected. The volume content of the carbon fibers in the far-infrared ceramic powder is 20 vol%, and the mass content of the sintering aid in the far-infrared ceramic powder is 3 wt%. The sintering temperature is 1200°C, and the sintering time is 2 h.
[0034] Among them, the surface oxidized carbon fiber is prepared by the following method: immersing carbon fiber (specification 3K, fiber diameter 6.9μm) in concentrated nitric acid, ultrasonically dispersing for 0.5h, heating under reflux for 24h, filtering, washing with water, and drying to obtain surface oxidized carbon fiber; the aminosilane coupling agent modified infrared ceramic powder is prepared by the following method: immersing far-infrared ceramic powder (composed of MgO-Al2O3-TiO2-ZrO2, with an average particle size of 0.02μm) in an ethanol-water (volume ratio of 3:1) mixed solvent containing γ-aminopropyltriethoxysilane, the amount of γ-aminopropyltriethoxysilane is 3wt% of the far-infrared ceramic powder, oxalic acid is added to adjust the pH value to 4, ultrasonically dispersing for 0.5h, heating under reflux for 4h, filtering, washing with alcohol, washing with water, and drying to obtain aminosilane coupling agent modified infrared ceramic powder.
[0035] The thermal radiation curve of the above infrared heat source is as follows Figure 2 As shown, the thermal radiation characteristics of moxa sticks are basically the same as those in the spontaneous combustion state.
[0036] Performance testing:
[0037] The infrared heat sources described in Examples 2 and 3 were tested for infrared radiation dominant wavelength and emissivity using the method of national standard GB / T7287-2008. The test results are shown in Table 1.
[0038] Table 1 Performance test results of the infrared heating source described in the embodiment
[0039] Radiation dominant wavelength (μm) emissivity Heating rate (℃ / min) Example 2 2-12 0.86 36 Example 3 2-12 0.93 53
[0040] The above description is only a preferred specific embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any technician familiar with the technical field, within the technical scope disclosed by the present invention, who makes equivalent replacements or changes based on the technical solution and inventive concept of the present invention, should be covered by the scope of protection of the present invention.
Claims
1. An infrared heat source, characterized in that: It comprises a ceramic base and an electric heat radiation element placed in a groove on the surface of the ceramic base; Wherein, the electric heat radiation element includes a far-infrared ceramic sintered body and carbon fibers embedded in the far-infrared ceramic sintered body.
2. The infrared heat source according to claim 1, characterized in that: It also includes positive and negative metal electrodes; the positive and negative metal electrodes pass through the surface of the ceramic base to open holes and are connected to the carbon fibers in the electric heat radiation element, so as to electrically connect the electric heat radiation element to an external power source.
3. The infrared heat source according to claim 1 or 2, characterized in that: It also includes a temperature sensor; the temperature sensor passes through a cavity on the surface of the ceramic base and is connected to the far-infrared ceramic sintered body in the electric heat radiation element, so as to measure the temperature of the electric heat radiation element.
4. A method for preparing the infrared heat source according to any one of claims 1 to 3, characterized in that: include: A groove is formed on the surface of the ceramic base, carbon fiber is added into the groove, and then the groove is filled with far-infrared ceramic powder, compacted to form an electric heat radiation element embryo, and then placed in a kiln for sintering to obtain the infrared heat source.
5. The method for preparing the infrared heat source according to claim 4, characterized in that: The far-infrared ceramic powder is far-infrared ceramic powder modified by an aminosilane coupling agent; Preferably, the aminosilane coupling agent is γ-aminopropyltrimethoxysilane or γ-aminopropyltriethoxysilane.
6. The method for preparing the infrared heat source according to claim 5, characterized in that: The far-infrared ceramic powder also includes a sintering aid; Preferably, the sintering aid is yttrium trioxide or aluminum trioxide.
7. The method for preparing an infrared heat source according to any one of claims 4 to 6, characterized in that: The carbon fiber is surface oxidized carbon fiber; Preferably, the specification of the carbon fiber is 1-12K, and the fiber diameter is 5-9 μm.
8. The method for preparing the infrared heat source according to claim 7, characterized in that: The volume content of the carbon fiber in the far-infrared ceramic powder is 5-50 vol%.
9. The method for preparing an infrared heat source according to any one of claims 4 to 8, characterized in that: The sintering is carried out under an inert atmosphere; Preferably, the sintering temperature is 1000-1400° C., and the sintering time is 1-3 hours.
10. The method for preparing an infrared heat source according to any one of claims 4 to 9, characterized in that: Also includes: A hole for installing positive and negative metal electrodes and / or a temperature sensor is reserved in the pressed embryo of the electric heat radiation element, and a cavity extending to the hole is opened on the surface of the ceramic base.