Process for extracting potassium in Bayer mother liquor by using composite potassium adsorbent
Through the preparation and application of composite potassium adsorbent, the problem of excessive addition of external substances extracted from potassium in the Bayer method mother liquor is solved, efficient potassium recycling and improved alumina quality, simplifying the process flow and reducing costs.
Patent Information
- Application Number
- CN202410979374.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-04-23
- Filing Date
- 2024-05-15
- Publication Date
- 2024-11-12
AI Technical Summary
In the prior art, when extracting potassium from the mother liquor produced by Bayer method, excessive addition of external substances has caused a large impact on alumina production, complex process and high cost, and has failed to achieve commercial application.
Complex potassium adsorbent is prepared from inorganic aluminum salts, inorganic silicates and inorganic potassium salts in an alkaline environment, and the adsorbent that combines polysulfone to form a porous structure is prepared by ultrasonic mixing, calcining and polysulfone wrapping. Adsorb and desorb potassium ions to achieve efficient recovery of potassium.
It realizes efficient extraction and recycling of potassium in Bayer mother liquor, improves the quality of alumina products, simplifies the process flow, reduces production costs, and avoids interference to alumina production.
Smart Images

Figure CN118925654A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of potassium ion adsorbents and relates to a process for extracting potassium from Bayer mother liquor by using a composite potassium adsorbent. Background Art
[0002] Potassium and its compounds are widely used in agriculture, energy, chemical industry, medical and other fields, and are important agricultural and industrial materials. In recent years, with the rapid development of the aluminum industry and the large-scale use of bauxite resources, some problems existing in bauxite have also become prominent.
[0003] The Bayer process for producing alumina is a cyclic process, in which the potassium content in the mother liquor can reach 75g / L. Such a high concentration of potassium will not only increase the potassium content in the produced alumina and reduce the quality of alumina, but also cause the electrolyte system in the downstream electrolytic aluminum process to become complicated and the conductivity to decrease, thereby increasing the electrolysis energy consumption and reducing the life of the electrolytic cell, seriously affecting the normal production of electrolytic aluminum enterprises, but also providing a new source of potassium.
[0004] At present, the method of extracting potassium from alumina mother liquor is mainly to add carbonate, tartrate and nitrate and then obtain the corresponding potassium salt by using the solubility difference after multiple evaporation and cooling crystallization, or to extract potassium from the mother liquor by precipitation method.
[0005] Patent CN103601221A discloses a method for extracting potassium nitrate from the circulating mother liquor of alumina produced by the Bayer process. The method adds sodium nitrate to the circulating mother liquor and extracts potassium nitrate by multiple cooling and crystallization. However, since a large amount of sodium nitrate needs to be added, the impact of a large amount of nitrate on subsequent alumina production is uncertain, and the energy consumption of cooling and heating is also high, this method has not been applied in large quantities.
[0006] Patent CN115417431A discloses a method for extracting potassium in the process of producing alumina by the Bayer process. The method uses sodium tetraphenylborate solution as a precipitant, and potassium ions are precipitated in the form of potassium tetraphenylborate. The solid-liquid separation and solid washing are performed to obtain potassium tetraphenylborate, and potassium tetraphenylborate is calcined to obtain potassium oxide and boron oxide. Patent CN104445277A discloses a method for separating potassium oxide from a potassium-containing sodium aluminate solution. The method uses one or a mixture of sodium sulfate, aluminum sulfate (basic aluminum sulfate), potassium (sodium) alum, and alumite ore (pure alumite) to introduce SO4 2-, so that the potassium oxide in the sodium aluminate solution is converted into potassium sulfate, which is separated and precipitated in the form of glauberite. Glauberite is then purified into potassium sulfate by temperature-variable dissolution separation, potassium chloride conversion, potassium aluminate replacement and other methods. The precipitation is carried out under high caustic soda and low temperature conditions, which can avoid sodium sulfate from remaining in the solution and purify the solution. Both methods precipitate potassium by adding a large amount of external substances to the sodium aluminate solution. The added external substances have a large amount of residues in the Bayer mother liquor, which affects the subsequent alumina production. In addition, the production process is long and the process is complicated. The above methods have not been commercially applied.
[0007] Potassium salt is the material basis of agricultural production. It is irreplaceable and indispensable. About 95% of potassium salt is used to produce potassium fertilizer. It is called the "food" of grain. It can effectively improve the growth, development, photosynthesis and stress resistance of plants. It has great economic potential and strategic value.
[0008] Therefore, in order to recycle potassium in the Bayer process for producing alumina, it is necessary to develop a new process for extracting potassium and synthesizing potassium salts. Summary of the invention
[0009] The object of the present invention is to provide a process for extracting potassium from Bayer mother liquor by using a composite potassium adsorbent. The preparation process of the composite potassium adsorbent is easy to control, can be used for recovering potassium ions from Bayer mother liquor, can effectively extract potassium ions from Bayer mother liquor, does not affect the production of alumina, and has a simple and efficient process.
[0010] The purpose of the present invention can be achieved through the following technical solutions:
[0011] A method for preparing a composite potassium adsorbent comprises the following steps:
[0012] S11, adding an inorganic aluminum salt, an inorganic silicate and an inorganic potassium salt in a molar ratio of (1-3): (4-15): 1 to an alkaline solution with a concentration of 0.5-1 mol / L, and ultrasonically mixing for 2 hours, heating and evaporating the solution to a solid, and then calcining at 250-350° C. for 1-4 hours, and preparing an active complex salt after the calcination is completed;
[0013] S12, dissolving polysulfone molecules in an organic solvent to obtain a uniform polysulfone solution with a mass fraction of 10 to 40%, uniformly dispersing an active double salt in the polysulfone solution, wherein the mass fraction of the active double salt is 20 to 60%, and then dropping the polysulfone solution mixed with the active double salt into deionized water, and filtering to obtain polysulfone-coated solid particles;
[0014] S13, drying the polysulfone-wrapped solid particles in a vacuum drying oven at 80-100° C. for 10-16 hours, sterilizing them with an ultraviolet light for 35-45 minutes, and then cooling them to 25-35° C. to prepare the composite potassium adsorbent.
[0015] As a preferred technical solution of the present invention, in step S11, the alkali is sodium hydroxide.
[0016] As a preferred technical solution of the present invention, in step S12, the inorganic aluminum salt is one of aluminum sulfate and aluminum chloride, the inorganic silicate is sodium silicate, and the inorganic potassium salt is one of potassium chloride, potassium sulfate and potassium hydroxide.
[0017] As a preferred technical solution of the present invention, in step S12, the organic solvent is one or more of N,N-dimethylacetamide, N,N-dimethylformamide, N-methylpyrrolidone and 1,4-dioxane.
[0018] A process for extracting potassium from Bayer mother liquor using a composite potassium adsorbent comprises the following steps:
[0019] S51, adsorption: passing the Bayer mother liquor into an adsorption device loaded with the composite potassium adsorbent prepared in S13, and stopping the adsorption when the potassium ion concentration in the effluent after adsorption is close to 10-50% of the potassium ion concentration in the feed solution. The temperature of the Bayer mother liquor during adsorption is 20-60° C.;
[0020] S52, washing: passing deionized water or a sodium hydroxide solution with a mass fraction of 0.1-2% as a cleaning liquid into the adsorption device after the adsorption is completed to clean the composite potassium adsorbent after step S51, and wash away the Bayer mother liquor and impurities adsorbed on the surface;
[0021] S53, desorption: at 60-100° C., passing the prepared desorption liquid into the adsorption device to desorb the composite potassium adsorbent after step S52, so that the potassium ions adsorbed in the composite potassium adsorbent are desorbed into the desorption liquid to obtain a potassium-enriched desorption liquid;
[0022] S54, washing: using deionized water or a sodium hydroxide solution with a mass fraction of 0.1-2% to wash the composite potassium adsorbent after step S53, and the composite potassium adsorbent can be recycled after washing;
[0023] S55, filtering: removing impurities from the potassium-enriched desorption liquid by using a nanofiltration membrane to remove calcium, magnesium, aluminum, and iron impurity ions, wherein the nanofiltration membrane is a polyamide nanofiltration membrane or a polypiperazineamide nanofiltration membrane;
[0024] S56, purification: the potassium-rich liquid after impurities are removed is evaporated, concentrated, crystallized and heat-insulated to settle. The sodium salt precipitated first is used for the preparation of the desorption liquid, and then cooled and crystallized to precipitate the potassium salt. The potassium salt product is obtained after centrifugal separation, saturated potassium salt washing and purification, drying and packaging.
[0025] As a preferred technical solution of the present invention, in step S51, the Bayer mother liquor is one of the seed mother liquor, the circulating mother liquor, the evaporated mother liquor and the gallium-extracted mother liquor after gallium extraction, and contains potassium ions at a concentration of 10 to 100 g / L.
[0026] As a preferred technical solution of the present invention, in step S51, the adsorption device is one of an adsorption tower, an adsorption column and an adsorption tank.
[0027] As a preferred technical solution of the present invention, in step S51, the Bayer mother liquor after adsorption can be directly used in the next step of Bayer process alumina production.
[0028] As a preferred technical solution of the present invention, in step S53, the desorption liquid is one of sodium chloride solution, sodium nitrate solution and sodium sulfate solution, wherein the mass fraction of the desorption liquid is 20-50%.
[0029] As a preferred technical solution of the present invention, in step S56, the potassium salt product is one of potassium nitrate, potassium chloride and potassium sulfate, wherein the mass purity of the potassium salt is 96-99.9%.
[0030] Beneficial effects of the present invention:
[0031] (1) The present invention uses three inorganic salts, and the alkaline environment provided by the sodium hydroxide solution is used to improve the crystallinity of the complex salt. Potassium-containing aluminosilicate is obtained by calcination, and different proportions of potassium-containing aluminosilicate can be formed by adjusting different proportions of the three salts. After being combined with polysulfone with excellent corrosion resistance, a composite potassium adsorbent with a porous structure is obtained, which has a large specific surface area and strong adsorption. While retaining the active sites, the excellent alkali resistance and high temperature resistance of polysulfone are introduced, so that the solution environment of Bayer mother liquor can be met, and it can be used to adsorb potassium ions in a high alkaline solution; according to the thermodynamic equilibrium characteristics of ion exchange, the ion exchange selectivity is related to the hydration radius and ion concentration of the ion. When the potassium-containing aluminosilicate is in contact with potassium ions, due to the characteristics of ion exchange, the cations in the aluminosilicate will undergo a substitution reaction with the potassium ions, so that the cations in the aluminosilicate will be replaced by the potassium ions. This process is driven by the similarity between the potassium ions and the cations in the aluminosilicate in charge and radius, and the higher reactivity of the potassium ions. At room temperature, the hydration radius of potassium ions is 0.3nm, and the hydration radius of sodium ions is 0.4nm. The composite potassium adsorbent has a higher selectivity for potassium ions at room temperature and can achieve highly selective adsorption of potassium ions. At higher temperatures, the hydration radius of sodium ions decreases and is close to the hydration radius of potassium ions. At this time, high concentrations of sodium ions can be used to replace potassium ions in the adsorbent and elute the adsorbent.
[0032] (2) A composite potassium adsorbent is used to realize the recovery of potassium in the seed liquor of the Bayer process for producing alumina, which not only provides a new potassium source, but also improves the product quality of alumina, and has no interference with the existing alumina production. The composite potassium adsorbent is obtained by compounding the active double salt and polysulfone, and can realize efficient adsorption of potassium ions in the high-temperature and high-alkalinity Bayer mother liquor. The adsorbent prepared by the present invention is easy to prepare, the process is simple, and the extraction of potassium in the Bayer mother liquor can be realized. In addition, the adsorption process is simple, easy to be automatically controlled, and the production cost of potassium salt is low.
[0033] (3) In the present invention, the potassium adsorption process only requires the Bayer mother liquor to pass through the adsorption device. After adsorption, the next production link of alumina can be continued without heating and cooling operations, and there is no need to change the process parameters of the Bayer process for producing alumina. It has no effect on subsequent production conditions, and the equipment process is simple and effective.
[0034] (4) The process of extracting potassium from Bayer mother liquor of the present invention adopts nanofiltration membrane to carry out systematic impurity removal on the desorption liquid, has high interception rate for divalent and trivalent cations, is simple and efficient, and does not introduce external impurities in the whole process; after desorption, the composite potassium adsorbent is eluted with cleaning liquid, and its surface becomes alkaline adsorbent, which can be directly recycled and reused, and will not stimulate the decomposition of sodium aluminate molecules in Bayer mother liquor. The potassium concentration in the potassium-rich desorption liquid is high, and the solution composition is simple. Through evaporation, concentration and crystallization, high-purity potassium salt can be obtained, and the production cost is low. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] In order to facilitate understanding by those skilled in the art, the present invention is further described below with reference to the accompanying drawings.
[0036] Figure 1 This is a scanning electron microscope image of the active double salt prepared in Example 1;
[0037] Figure 2 This is a scanning electron microscope image of the composite potassium adsorbent prepared in Example 1;
[0038] Figure 3 This is the process flow chart for extracting potassium from Bayer mother liquor using a composite potassium adsorbent. DETAILED DESCRIPTION
[0039] In order to further explain the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the specific implementation methods, structures, features and effects of the present invention are described in detail below in conjunction with the accompanying drawings and preferred embodiments.
[0040] Example 1
[0041] Preparation of composite potassium adsorbent:
[0042] S11, adding aluminum sulfate, sodium silicate and potassium hydroxide in a molar ratio of 1:4:1 to a sodium hydroxide solution with a concentration of 0.5 mol / L, ultrasonically mixing for 2 hours, heating the solution to evaporate to a solid, and then calcining at 250° C. for 1 hour, and after the calcination, an active double salt is prepared;
[0043] S12, dissolving polysulfone molecules in N,N-dimethylacetamide to obtain a uniform polysulfone solution with a mass fraction of 10%, uniformly dispersing active double salt in the polysulfone solution, wherein the mass fraction of the active double salt is 20%, and then dropping the polysulfone solution mixed with the active double salt into deionized water, filtering to obtain solid particles wrapped with polysulfone;
[0044] S13, drying the polysulfone-wrapped solid particles in a vacuum drying oven at 80° C. for 10 h, sterilizing them with an ultraviolet light for 35 min, and then cooling them to 25° C. to prepare a composite potassium adsorbent.
[0045] according to Figure 2 The obtained scanning electron microscope image shows that the prepared composite potassium adsorbent has a porous structure.
[0046] Process of extracting potassium from Bayer mother liquor using composite potassium adsorbent:
[0047] S51, adsorption: passing the Bayer mother liquor into an adsorption tower loaded with the composite potassium adsorbent prepared in S13, the potassium ion concentration in the Bayer mother liquor is 32 g / L, and the adsorption is stopped when the potassium ion concentration in the effluent after adsorption is 8 g / L. The temperature of the Bayer mother liquor during adsorption is 35° C.;
[0048] S52, washing: passing a sodium hydroxide solution with a mass fraction of 1% as a cleaning liquid into the adsorption device after the adsorption is completed to clean the composite potassium adsorbent after step S51, and wash away the Bayer mother liquor and impurities adsorbed on the surface;
[0049] S53, desorption: heating a sodium nitrate solution with a mass fraction of 45% to 95° C., and then passing it into an adsorption device to desorb the composite potassium adsorbent after step S52, so that the potassium ions adsorbed in the composite potassium adsorbent are desorbed into the desorption liquid, and a potassium-enriched desorption liquid is obtained, wherein the potassium ion concentration is 38 g / L;
[0050] S54, washing: washing the composite potassium adsorbent after step S52 with a sodium hydroxide solution having a mass fraction of 1%, and the composite potassium adsorbent can be recycled after washing;
[0051] S55, filtration: using a polyamide nanofiltration membrane to remove impurities from the potassium-enriched desorption solution, removing calcium, magnesium, aluminum, and iron impurity ions, and the potassium ion concentration in the desorption solution after filtration is 35 g / L;
[0052] S56, purification: the potassium-rich liquid after impurities are removed is evaporated, concentrated, crystallized and heat-insulated to settle. The precipitated sodium nitrate is used for the preparation of the desorption liquid, and then cooled and crystallized to precipitate crude potassium nitrate. The potassium nitrate product is obtained after centrifugal separation, washing and purification with saturated potassium nitrate, drying and packaging.
[0053] After testing, the content of the components in the potassium nitrate prepared in this embodiment: potassium nitrate content is 99.8%, sodium nitrate content is 0.1%, which meets the requirements of industrial potassium nitrate.
[0054] Example 2
[0055] Preparation of composite potassium adsorbent:
[0056] S11, adding aluminum chloride, sodium silicate and potassium hydroxide in a molar ratio of 2:6:1 to a sodium hydroxide solution with a concentration of 0.9 mol / L, ultrasonically mixing for 2 hours, heating the solution to evaporate to a solid, and then calcining at 250° C. for 3 hours, and preparing an active double salt after calcination;
[0057] S12, dissolving polysulfone molecules in N,N-dimethylformamide to obtain a uniform polysulfone solution with a mass fraction of 30%, uniformly dispersing active double salt in the polysulfone solution, wherein the mass fraction of the active double salt is 30%, and then dropping the polysulfone solution mixed with the active double salt into deionized water, filtering to obtain solid particles wrapped with polysulfone;
[0058] S13, drying the polysulfone-wrapped solid particles in a vacuum drying oven at 90° C. for 12 h, sterilizing them with an ultraviolet light for 40 min, and then cooling them to 30° C. to prepare a composite potassium adsorbent.
[0059] Process of extracting potassium from Bayer mother liquor using composite potassium adsorbent:
[0060] S51, adsorption: passing the Bayer mother liquor into an adsorption tower loaded with the composite potassium adsorbent prepared in S13, the potassium ion concentration in the Bayer mother liquor is 55 g / L, and the adsorption is stopped when the potassium ion concentration in the effluent after adsorption is 10 g / L. The temperature of the Bayer mother liquor during adsorption is 45° C.;
[0061] S52, washing: passing a sodium hydroxide solution with a mass fraction of 1% as a cleaning liquid into the adsorption device after the adsorption is completed to clean the composite potassium adsorbent after step S51, and wash away the Bayer mother liquor and impurities adsorbed on the surface;
[0062] S53, desorption: heating a sodium chloride solution with a mass fraction of 28% to 95° C., and then passing it into an adsorption device to desorb the composite potassium adsorbent after step S52, so that the potassium ions adsorbed in the composite potassium adsorbent are desorbed into the desorption liquid, and a potassium-enriched desorption liquid is obtained, wherein the potassium ion concentration is 36 g / L;
[0063] S54, washing: using a sodium hydroxide solution with a mass fraction of 1% to wash the composite potassium adsorbent after step S53, and the composite potassium adsorbent can be recycled after washing;
[0064] S55, filtration: using a polyamide nanofiltration membrane to remove impurities from the potassium-enriched desorption solution, removing calcium, magnesium, aluminum, and iron impurity ions, and the potassium ion concentration in the desorption solution after filtration is 34 g / L;
[0065] S56, purification: the potassium-rich liquid after impurities are removed is evaporated, concentrated, crystallized and heat-insulated to obtain the corresponding potassium salt. The sodium chloride precipitated first is used for the preparation of the desorption liquid, and then cooled and crystallized to precipitate crude potassium chloride. The potassium chloride product is obtained after centrifugal separation, washing and purification with saturated potassium nitrate, drying and packaging.
[0066] After testing, the mass fraction of potassium chloride (K2O) prepared by the method described in this embodiment is 60%, and the mass fraction of sodium chloride is 1.4%, which meets the standard of potassium chloride for agricultural use.
[0067] Example 3
[0068] Preparation of composite potassium adsorbent:
[0069] S11, adding aluminum sulfate, sodium silicate and potassium chloride in a molar ratio of 2.6:10.4:1 to an alkaline solution with a concentration of 1 mol / L, ultrasonically mixing for 2 hours, heating the solution to evaporate to a solid, and then calcining at 350° C. for 1 hour, and after the calcination, an active double salt is prepared;
[0070] S12, dissolving polysulfone molecules in N-methylpyrrolidone to obtain a uniform polysulfone solution with a mass fraction of 40%, uniformly dispersing active double salt in the polysulfone solution, wherein the mass fraction of the active double salt is 60%, and then dropping the polysulfone solution mixed with the active double salt into deionized water, filtering to obtain polysulfone-coated solid particles;
[0071] S13, drying the polysulfone-wrapped solid particles in a vacuum drying oven at 100° C. for 16 h, sterilizing them with an ultraviolet light for 45 min, and then cooling them to 35° C. to prepare a composite potassium adsorbent.
[0072] Process of extracting potassium from Bayer mother liquor using composite potassium adsorbent:
[0073] S51, adsorption: passing the Bayer mother liquor into an adsorption tower loaded with the composite potassium adsorbent prepared in S13, the potassium ion concentration in the Bayer mother liquor is 55 g / L, and the adsorption is stopped when the potassium ion concentration in the effluent after adsorption is 10 g / L. The temperature of the Bayer mother liquor during adsorption is 45° C.;
[0074] S52, washing: passing a sodium hydroxide solution with a mass fraction of 2% as a cleaning liquid into the adsorption device after the adsorption is completed to clean the composite potassium adsorbent after step S51, and wash away the Bayer mother liquor and impurities adsorbed on the surface;
[0075] S53, desorption: heating a sodium chloride solution with a mass fraction of 20% to 95° C., and then passing it into an adsorption device to desorb the composite potassium adsorbent after step S52, so that the potassium ions adsorbed in the composite potassium adsorbent are desorbed into the desorption liquid, and a potassium-enriched desorption liquid is obtained, wherein the potassium ion concentration is 32 g / L;
[0076] S54, washing: using a sodium hydroxide solution with a mass fraction of 2% to wash the composite potassium adsorbent after step S53, and the composite potassium adsorbent can be recycled after washing;
[0077] S55, filtration: using a polyamide nanofiltration membrane to remove impurities from the potassium-enriched desorption solution, removing calcium, magnesium, aluminum, and iron impurity ions, and the potassium ion concentration in the desorption solution after filtration is 30 g / L;
[0078] S56, purification: The potassium-rich liquid after impurities are removed is evaporated, concentrated, crystallized and heat-insulated to settle. The precipitated sodium chloride is used for the preparation of the desorption liquid, and then cooled and crystallized to precipitate crude potassium chloride. The potassium chloride product is obtained after centrifugal separation, washing and purification with saturated potassium nitrate, drying and packaging.
[0079] After testing, the mass fraction of potassium chloride (K2O) prepared by the method described in this embodiment is 62%, and the mass fraction of sodium chloride is 2.4%, which meets the standard of potassium chloride for agricultural use.
[0080] Example 4
[0081] Preparation of composite potassium adsorbent:
[0082] S11, adding aluminum chloride, sodium silicate and potassium hydroxide in a molar ratio of 3:15:1 to a sodium hydroxide solution with a concentration of 0.8 mol / L, ultrasonically mixing for 2 hours, heating the solution to evaporate to a solid, and then calcining at 280° C. for 3 hours, and preparing an active double salt after the calcination is completed;
[0083] S12, dissolving polysulfone molecules in 1,4-dioxane to obtain a uniform polysulfone solution with a mass fraction of 40%, uniformly dispersing an active double salt in the polysulfone solution, wherein the mass fraction of the active double salt is 30%, and then dropping the polysulfone solution mixed with the active double salt into deionized water, and filtering to obtain solid particles wrapped with polysulfone;
[0084] S13, drying the polysulfone-wrapped solid particles in a vacuum drying oven at 80° C. for 12 h, sterilizing them with an ultraviolet light for 35 min, and then cooling them to 30° C. to prepare a composite potassium adsorbent.
[0085] Process of extracting potassium from Bayer mother liquor using composite potassium adsorbent:
[0086] S51, adsorption: passing the Bayer mother liquor into an adsorption tower loaded with the composite potassium adsorbent prepared in S13, the potassium ion concentration in the Bayer mother liquor is 48 g / L, and the adsorption is stopped when the potassium ion concentration in the effluent after adsorption is 4.8 g / L. The temperature of the Bayer mother liquor during adsorption is 20° C.;
[0087] S52, washing: passing a sodium hydroxide solution with a mass fraction of 0.1% as a washing liquid into the adsorption device after the adsorption is completed to wash the composite potassium adsorbent after step S51, and wash away the Bayer mother liquor and impurities attached to the surface of the composite potassium adsorbent;
[0088] S53, desorption: heating a sodium nitrate solution with a mass fraction of 45% to 100° C., and then passing it into an adsorption device to desorb the composite potassium adsorbent after step S52, so that the potassium ions adsorbed in the composite potassium adsorbent are desorbed into the desorption liquid, and a potassium-enriched desorption liquid is obtained, wherein the potassium ion concentration is 44 g / L;
[0089] S54, washing: using a sodium hydroxide solution with a mass fraction of 0.1% to wash the composite potassium adsorbent after step S53, and the composite potassium adsorbent can be recycled after washing;
[0090] S55, filtration: using a polyamide nanofiltration membrane to remove impurities from the potassium-enriched desorption solution, removing calcium, magnesium, aluminum, and iron impurity ions, and the potassium ion concentration in the desorption solution after filtration is 42 g / L;
[0091] S56, purification: the potassium-rich liquid after impurities are removed is evaporated, concentrated, crystallized and heat-insulated to settle. The precipitated sodium nitrate is used for the preparation of the desorption liquid, and then cooled and crystallized to precipitate crude potassium nitrate. The potassium nitrate product is obtained after centrifugal separation, washing and purification with saturated potassium nitrate, drying and packaging.
[0092] After testing, the potassium nitrate prepared by the method described in this embodiment has a potassium nitrate content of 99.0% and a sodium nitrate content of 0.5%, which meets the requirements of industrial potassium nitrate.
[0093] Example 5
[0094] Preparation of composite potassium adsorbent:
[0095] S11, adding aluminum chloride, sodium silicate and potassium sulfate in a molar ratio of 3:15:1 to an alkaline solution with a concentration of 1 mol / L, ultrasonically mixing for 2 hours, heating the solution to evaporate to a solid, and then calcining at 280° C. for 4 hours, and preparing an active double salt after the calcination is completed;
[0096] S12, dissolving polysulfone molecules in 1,4-dioxane to obtain a uniform polysulfone solution with a mass fraction of 40%, uniformly dispersing an active double salt in the polysulfone solution, wherein the mass fraction of the active double salt is 30%, and then dropping the polysulfone solution mixed with the active double salt into deionized water, and filtering to obtain solid particles wrapped with polysulfone;
[0097] S13, drying the polysulfone-wrapped solid particles in a vacuum drying oven at 100° C. for 10 h, sterilizing them with an ultraviolet light for 35 min, and then cooling them to 30° C. to prepare a composite potassium adsorbent.
[0098] Process of extracting potassium from Bayer mother liquor using composite potassium adsorbent:
[0099] S51, adsorption: passing the Bayer mother liquor into an adsorption tower loaded with the composite potassium adsorbent prepared by S134, the potassium ion concentration in the Bayer mother liquor is 66 g / L, and the adsorption is stopped when the potassium ion concentration in the effluent after adsorption is 15 g / L. The temperature of the Bayer mother liquor during adsorption is 40° C.;
[0100] S52, washing: passing a sodium hydroxide solution with a mass fraction of 1% as a washing liquid into the adsorption device after the adsorption is completed to wash the composite potassium adsorbent after step S51, and wash away the Bayer mother liquor and impurities attached to the surface of the composite potassium adsorbent;
[0101] S53, desorption: heating a sodium sulfate solution with a mass fraction of 30% to 90° C., and then passing it into an adsorption device to desorb the composite potassium adsorbent after step S52, so that the potassium ions adsorbed in the composite potassium adsorbent are desorbed into the desorption liquid, and a potassium-enriched desorption liquid is obtained, wherein the potassium ion concentration is 48 g / L;
[0102] S54, washing: washing the composite potassium adsorbent after step S53 with deionized water, and the composite potassium adsorbent can be recycled after washing;
[0103] S55, filtration: using a polypiperazineamide nanofiltration membrane to remove impurities from the potassium-enriched desorption solution, removing calcium, magnesium, aluminum, and iron impurity ions, and the potassium ion concentration in the desorption solution after filtration is 45 g / L;
[0104] S56, purification: the potassium-rich liquid after impurities removal is evaporated, concentrated, crystallized and heat-insulated to settle. The sodium sulfate precipitated first is used for the preparation of the desorption liquid, and then cooled and crystallized to precipitate crude potassium sulfate. The potassium sulfate product is obtained after centrifugal separation, saturated potassium sulfate washing and purification, drying and packaging.
[0105] After testing, the mass fraction of water-soluble potassium oxide (K2O) of potassium sulfate prepared by the method described in this embodiment is 53%, and the mass fraction of chloride ions is 0.2%, which meets the standard of potassium sulfate for agricultural use.
[0106] Example 6
[0107] Preparation of composite potassium adsorbent:
[0108] S11, adding aluminum sulfate, sodium silicate and potassium hydroxide in a molar ratio of 1:4:1 to a sodium hydroxide solution with a concentration of 0.5 mol / L, ultrasonically mixing for 2 hours, heating the solution to evaporate to a solid, and then calcining at 250° C. for 1 hour, and after the calcination, an active double salt is prepared;
[0109] S12, dissolving polysulfone molecules in N,N-dimethylacetamide to obtain a uniform polysulfone solution with a mass fraction of 10%, uniformly dispersing active double salt in the polysulfone solution, wherein the mass fraction of the active double salt is 20%, and then dropping the polysulfone solution mixed with the active double salt into deionized water, filtering to obtain solid particles wrapped with polysulfone;
[0110] S13, drying the polysulfone-wrapped solid particles in a vacuum drying oven at 80° C. for 10 h, sterilizing them with an ultraviolet light for 35 min, and then cooling them to 25° C. to prepare a composite potassium adsorbent.
[0111] Process of extracting potassium from Bayer mother liquor using composite potassium adsorbent:
[0112] S51, adsorption: passing the Bayer mother liquor into an adsorption tower loaded with the composite potassium adsorbent prepared in S13, the potassium ion concentration in the Bayer mother liquor is 66 g / L, and the adsorption is stopped when the potassium ion concentration in the effluent after adsorption is 33 g / L. The temperature of the Bayer mother liquor during adsorption is 60° C.;
[0113] S52, washing: passing deionized water as a washing liquid into the adsorption device after the adsorption is completed to wash the composite potassium adsorbent after step S51, and wash away the Bayer mother liquor and impurities adsorbed on the surface;
[0114] S53, desorption: heating a sodium nitrate solution with a mass fraction of 50% to 90° C., and then passing it into an adsorption device to desorb the composite potassium adsorbent after step S52, so that the potassium ions adsorbed in the composite potassium adsorbent are desorbed into the desorption liquid, and a potassium-enriched desorption liquid is obtained, wherein the potassium ion concentration is 50 g / L;
[0115] S54, washing: using a sodium hydroxide solution with a mass fraction of 1% to wash the composite potassium adsorbent after step S53, and the composite potassium adsorbent can be recycled after washing;
[0116] S55, filtration: using a polypiperazineamide nanofiltration membrane to remove impurities from the potassium-enriched desorption solution, removing calcium, magnesium, aluminum, and iron impurity ions, and the potassium ion concentration in the desorption solution after filtration is 45 g / L;
[0117] S56, purification: the potassium-rich liquid after impurities are removed is evaporated, concentrated, crystallized and heat-insulated to settle. The precipitated sodium nitrate is used for the preparation of the desorption liquid, and then cooled and crystallized to precipitate crude potassium nitrate. The potassium nitrate product is obtained after centrifugal separation, washing and purification with saturated potassium nitrate, drying and packaging.
[0118] After testing, the potassium nitrate prepared by the method described in this embodiment has a content of 99.5% and sodium nitrate of 0.2%, which meets the requirements of industrial potassium nitrate.
[0119] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technical personnel in this field can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any brief modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.
Claims
1. A process for extracting potassium from Bayer mother liquor using a composite potassium adsorbent, characterized in that: The following steps are involved: S51, adsorption: passing the Bayer mother liquor into an adsorption device loaded with a composite potassium adsorbent, and stopping the adsorption when the potassium ion concentration in the effluent after adsorption is close to 10-50% of the potassium ion concentration in the feed solution. The temperature of the Bayer mother liquor during adsorption is 20-60° C.; S52, washing: passing deionized water or a sodium hydroxide solution with a mass fraction of 0.1-2% as a cleaning liquid into the adsorption device after the adsorption is completed to clean the composite potassium adsorbent after step S51, and wash away the Bayer mother liquor and impurities adsorbed on the surface; S53, desorption: at 60-100° C., passing the prepared desorption liquid into the adsorption device to desorb the composite potassium adsorbent after step S52, so that the potassium ions adsorbed in the composite potassium adsorbent are desorbed into the desorption liquid to obtain a potassium-enriched desorption liquid; S54, washing: using deionized water or a sodium hydroxide solution with a mass fraction of 0.1-2% to wash the composite potassium adsorbent after step S53, and the composite potassium adsorbent can be recycled after washing; S55, filtering: removing impurities from the potassium-enriched desorption liquid by using a nanofiltration membrane to remove calcium, magnesium, aluminum, and iron impurity ions, wherein the nanofiltration membrane is a polyamide nanofiltration membrane or a polypiperazineamide nanofiltration membrane; S56, purification: the potassium-rich liquid after impurities are removed is evaporated, concentrated, crystallized and heat-insulated to settle. The sodium salt precipitated first is used for the preparation of the desorption liquid, and then cooled and crystallized to precipitate the potassium salt. The potassium salt product is obtained after centrifugal separation, saturated potassium salt washing and purification, drying and packaging.
2. The process for extracting potassium from Bayer mother liquor using a composite potassium adsorbent according to claim 1, characterized in that: In step S51, the Bayer mother liquor is one of the seed mother liquor, the circulating mother liquor, the evaporated mother liquor and the gallium-extracted mother liquor after gallium extraction, and contains potassium ions at a concentration of 10 to 100 g / L.
3. The process for extracting potassium from Bayer mother liquor using a composite potassium adsorbent according to claim 1, characterized in that: In step S51, the adsorption device is one of an adsorption tower, an adsorption column and an adsorption tank.
4. The process for extracting potassium from Bayer mother liquor using a composite potassium adsorbent according to claim 1, characterized in that: In step S51, the Bayer mother liquor after adsorption can be directly used in the next step of Bayer process alumina production.
5. The process for extracting potassium from Bayer mother liquor using a composite potassium adsorbent according to claim 1, characterized in that: In step S53, the desorption liquid is one of sodium chloride solution, sodium nitrate solution and sodium sulfate solution, wherein the mass fraction of the desorption liquid is 20-50%.
6. The process for extracting potassium from Bayer mother liquor using a composite potassium adsorbent according to claim 1, characterized in that: In step S56, the potassium salt product is one of potassium nitrate, potassium chloride and potassium sulfate, wherein the mass purity of the potassium salt is 96-99.9%.
Citation Information
Patent Citations
Preparation method of granular titanium-based lithium ion sieve adsorbent with high adsorption capacity
CN114345291A
Adsorbent for adsorbing lithium from refined liquid of aluminum oxide produced by Bayer process and use method of adsorbent for adsorbing lithium from refined liquid of aluminum oxide produced by Bayer process
CN116440873A
Device for removing impurity potassium in Bayer process circulating mother liquor
CN211338829U
Adsorbent and method for producing the same
JP2014180602A
Method of reducing impurity content in aqueous salt solution
US20070029259A1