Preparation method of yak manure-based material and application of yak manure-based material in selective adsorption of heavy metals
By modifying and pyrolysis, large-particle adsorbents suitable for acidic conditions were prepared, which solved the problem of poor selectivity and permeability of traditional adsorbents in acidic groundwater, and realized the composite heavy metals in acidic groundwater in mines efficient removal.
Patent Information
- Application Number
- CN202411193148.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-28
AI Technical Summary
Traditional groundwater treatment adsorbent materials have poor selectivity, poor long-term effectiveness and are prone to blockage under acidic conditions, making it difficult to effectively remove composite heavy metal pollution in acidic groundwater in mines.
By modifying and pyrolyzing the yak dung particles in large particles, a yak dung-based material with selective adsorption ability and good permeability was prepared, and solid-liquid reaction was used to carry out constant temperature water bath and oxygen-liquid heat-limiting To form an adsorbent suitable for acidic conditions.
It realizes efficient adsorption of characteristic heavy metals copper, lead, cadmium and iron, and the removal rate of coexisting magnesium ions, sulfate and silicates is less than 5%, and the permeability coefficient is greater than 10-3cm/s, breaking through the traditional biomass base Technical bottleneck of adsorbent materials, suitable for the treatment of composite heavy metal pollution in acidic groundwater in mines.
Smart Images

Figure BDA0005015635490000061
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of environmental protection, and discloses a method for preparing a yak dung-based material and an application of the material in selectively adsorbing heavy metals. Background Art
[0002] A large amount of wastewater will be generated during the development of mineral resources. These wastewaters contain acids, alkalis, suspended solids, heavy metal ions and various residual flotation agents, which will cause serious pollution to the mines and their surrounding soil and groundwater environment. At present, the treatment measures for acidic groundwater in non-ferrous metal mines mainly include source control technology and end-of-pipe treatment technology. Since source control technology is restricted by many factors in the process of preventing the generation of acidic groundwater, it is difficult to effectively curb the generation and pollution of acidic groundwater. Therefore, end-of-pipe treatment of acidic groundwater is a necessary link to prevent it from polluting the surrounding environment of the mining area. Traditional groundwater treatment adsorption materials have poor selectivity and small particle size (about 200 mesh). The poor selectivity causes the adsorption material to be saturated prematurely, resulting in poor long-term effectiveness. The small particle size leads to poor permeability of the adsorption material. Therefore, it is necessary to develop new groundwater adsorption materials to solve the above-mentioned problems.
[0003] Compared with mineral adsorption materials, biomass-based materials have the advantages of large specific surface area, rich pores and surface adsorption sites, and have been widely used in the treatment of heavy metal-containing wastewater. However, the biomass-based adsorption materials that have been reported are prone to adsorbing magnesium ions, sulfates and silicates that coexist in acidic groundwater in mines, occupying the adsorption active sites of the materials, resulting in poor long-term effectiveness of the adsorption materials. At the same time, due to the extremely fine particle size, the adsorption filling body has poor permeability and is easy to clog. Therefore, it is necessary to develop new large-particle biomass-based adsorption materials suitable for selective adsorption of characteristic heavy metals under acidic conditions, so as to achieve efficient removal of complex heavy metal pollution in acidic groundwater in mines. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide a method for preparing a large-particle yak dung-based material suitable for selective removal of composite heavy metal pollution in acidic groundwater in mines. The method controls the particle size of yak dung to be large particles, performs modification and pyrolysis under large-particle conditions, and realizes the selective adsorption of characteristic heavy metal copper, lead, cadmium, and iron ions in the acidic groundwater system with high sulfate, magnesium ions, and silicate ions. The material has good permeability, that is, the adsorption material only efficiently adsorbs characteristic heavy metal copper, lead, cadmium, and iron ions, while the removal rate of coexisting magnesium ions, sulfate ions, and silicate ions is less than 5%, and the permeability coefficient is greater than 10 -3 cm / s, breaking through the technical bottleneck of poor adsorption selectivity and permeability of traditional biomass-based adsorption materials for characteristic heavy metals in acidic mine groundwater.
[0005] To this end, the first technical solution of the present application discloses a method for preparing a yak dung-based material, comprising the following steps:
[0006] S1. Add yak dung pellets to Fe 3+ and Mn 7+ In the mixed solution, a solid-liquid reaction system is dispersed;
[0007] S2. The solid-liquid reaction system is dried in a constant temperature water bath to obtain a preliminary material;
[0008] S3. The preliminary material is subjected to oxygen-limited pyrolysis to obtain yak dung-based material.
[0009] Furthermore, the yak dung particles in S1 are obtained by crushing yak dung, and the particle size of the crushed yak dung particles is 30-60 meshes.
[0010] Further, S1 said Fe 3+ The concentration is 0.025mol / L, Mn 7+ The concentration is 0.050-0.075 mol / L, Fe 3+ and Mn 7+ The concentration ratio is 1:(2-3)(n:n).
[0011] Furthermore, the yak dung particles described in S1 and Fe 3+ and Mn 7+ The solid-liquid ratio of the mixed solution is (150-175):1000 (m / v).
[0012] Further, the dispersion in S1 is specifically to mix yak dung particles with Fe 3+ and Mn 7+ After the mixed solution is mixed, it is first stirred at a low speed and then ultrasonically dispersed. The low-speed stirring speed is 200-250 rpm, the stirring time is 60-90 minutes, and the ultrasonic dispersion time is 90-120 minutes.
[0013] Furthermore, the constant temperature water bath temperature in S2 is 90-95° C., and the time is 90-120 min.
[0014] Furthermore, the oxygen-limited pyrolysis in S3 is: heating to 400-450°C at a heating rate of 10°C / min, introducing nitrogen, and performing oxygen-limited pyrolysis under anaerobic conditions.
[0015] And, the yak dung-based material prepared according to the above preparation method.
[0016] The second technical solution of the present application discloses the application of the above-mentioned yak dung-based material as an adsorbent for selectively adsorbing complex heavy metals in mine groundwater.
[0017] Preferably, the mine groundwater is acidic groundwater, containing high concentrations of sulfate, magnesium ions and silicate, and the complex heavy metals include copper ions, cadmium ions, lead ions and iron ions.
[0018] The beneficial effects of the present invention are as follows:
[0019] The present invention uses yak dung, a common agricultural and animal husbandry waste in the high-cold climate zone of Tibet, as raw material, and FeCl 3 and KMnO 4 The modified mixture is pyrolyzed under oxygen-limited conditions to obtain an acidic groundwater treatment adsorption material with selective adsorption capacity and good permeability, and the process is simple. The acidic groundwater treatment selective adsorption material obtained by the preparation method of the present invention can effectively adsorb cadmium, iron, lead, and copper ions, while the removal rate of magnesium ions, sulfate and silicate is less than 5%, and the permeability coefficient is greater than 10 -3 cm / s, which is particularly suitable for the treatment of complex heavy metal pollution in acidic groundwater in mines, and has excellent pollution removal performance and economic applicability. DETAILED DESCRIPTION
[0020] The present invention is further described in detail below in conjunction with specific examples. This implementation case is implemented based on the technology of the present invention, and a detailed implementation method and specific operation process are now given to illustrate that the present invention is creative, but the protection scope of the present invention is not limited to the following examples.
[0021] Unless otherwise specified, the experimental methods used in the following examples are conventional methods.
[0022] Unless otherwise specified, the materials and reagents used in the following examples can be obtained from commercial sources.
[0023] The embodiment of the present application discloses a method for preparing a yak dung-based material, comprising the following steps:
[0024] S1. Adding Fe to yak dung pellets 3+ and Mn 7+ In the mixed solution, a solid-liquid reaction system is dispersed;
[0025] S2. The solid-liquid reaction system is dried in a constant temperature water bath to obtain a preliminary material;
[0026] S3. After the preliminary material is subjected to a first pyrolysis, the temperature is raised and oxygen-limited pyrolysis is performed to obtain a yak dung-based material.
[0027] It can be understood that the yak dung particles are obtained by crushing yak dung. The yak dung in the present application is taken from Tibet, which is an agricultural and animal husbandry waste in a high-cold climate. It is crushed to a particle size of 30-60 mesh.
[0028] In this embodiment, the crushed yak dung particles are added to the Fe 3+ and Mn 7+ FeCl 3 and KMnO 4 The purpose of the mixed solution is to modify the yak dung and adjust the surface potential of the yak dung particles by changing the valence state of the variable metal iron and manganese elements, so as to adapt to the selective adsorption of heavy metal pollution in complex environments and improve the adsorption capacity. However, yak dung particles without surface potential adjustment are difficult to adapt to the selective removal of heavy metals in complex systems and have a small adsorption capacity. In a specific embodiment, the Fe 3+ and Mn 7+ The mixed solution can be 3+ and Mn 7+ salt, such as FeCl 3 and KMnO 4。
[0029] In a specific embodiment, the Fe 3+ The concentration is 0.025mol / L, Mn 7+ The concentration is 0.050-0.075 mol / L, Fe 3+ and Mn 7+ The concentration ratio is 1:(2-3)(n:n); the yak dung particles and Fe 3+ and Mn 7+ The solid-liquid ratio of the mixed solution is (150-175):1000 (m / v); the dispersion is specifically to mix the yak dung particles with Fe 3+ and Mn 7+ After the mixed solution is mixed, it is first stirred at a low speed and then ultrasonically dispersed. The low-speed stirring speed is 200-250 rpm, the stirring time is 60-90 minutes, and the ultrasonic dispersion time is 90-120 minutes.
[0030] In this embodiment, the modified yak dung solid-liquid reaction system is subjected to a constant temperature water bath treatment. The purpose of this step is to make Fe 3+ and Mn 7+ Fully react with yak dung particles to achieve uniform attachment of iron and manganese elements to the surface of yak dung particles.
[0031] In a specific embodiment, the temperature of the constant temperature water bath is 90-95°C, and the time is 90-120 min. It is understandable that the material needs to be dried after the reaction, and the drying temperature is preferably 80°C.
[0032] In this embodiment, the preliminary material after the constant temperature water bath treatment is subjected to oxygen-limited treatment. The purpose of this step is to convert the cellulose and hemicellulose components inside the yak dung particles into active groups with selective heavy metal adsorption properties, so as to increase the selective adsorption performance of yak dung-based materials for heavy metals in complex systems.
[0033] Furthermore, the oxygen-limited pyrolysis in S3 is: heating to 400-450°C at a heating rate of 10°C / min, introducing nitrogen, and performing oxygen-limited pyrolysis under anaerobic conditions.
[0034] In this embodiment, the heating rate is 10°C / min. The purpose of this step is that the heating rate of 10°C / min can gradually pyrolyze cellulose and hemicellulose into biochar-based materials; the oxygen-limited pyrolysis temperature is 400-450°C. The purpose of this step is to maximize the pyrolysis of cellulose and hemicellulose under this temperature condition, and then produce the maximum yield of yak dung-based materials.
[0035] The second embodiment of the present application discloses the use of the yak dung-based material prepared by the above preparation method as an adsorbent for selectively complexing heavy metals in mine groundwater.
[0036] It should be noted that mine groundwater is wastewater generated during the development of mineral resources. These wastewaters contain acids, alkalis, suspended solids, heavy metal ions and various residual flotation agents, etc., and are generally acidic. The biomass-based adsorbents reported in the prior art not only adsorb heavy metal ions, but also easily adsorb magnesium ions, sulfate ions, silicate ions, etc. coexisting in groundwater, which will occupy the active sites of the material, resulting in poor long-term effectiveness of the adsorption material.
[0037] The yak-based material prepared by the above preparation method in the present application can selectively adsorb heavy metal ions, including but not limited to copper ions, cadmium ions, lead ions, iron ions, etc., when used as an adsorbent to adsorb heavy metal ions in mine groundwater in the presence of magnesium ions, sulfate ions, silicate ions, etc., while the removal rate of magnesium ions, sulfate ions and silicate ions is less than 5%, and the permeability coefficient is greater than 10 -3 cm / s, so it is particularly suitable for the treatment of complex heavy metal pollution in acidic groundwater in copper mines, and has excellent pollution removal performance and economic applicability.
[0038] In order to make the technical problems to be solved, technical solutions and advantages of the present invention more clear, they are described in detail below in conjunction with specific embodiments.
[0039] The following examples contain Fe 3+ The solution was prepared by adding FeCl 3 Get, containing Mn 7+ The solution was prepared by adding KMnO 4It was determined through preliminary experimental studies that FeCl 3 The concentration is 0.025 mol / L, KMnO 4 The concentration of 0.075 mol / L is the optimal modification concentration, so the embodiment is described in detail by changing the solid-liquid ratio of yak dung particles and the modified solution.
[0040] Example 1 Preparation of yak dung-based materials
[0041] S1. Add 6.76 g FeCl 3 6H 2 O and 11.85g KMnO 4 Place in a beaker and add 1000 mL of water to prepare FeCl 3 6H 2 O and KMnO 4 Mixed solution. Add 165 g of yak dung particles (30-60 mesh) to the aforementioned 1000 mL mixed solution, stir at 200 rpm for 60 minutes at room temperature (25°C), and then put it into an ultrasonic cleaner (25°C) for ultrasonic dispersion for 120 minutes to obtain a solid-liquid reaction system.
[0042] S2. The solid-liquid reaction system was placed in a water bath and heated at a constant temperature (95°C) for 2 hours, then filtered and dried at 80°C to obtain a preliminary material.
[0043] S3. The preliminary material was pyrolyzed in a tubular furnace, heated to 450°C at a heating rate of 10°C / min, nitrogen was introduced, and oxygen-limited pyrolysis was carried out under anaerobic conditions for 2 hours. After closed and natural cooling, yak dung-based materials were obtained.
[0044] Example 2 Preparation of yak dung-based materials
[0045] S1. Add 6.76 g FeCl 3 6H 2 O and 11.85g KMnO 4 Place in a beaker and add 1000 mL of water to prepare FeCl 3 and KMnO 4 Mixed solution. Add 175 g of yak dung particles (30-60 mesh) to the aforementioned 1000 mL mixed solution, stir at 200 rpm for 60 minutes at room temperature (25°C), and then put it into an ultrasonic cleaner (25°C) for ultrasonic dispersion for 90 minutes to obtain a solid-liquid reaction system.
[0046] S2. The solid-liquid reaction system was placed in a water bath and heated at a constant temperature (90°C) for 1.5 hours, then filtered and dried at 80°C to obtain a preliminary material.
[0047] S3. The preliminary material was pyrolyzed in a tube furnace and heated to 400°C at a heating rate of 10°C / min under oxygen-limited conditions for 2 hours. After closed and naturally cooled, the yak dung-based material was obtained.
[0048] Example 3 Preparation of yak dung-based materials
[0049] S1. Add 6.76 g FeCl 3 6H 2 O and 11.85g KMnO 4 Place in a beaker and add 1000 mL of water to prepare FeCl 3 6H 2 O and KMnO 4 Mixed solution. Add 150 g of yak dung particles (30-60 mesh) to the aforementioned 1000 mL mixed solution, stir at 200 rpm for 60 minutes at room temperature (25°C), and then put it into an ultrasonic cleaner (25°C) for ultrasonic dispersion for 120 minutes to obtain a solid-liquid reaction system.
[0050] S2. The solid-liquid reaction system was placed in a water bath and heated at a constant temperature (92°C) for 2 hours, then filtered and dried at 80°C to obtain a preliminary material.
[0051] S3. The preliminary material was pyrolyzed in a tubular furnace, heated to 420°C at a heating rate of 10°C / min, nitrogen was introduced, and oxygen-limited pyrolysis was carried out under anaerobic conditions for 2 hours. After closed and natural cooling, yak dung-based materials were obtained.
[0052] Comparative Example 1 Preparation of yak dung-based materials
[0053] The preparation method is the same as that in Example 1, the difference is that water is used instead of FeCl 3 6H 2 O and KMnO 4 The mixed solution is dispersed.
[0054] Comparative Example 2 Preparation of yak dung-based materials
[0055] The preparation method is the same as that of Example 1, except that the constant temperature water bath treatment described in S2 is not performed in Comparative Example 2.
[0056] Comparative Example 3 Preparation of yak dung-based materials
[0057] The preparation method is the same as that of Example 1, except that, in Comparative Example 3, the oxygen-limited pyrolysis reaction described in S3 is not performed.
[0058] Test Example 1 Selective adsorption experiment of yak dung-based materials
[0059] Experimental method: Weigh 0.8g of the yak dung-based material prepared in Examples 1-3 and Comparative Examples 1-3 into a 1000mL beaker, add 800mL of a mixed solution with a pH of 5.0, a copper ion concentration of 2mg / L, a cadmium ion concentration of 0.02mg / L, a lead ion concentration of 0.40mg / L, a magnesium ion concentration of 10mg / L, a sulfate ion concentration of 1000mg / L, and a silicate ion concentration of 25mg / L, and rapidly adsorb for 2.0 hours at room temperature, then filter and use ICP-OES to test the heavy metal concentration in the filtrate.
[0060] Experimental results: See Table 1.
[0061] Table 1 Results of selective adsorption experiments on yak dung-based materials
[0062]
[0063] Results analysis: From Table 1, it can be seen that the adsorption rate of the yak dung-based materials prepared in Examples 1-3 for heavy metal copper ions is as high as 87.9%, the adsorption rate for cadmium ions is as high as 88.3%, and the adsorption rate for lead ions is as high as 99.4%, while the adsorption capacity for magnesium ions, sulfate and silicate is relatively weak, all below 5%. At the same time, the permeability coefficient of the prepared yak dung material is 0.007 cm / s, while the permeability coefficient of the main water-bearing rock formation in the mine is generally 7.64×10 -7 cm / s. This indicates that the material prepared by the present application has strong adsorption selectivity and good permeability, thereby extending the service life of the material (improving long-term effectiveness), and solving the problem of clogging of the reported biomass-based adsorption materials due to extremely fine particle size, which is conducive to industrial application. The method of the present invention achieves the purpose of preparing selective large-particle adsorption materials for acidic groundwater treatment by controlling the particle size, modification conditions and oxygen-limited roasting conditions of yak dung.
[0064] Comparative Examples 1-3 show that only the yak dung-based materials prepared under the modification conditions, constant temperature water bath and oxygen-limited roasting conditions specified in this application can achieve the purpose of preparing selective large-particle adsorption materials for acidic groundwater treatment.
[0065] The above is a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing yak dung-based materials, characterized in that: The steps include: S1. Add yak dung pellets to Fe 3+ and Mn 7+ A solid-liquid reaction system is dispersed in a mixed solution; S2. The solid-liquid reaction system is dried in a constant temperature water bath to obtain a preliminary material; S3. The preliminary material is subjected to oxygen-limited pyrolysis to obtain yak dung-based material.
2. The preparation method according to claim 1, characterized in that: S1 The yak dung particles are obtained by crushing yak dung, and the particle size of the crushed yak dung particles is 30-60 meshes.
3. The preparation method according to claim 1, characterized in that: S1Fe 3+ The concentration is 0.025mol / L, Mn 7+ The concentration is 0.050-0.075 mol / L, Fe 3+ and Mn 7+ The concentration ratio is 1:(2-3)(n:n).
4. The preparation method according to claim 1, characterized in that: S1 Yak dung pellets and Fe 3+ and Mn 7+ The solid-liquid ratio of the mixed solution is (150-175):1000 (m / v).
5. The preparation method according to claim 1, characterized in that: S1 The dispersion is specifically to mix yak dung particles with Fe 3+ and Mn 7+ After the mixed solution is mixed, it is first stirred at a low speed and then ultrasonically dispersed. The low-speed stirring speed is 200-250 rpm, the stirring time is 60-90 minutes, and the ultrasonic dispersion time is 90-120 minutes.
6. The preparation method according to claim 1, characterized in that: The constant temperature water bath temperature in S2 is 90-95°C and the time is 90-120min.
7. The preparation method according to claim 1, characterized in that: The oxygen-limited pyrolysis in S3 is as follows: heating the temperature to 400-450°C at a heating rate of 10°C / min, then introducing nitrogen, and performing oxygen-limited pyrolysis under anaerobic conditions.
8. A yak dung-based material prepared according to any one of the preparation methods of claims 1-7.
9. Use of the yak dung-based material according to claim 8 as an adsorbent for selectively adsorbing complex heavy metals in mine groundwater.
10. The use according to claim 9, characterized in that: The mine groundwater is acidic groundwater, containing high concentrations of sulfate, magnesium ions and silicate, and the complex heavy metals include copper ions, cadmium ions and lead ions.
Citation Information
Patent Citations
Preparation method and application of cow dung biological carbon
CN105921110A
Method for synchronously adsorbing arsenic and fluorine in water with iron-loaded yak dung biochar
CN108821377A
Sheep manure biochar and application thereof in heavy metal adsorption
CN112547006A
Preparation method and application of heavy metal biochar for repairing plateau tailings