Adsorbing material as well as preparation method and application thereof

By loading a eutectic solvent onto activated carbon, the problem of poor adsorption performance of conventional activated carbon for C2 and C3 light hydrocarbons is solved, achieving efficient and safe VOCs recovery.

CN118925673APending Publication Date: 2024-11-12CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310529823.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-11
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing conventional activated carbon materials have poor adsorption performance for C2 and C3 light hydrocarbons and are prone to safety risks, especially when the temperature rises during the adsorption process.

Method used

Activated carbon material loaded with a eutectic solvent, consisting of hydrogen bond acceptors and hydrogen bond donors, is prepared by ultrasonication and drying processes to improve the adsorption performance of C2-C3 light hydrocarbons.

Benefits of technology

It improves the adsorption performance for C2-C3 light hydrocarbons, reduces the safety risks of the adsorption process, and has low material cost, simple operation, and high VOCs recovery efficiency and safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004224198500000181
    Figure BDA0004224198500000181
Patent Text Reader

Abstract

The invention relates to the field of oil gas recovery and discloses an adsorption material as well as a preparation method and application thereof. The adsorption material comprises activated carbon and a eutectic solvent loaded on the activated carbon, the eutectic solvent contains at least one pair of hydrogen bond acceptor-hydrogen bond donor; the hydrogen bond acceptor is selected from one or more than two of tetrabutylammonium bromide, tetraoctyl ammonium chloride, menthol and thymol; the hydrogen bond donor is organic acid; in the eutectic solvent, the ratio of the amount of substance of the hydrogen bond acceptor to the amount of substance of the hydrogen bond donor is 1: (1-5). The adsorption material has excellent adsorption performance on C2-C3 light hydrocarbons. And the device has the characteristics of low cost and easiness in operation and maintenance, and has dual significance of improving the VOCs recovery efficiency and the process safety.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of oil and gas recovery, and in particular to an adsorption material and a preparation method and application thereof. Background Art

[0002] At present, the deep treatment of volatile organic compounds (VOCs) is still the main task of atmospheric environmental protection in my country. The oil and gas produced during the processing, storage and transportation of oil and gas in the petrochemical industry contains a large amount of VOCs. As a key industry for VOCs treatment, the VOCs treatment technologies currently used by oil storage depots and refining companies mainly include destruction and recovery methods.

[0003] The destruction method uses incineration or catalytic oxidation to decompose VOCs into small molecules such as water and carbon dioxide, which will produce greenhouse gases and is not in line with the concept of carbon emission reduction. In addition, the high-temperature operating environment of the destruction method increases the risk of safety accidents. Oil and gas recovery methods mainly include condensation, adsorption, absorption and membrane separation processes. At present, petrochemical companies generally use a combination of multiple recovery methods, such as condensation-adsorption, adsorption-absorption, etc. Among them, the adsorption method is based on the selective interaction between the adsorbent surface with a porous structure and the gas molecules to achieve gas separation.

[0004] Activated carbon is a commonly used adsorbent due to its low cost, rich pore structure and large specific surface area. However, conventional activated carbon has a weak adsorption capacity for light hydrocarbons, especially C2 and C3 components in oil and gas; in addition, the interaction between activated carbon and hydrocarbon substances has a significant thermal effect, so the temperature of the adsorption process increases, which may cause safety risks and accidents. Summary of the invention

[0005] The purpose of the present invention is to overcome the problems of poor adsorption performance of conventional activated carbon materials for C2 and C3 light hydrocarbons and easy temperature rise in the prior art, and to provide an adsorption material and a preparation method and application thereof.

[0006] In order to achieve the above object, the present invention provides an adsorption material on one hand, the adsorption material comprising: activated carbon and a deep eutectic solvent supported on the activated carbon;

[0007] Wherein, the deep eutectic solvent contains at least one pair of hydrogen bond acceptor-hydrogen bond donor;

[0008] The hydrogen bond acceptor is selected from one or more of tetrabutylammonium bromide, tetraoctylammonium chloride, menthol and thymol; the hydrogen bond donor is an organic acid;

[0009] In the deep eutectic solvent, the ratio of the amount of the hydrogen bond acceptor substance to the amount of the hydrogen bond donor substance is 1:1-5.

[0010] Preferably, the organic acid is selected from levulinic acid and / or C6-C18 fatty acids;

[0011] Preferably, the C6-C18 fatty acid is selected from one or more of n-hexanoic acid, oleic acid, n-decanoic acid and n-octanoic acid.

[0012] Preferably, when the low eutectic solvent contains tetrabutylammonium bromide-oleic acid, the molar ratio of tetrabutylammonium bromide to oleic acid in the tetrabutylammonium bromide-oleic acid is 1:3-5.

[0013] Preferably, when the deep eutectic solvent contains tetraoctylammonium chloride-n-hexanoic acid, the molar ratio of tetraoctylammonium chloride to n-hexanoic acid in the tetraoctylammonium chloride-n-hexanoic acid is 1:3-5.

[0014] Preferably, when the deep eutectic solvent contains menthol-n-decanoic acid, the molar ratio of menthol to n-decanoic acid in the menthol-n-decanoic acid is 1:1-3.

[0015] Preferably, when the deep eutectic solvent contains thymol-octanoic acid, the amount of thymol to octanoic acid in the thymol-octanoic acid is 1:1-3.

[0016] Preferably, when the deep eutectic solvent contains menthol-oleic acid, the molar ratio of menthol to oleic acid in the menthol-oleic acid is 1:1-3.

[0017] Preferably, the activated carbon is coconut shell charcoal, wood charcoal or coal charcoal;

[0018] Preferably, the specific surface area of ​​the activated carbon is 600-1200m 2 / g;

[0019] Preferably, the mesoporous content of the activated carbon is 10-70%;

[0020] Preferably, the BJH adsorption average pore size of the activated carbon is 2.5-6 nm.

[0021] Preferably, the low eutectic solvent is supported on the pores of the activated carbon.

[0022] A second aspect of the present invention provides a method for preparing an adsorbent material, the method comprising the following steps:

[0023] (1) pre-treating the activated carbon;

[0024] (2) mixing the pretreated activated carbon and the deep eutectic solvent, ultrasonicating, and then drying;

[0025] Wherein, the deep eutectic solvent contains at least one pair of hydrogen bond acceptor-hydrogen bond donor;

[0026] The hydrogen bond acceptor is selected from one or more of tetrabutylammonium bromide, tetraoctylammonium chloride, menthol and thymol; the hydrogen bond donor is an organic acid;

[0027] In the deep eutectic solvent, the ratio of the amount of the hydrogen bond acceptor substance to the amount of the hydrogen bond donor substance is 1:1-5.

[0028] Preferably, the organic acid is selected from levulinic acid and / or C6-C18 fatty acids;

[0029] Preferably, the C6-C18 fatty acid is selected from one or more of n-hexanoic acid, oleic acid, n-decanoic acid and n-octanoic acid.

[0030] Preferably, the activated carbon is coconut shell charcoal, wood charcoal or coal charcoal.

[0031] Preferably, the specific surface area of ​​the activated carbon is 600-1200m 2 / g;

[0032] Preferably, the mesoporous content of the activated carbon is 10-70%;

[0033] Preferably, the BJH adsorption average pore size of the activated carbon is 2.5-6 nm.

[0034] Preferably, in step (1), the pretreatment is performed by heat treatment;

[0035] Preferably, the heat treatment conditions include: temperature of 200-800° C.; time of 1-12 h; and inert atmosphere.

[0036] Preferably, in step (2), the weight ratio of the pretreated activated carbon to the low eutectic solvent is 1:0.05-0.5.

[0037] Preferably, in step (2), the ultrasonic conditions include: ultrasonic power of 200-500 W; ultrasonic frequency of 28-40 kHz; and time of 30-60 min.

[0038] Preferably, in step (2), the drying conditions include: pressure of 0.1-5 kPa, temperature of 60-150° C., and time of 12-72 h.

[0039] Preferably, the method for preparing the low eutectic solvent comprises: mixing a hydrogen bond donor and a hydrogen bond acceptor, and stirring the mixture at 20 to 100° C. for 10 to 100 minutes.

[0040] The third aspect of the present invention provides an adsorption material prepared by the method described above.

[0041] The fourth aspect of the present invention provides the use of the adsorption material described above in the adsorption of VOCs.

[0042] A fifth aspect of the present invention provides a method for adsorbing VOCs, the method comprising: mixing and contacting the adsorption material described above with a gas containing VOCs;

[0043] Wherein, the temperature of the mixed contact is 0-60°C and the pressure is 0.1-1MPa.

[0044] The present invention discloses an adsorption material, which includes activated carbon and a low eutectic solvent loaded on the activated carbon, and has excellent adsorption performance for C2-C3 light hydrocarbons in VOCs. It has the characteristics of low cost, easy operation and maintenance, and has the dual significance of improving VOCs recovery efficiency and process safety. DETAILED DESCRIPTION

[0045] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.

[0046] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0047] In one aspect, the present invention provides an adsorption material, the adsorption material comprising: activated carbon and a deep eutectic solvent supported on the activated carbon;

[0048] Wherein, the deep eutectic solvent contains at least one pair of hydrogen bond acceptor-hydrogen bond donor;

[0049] The hydrogen bond acceptor is selected from one or more of tetrabutylammonium bromide, tetraoctylammonium chloride, menthol and thymol; the hydrogen bond donor is an organic acid;

[0050] In the deep eutectic solvent, the ratio of the amount of the hydrogen bond acceptor substance to the amount of the hydrogen bond donor substance is 1:1-5.

[0051] Preferably, the low eutectic solvent is supported on the pores of the activated carbon.

[0052] Low eutectic solvents are a new type of green solvents with extremely low saturated vapor pressure, easy raw material availability, simple preparation process, and environmental friendliness. In the present invention, an adsorbent material with high light hydrocarbon (especially C2-C3 light hydrocarbon) adsorption performance and safety performance is obtained by combining low eutectic solvents and activated carbon. At the same time, since low eutectic solvents have the advantages of being hydrophobic and non-flammable, the influence of moisture on adsorption performance can be reduced, thereby improving the safety performance of the adsorbent material.

[0053] In a specific embodiment, in the deep eutectic solvent, the ratio of the total amount of hydrogen bond acceptors to the total amount of hydrogen bond donors can be 1:1, 1:2, 1:3, 1:4 or 1:5.

[0054] In a preferred embodiment, the organic acid is selected from levulinic acid and / or C6-C18 fatty acids.

[0055] Further preferably, the C6-C18 fatty acid is selected from one or more of n-hexanoic acid, oleic acid, n-decanoic acid and n-octanoic acid.

[0056] In the present invention, a low eutectic solvent refers to a low eutectic mixture composed of a hydrogen bond acceptor and a hydrogen bond donor in a certain stoichiometric ratio. Based on this, the hydrogen bond acceptor-hydrogen bond donor means that the hydrogen bond donor and the hydrogen bond acceptor usually appear in pairs, that is, when there is a hydrogen bond donor, there must also be a hydrogen bond acceptor.

[0057] In order to further improve the adsorption performance of the adsorbent material for C2-C3 light hydrocarbons, in a preferred embodiment, the low eutectic solvent contains at least one of tetrabutylammonium bromide-oleic acid, tetraoctylammonium chloride-hexanoic acid, menthol-decanoic acid, thymol-octanoic acid and menthol-oleic acid.

[0058] Preferably, when the low eutectic solvent contains tetrabutylammonium bromide-oleic acid, the molar ratio of tetrabutylammonium bromide to oleic acid in the tetrabutylammonium bromide-oleic acid is 1:3-5; specifically, it can be 1:3, 1:3.5, 1:4, 1:4.5 or 1:5.

[0059] Preferably, when the low eutectic solvent contains tetraoctylammonium chloride-n-hexanoic acid, the molar ratio of tetraoctylammonium chloride to n-hexanoic acid in the tetraoctylammonium chloride-n-hexanoic acid is 1:3-5; specifically, it can be 1:3, 1:3.5, 1:4, 1:4.5 or 1:5.

[0060] Preferably, when the deep eutectic solvent contains menthol-n-decanoic acid, the molar ratio of menthol to n-decanoic acid in the menthol-n-decanoic acid is 1:1-3; specifically, it can be 1:1, 1:1.5, 1:2, 1:2.5 or 1:3.

[0061] Preferably, when the low eutectic solvent contains thymol-octanoic acid, the molar ratio of thymol to octanoic acid in the thymol-octanoic acid is 1:1-3; specifically, it can be 1:1, 1:1.5, 1:2, 1:2.5 or 1:3.

[0062] Preferably, when the low eutectic solvent contains menthol-oleic acid, the molar ratio of menthol to oleic acid in the menthol-oleic acid is 1:1-3; specifically, it can be 1:1, 1:1.5, 1:2, 1:2.5 or 1:3.

[0063] In a preferred embodiment, the activated carbon is coconut shell charcoal, wood charcoal or coal charcoal.

[0064] In the present invention, in order to further improve the adsorption performance of the adsorbent material for C2-C3 light hydrocarbons, in a preferred embodiment, the specific surface area, mesopore content and BJH adsorption average pore size of the activated carbon can be reasonably controlled.

[0065] In a preferred embodiment, the specific surface area of ​​the activated carbon is 600-1200m 2 / g, more preferably 700-1100m 2 In a specific embodiment, the specific surface area of ​​the activated carbon can be 734m 2 / g, 750m 2 / g、779m 2 / g、800m 2 / g、853m 2 / g、900m 2 / g, 965m 2 / g、1000m 2 / g or 1090m 2 / g.

[0066] In a preferred embodiment, the mesopore content of the activated carbon is 10-70%, more preferably 30-60%. In a specific embodiment, the mesopore content of the activated carbon can be 20%, 21%, 25%, 30%, 35%, 36%, 38%, 40%, 42%, 43%, 44%, 45%, 46%, 50%, 55%, 60%, 62% or 65%.

[0067] In a preferred embodiment, the BJH adsorption average pore size of the activated carbon is 2.5-6 nm. Specifically, it can be 2.5 nm, 2.8 nm, 2.9 nm, 3 nm, 3.1 nm, 3.2 nm, 3.3 nm, 3.4 nm, 3.5 nm, 3.8 nm, 4 nm, 4.2 nm, 4.5 nm, 5 nm, 5.5 nm, 5.6 nm or 6 nm.

[0068] A second aspect of the present invention provides a method for preparing an adsorbent material, the method comprising the following steps:

[0069] (1) pre-treating the activated carbon;

[0070] (2) mixing the pretreated activated carbon and the deep eutectic solvent, ultrasonicating, and then drying;

[0071] Wherein, the deep eutectic solvent contains at least one pair of hydrogen bond acceptor-hydrogen bond donor;

[0072] The hydrogen bond acceptor is selected from one or more of tetrabutylammonium bromide, tetraoctylammonium chloride, menthol and thymol; the hydrogen bond donor is an organic acid;

[0073] In the deep eutectic solvent, the ratio of the amount of the hydrogen bond acceptor substance to the amount of the hydrogen bond donor substance is 1:1-5.

[0074] In the present invention, when the deep eutectic solvent contains one or more pairs of hydrogen bond acceptors and hydrogen bond donors, the ratio of the amount of the hydrogen bond acceptor substance to the amount of the hydrogen bond donor substance is 1:1-5. That is, the ratio of the total amount of the hydrogen bond acceptors contained in the deep eutectic solvent to the total amount of the hydrogen bond donor substance is 1:1-5.

[0075] In a specific embodiment, in the deep eutectic solvent, the ratio of the amount of the hydrogen bond acceptor substance to the amount of the hydrogen bond donor substance can be 1:1, 1:2, 1:3, 1:4 or 1:5.

[0076] In a preferred embodiment, the organic acid is selected from levulinic acid and / or C6-C18 fatty acids.

[0077] Further preferably, the C6-C18 fatty acid is selected from one or more of n-hexanoic acid, oleic acid, n-decanoic acid and n-octanoic acid.

[0078] In order to further improve the adsorption performance of the adsorbent material for C2-C3 light hydrocarbons, in the present invention, when the low eutectic solvent contains a hydrogen bond acceptor tetrabutylammonium bromide, the hydrogen bond donor matching the tetrabutylammonium bromide is oleic acid; when the low eutectic solvent contains a hydrogen bond acceptor tetraoctylammonium chloride, the hydrogen bond donor matching the tetraoctylammonium chloride is n-hexanoic acid; when the low eutectic solvent contains a hydrogen bond acceptor menthol, the hydrogen bond donor matching the menthol is n-decanoic acid or oleic acid; when the low eutectic solvent contains a hydrogen bond acceptor thymol, the hydrogen bond donor matching the thymol is oleic acid.

[0079] In a preferred embodiment, the deep eutectic solvent contains at least one of tetrabutylammonium bromide-oleic acid, tetraoctylammonium chloride-hexanoic acid, menthol-decanoic acid, thymol-octanoic acid and menthol-oleic acid.

[0080] Preferably, when the low eutectic solvent contains tetrabutylammonium bromide-oleic acid, the molar ratio of tetrabutylammonium bromide to oleic acid in the tetrabutylammonium bromide-oleic acid is 1:3-5; specifically, it can be 1:3, 1:3.5, 1:4, 1:4.5 or 1:5.

[0081] Preferably, when the low eutectic solvent contains tetraoctylammonium chloride-n-hexanoic acid, the molar ratio of tetraoctylammonium chloride to n-hexanoic acid in the tetraoctylammonium chloride-n-hexanoic acid is 1:3-5; specifically, it can be 1:3, 1:3.5, 1:4, 1:4.5 or 1:5.

[0082] Preferably, when the deep eutectic solvent contains menthol-n-decanoic acid, the molar ratio of menthol to n-decanoic acid in the menthol-n-decanoic acid is 1:1-3; specifically, it can be 1:1, 1:1.5, 1:2, 1:2.5 or 1:3.

[0083] Preferably, when the low eutectic solvent contains thymol-octanoic acid, the molar ratio of thymol to octanoic acid in the thymol-octanoic acid is 1:1-3; specifically, it can be 1:1, 1:1.5, 1:2, 1:2.5 or 1:3.

[0084] Preferably, when the low eutectic solvent contains menthol-oleic acid, the molar ratio of menthol to oleic acid in the menthol-oleic acid is 1:1-3; specifically, it can be 1:1, 1:1.5, 1:2, 1:2.5 or 1:3.

[0085] In the method described in the present invention, in order to further improve the adsorption performance of the adsorbent material for C2-C3 light hydrocarbons, in a preferred embodiment, the specific surface area, mesopore content and BJH adsorption average pore size of the activated carbon can be reasonably controlled.

[0086] Preferably, the activated carbon is coconut shell charcoal, wood charcoal or coal charcoal.

[0087] Preferably, the specific surface area of ​​the activated carbon is 600-1200m 2 / g; more preferably 700-1100m 2 In a specific embodiment, the specific surface area of ​​the activated carbon can be 734m 2 / g, 750m 2 / g、779m 2 / g、800m 2 / g、853m2 / g、900m 2 / g, 965m 2 / g、1000m 2 / g or 1090m 2 / g.

[0088] Preferably, the mesopore content of the activated carbon is 10-70%, more preferably 30-60%. In a specific embodiment, the mesopore content of the activated carbon can be 20%, 21%, 25%, 30%, 35%, 36%, 38%, 40%, 42%, 43%, 44%, 45%, 46%, 50%, 55%, 60%, 62% or 65%.

[0089] Preferably, the BJH adsorption average pore size of the activated carbon is 2.5-6 nm; specifically, it can be 2.5 nm, 2.8 nm, 2.9 nm, 3 nm, 3.1 nm, 3.2 nm, 3.3 nm, 3.4 nm, 3.5 nm, 3.8 nm, 4 nm, 4.2 nm, 4.5 nm, 5 nm, 5.5 nm, 5.6 nm or 6 nm.

[0090] In the method of the present invention, the activated carbon can be obtained commercially. Pre-treating the activated carbon can remove the moisture and volatile components adsorbed by the activated carbon during storage or transportation without changing the original structure of the activated carbon, thereby improving the adsorption performance of the adsorption material.

[0091] In a preferred embodiment, in step (1), the pretreatment is performed by heat treatment.

[0092] Further preferably, the heat treatment conditions include: temperature of 200-800°C; time of 1-12h; inert atmosphere. Specifically, the temperature may be 200°C, 300°C, 400°C, 500°C, 600°C, 700°C or 800°C; the time may be 1h, 2h, 3h, 4h, 5h, 6h, 7h, 8h, 9h, 10h, 11h or 12h, and the inert atmosphere may be nitrogen, argon or helium.

[0093] In the method of the present invention, in order to further improve the adsorption performance of the adsorbent material, the weight ratio of the pretreated activated carbon to the deep eutectic solvent can be reasonably controlled. In a preferred embodiment, in step (2), the weight ratio of the pretreated activated carbon to the deep eutectic solvent is 1:0.05-0.5. Specifically, it can be 1:0.05, 1:0.1, 1:0.2, 1:0.3, 1:0.4 or 1:0.5.

[0094] In a preferred embodiment, in step (2), the ultrasonic conditions include: ultrasonic power of 200-500W; ultrasonic frequency of 28-40kHz; and time of 30-60min. Specifically, the ultrasonic power may be 200W, 300W, 400W or 500W; the ultrasonic frequency may be 28kHz, 30kHz, 32kHz, 34kHz, 36kHz, 38kHz or 40kHz; and the ultrasonic time may be 30min, 35min, 40min, 45min, 50min, 55min or 60min.

[0095] In a preferred embodiment, in step (2), the drying conditions include: pressure of 0.1-5 kPa, temperature of 60-150°C, and time of 12-72 hours. Specifically, the drying pressure may be 0.1 kPa, 0.5 kPa, 1 kPa, 2 kPa, 3 kPa, 4 kPa or 5 kPa; the drying temperature may be 60°C, 70°C, 80°C, 90°C, 100°C, 110°C, 120°C, 130°C, 140°C or 150°C; and the time may be 12 hours, 16 hours, 18 hours, 20 hours, 24 hours, 28 hours, 36 hours, 40 hours, 48 ​​hours, 60 hours or 72 hours.

[0096] In a preferred embodiment, the method for preparing the low eutectic solvent comprises: mixing a hydrogen bond donor and a hydrogen bond acceptor, and stirring the mixture at 20 to 100° C. for 10 to 100 minutes.

[0097] The present invention adopts an ultrasonic impregnation method to load the low eutectic solvent onto the activated carbon, does not require high-temperature heating, and has a simple preparation method.

[0098] The third aspect of the present invention provides an adsorption material prepared by the method described above.

[0099] The fourth aspect of the present invention provides the use of the adsorption material described above in the adsorption of VOCs.

[0100] The adsorption material of the present invention can be used in the adsorption of VOCs, and especially exhibits excellent adsorption performance for C2-C3 components (such as ethane and propane) in oil and gas. It can be used again after vacuum desorption, and has good repeatability.

[0101] A fifth aspect of the present invention provides a method for adsorbing VOCs, the method comprising: mixing and contacting the adsorption material described above with a gas containing VOCs;

[0102] Wherein, the temperature of the mixed contact is 0-60°C and the pressure is 0.1-1MPa.

[0103] The present invention will be described in detail below through examples, but the protection scope of the present invention is not limited thereto.

[0104] Example 1

[0105] Preparation of low eutectic solvent: Weigh 0.2815 g of tetrabutylammonium bromide and 0.7414 g of oleic acid, heat and stir at 80° C. for 60 min to form a clear liquid, and cool to room temperature, wherein the molar ratio of tetrabutylammonium bromide to oleic acid is 1:3.

[0106] Activated carbon sample: coconut shell granular carbon, specific surface area of ​​734m 2 / g, mesopore content is 46.8%, and BJH adsorption average pore diameter is 3.2nm.

[0107] Preparation of adsorption materials:

[0108] (1) Activated carbon pretreatment: The activated carbon was heated at 400 °C for 8 h under nitrogen environment;

[0109] (2) Add 5 g of pretreated activated carbon to the prepared low eutectic solvent, wherein the weight ratio of the pretreated activated carbon to the low eutectic solvent is about 1:0.2, and then ultrasonicate at 200 W and 28 kHz ultrasonic frequency for 30 min, and then dry in a vacuum drying oven at a pressure of 1.2 kPa, a temperature of 80° C., and a time of 48 h to obtain adsorbent material S1.

[0110] Example 2

[0111] Preparation of low eutectic solvent: Weigh 1.252 g of tetraoctylammonium chloride and 0.868 g of n-hexanoic acid, heat and stir at 90° C. for 50 min to form a clear liquid, and cool to room temperature, wherein the molar ratio of tetraoctylammonium chloride to n-hexanoic acid is 1:3.

[0112] Activated carbon sample: wood granular carbon, specific surface area 853m 2 / g, mesopore content is 35.6%, and BJH adsorption average pore diameter is 2.8nm.

[0113] Preparation of adsorption materials:

[0114] (1) Activated carbon pretreatment: The activated carbon was heated at 300 °C for 6 h under nitrogen environment;

[0115] (2) Add 5 g of pretreated activated carbon to the prepared low eutectic solvent, wherein the weight ratio of the pretreated activated carbon to the low eutectic solvent is about 1:0.4, and then ultrasonicate at 200 W and 28 kHz ultrasonic frequency for 60 min, and then dry in a vacuum drying oven at a pressure of 1.0 kPa, a temperature of 100 ° C, and a time of 72 h to obtain adsorbent material S2.

[0116] Example 3

[0117] Preparation of low eutectic solvent: Weigh 0.724 g of menthol and 0.799 g of decanoic acid, heat and stir at 70° C. for 30 min to form a clear liquid, and cool to room temperature, wherein the molar ratio of menthol to decanoic acid is 1:1.

[0118] Activated carbon sample: coal-based granular carbon, specific surface area 779m 2 / g, mesopore content is 47.1%, and BJH adsorption average pore diameter is 3.1nm.

[0119] Preparation of adsorption materials:

[0120] (1) Activated carbon pretreatment: The activated carbon was heated at 500 °C for 3 h under nitrogen environment;

[0121] (2) Add 5 g of pretreated activated carbon to the prepared low eutectic solvent, wherein the weight ratio of the pretreated activated carbon to the low eutectic solvent is about 1:0.3, and then ultrasonicate at 200 W and 28 kHz ultrasonic frequency for 45 min, and then dry in a vacuum drying oven at a pressure of 3 kPa, a temperature of 60°C, and a time of 36 h to obtain adsorbent material S3.

[0122] Example 4

[0123] Preparation of low eutectic solvent: Weigh 0.671 g of thymol and 1.288 g of octanoic acid, heat and stir at 65° C. for 90 min to form a clear liquid, and cool to room temperature, wherein the molar ratio of thymol to octanoic acid is 1:2.

[0124] Activated carbon sample: coconut shell granular carbon, specific surface area 1090m 2 / g, mesopore content 21%, BJH adsorption average pore diameter 2.7nm.

[0125] Preparation of adsorption materials:

[0126] (1) Activated carbon pretreatment: The activated carbon was heated at 200 °C for 10 h under nitrogen environment;

[0127] (2) Add 5 g of pretreated activated carbon to the prepared low eutectic solvent, wherein the weight ratio of the pretreated activated carbon to the low eutectic solvent is about 1:0.4, and then ultrasonicate at 200 W and 28 kHz ultrasonic frequency for 60 min, and then dry in a vacuum drying oven at a pressure of 0.8 kPa, a temperature of 60° C., and a time of 20 h to obtain adsorbent material S4.

[0128] Example 5

[0129] Preparation of low eutectic solvent: Weigh 0.391 g of menthol and 2.118 g of oleic acid, heat and stir at 80° C. for 60 min to form a clear liquid, and cool to room temperature, wherein the molar ratio of menthol to oleic acid is 1:3.

[0130] Activated carbon sample: coconut shell granular carbon, specific surface area 965m 2 / g, mesopore content is 43.9%, and BJH adsorption average pore diameter is 2.8nm.

[0131] Preparation of adsorption materials:

[0132] (1) Activated carbon pretreatment: The activated carbon was heated at 200 °C for 10 h under nitrogen environment;

[0133] (2) Add 5 g of pretreated activated carbon to the prepared low eutectic solvent, wherein the weight ratio of the pretreated activated carbon to the low eutectic solvent is about 1:0.5, and then ultrasonicate at 200 W and 28 kHz ultrasonic frequency for 90 min, and then dry in a vacuum drying oven at a pressure of 0.8 kPa, a temperature of 80°C, and a time of 24 h to obtain adsorbent material S5.

[0134] Example 6

[0135] Preparation of low eutectic solvent: Weigh 0.039 g of menthol and 0.212 g of oleic acid, heat and stir at 80° C. for 60 min to form a clear liquid, and cool to room temperature, wherein the molar ratio of menthol to oleic acid is 1:3.

[0136] Activated carbon sample: coconut shell granular carbon, specific surface area 965m 2 / g, mesopore content is 43.9%, and BJH adsorption average pore diameter is 2.8nm.

[0137] Preparation of adsorption materials:

[0138] (1) Activated carbon pretreatment: The activated carbon was heated at 200 °C for 10 h under nitrogen environment;

[0139] (2) Add 5 g of pretreated activated carbon to the prepared low eutectic solvent, wherein the weight ratio of the pretreated activated carbon to the low eutectic solvent is about 1:0.05, and then ultrasonicate at 200 W and 28 kHz ultrasonic frequency for 90 min, and then dry in a vacuum drying oven at a pressure of 0.8 kPa, a temperature of 80°C, and a time of 24 h to obtain adsorbent material S6.

[0140] Example 7

[0141] Preparation of low eutectic solvent: Weigh 0.391 g of menthol and 2.118 g of oleic acid, heat and stir at 80° C. for 60 min to form a clear liquid, and cool to room temperature, wherein the molar ratio of menthol to oleic acid is 1:3.

[0142] Activated carbon sample: coconut shell granular carbon, specific surface area 965m 2 / g, mesopore content is 43.9%, and BJH adsorption average pore diameter is 2.8nm.

[0143] Preparation of adsorption materials:

[0144] (1) Activated carbon pretreatment: The activated carbon was heated at 200 °C for 1 h under nitrogen environment;

[0145] (2) Add 5 g of pretreated activated carbon to the prepared low eutectic solvent, wherein the weight ratio of the pretreated activated carbon to the low eutectic solvent is about 1:0.5, and then ultrasonicate at 200 W and 28 kHz ultrasonic frequency for 90 min, and then dry in a vacuum drying oven at a pressure of 0.8 kPa, a temperature of 80° C., and a time of 24 h to obtain adsorbent material S7.

[0146] Example 8

[0147] Preparation of low eutectic solvent: Weigh 0.391 g of menthol and 2.118 g of oleic acid, heat and stir at 80° C. for 60 min to form a clear liquid, and cool to room temperature, wherein the molar ratio of menthol to oleic acid is 1:3.

[0148] Activated carbon sample: coconut shell granular carbon, specific surface area 965m 2 / g, mesopore content is 43.9%, and BJH adsorption average pore diameter is 2.8nm.

[0149] Preparation of adsorption materials:

[0150] (1) Activated carbon pretreatment: The activated carbon was heated at 200 °C for 10 h under nitrogen environment;

[0151] (2) Add 5 g of pretreated activated carbon to the prepared low eutectic solvent, wherein the weight ratio of the pretreated activated carbon to the low eutectic solvent is about 1:0.5, and then ultrasonicate at 200 W and 28 kHz ultrasonic frequency for 20 min, and then dry in a vacuum drying oven at a pressure of 0.8 kPa, a temperature of 80°C, and a time of 24 h to obtain adsorbent material S8.

[0152] Example 9

[0153] Preparation of low eutectic solvent: Weigh 0.391 g of menthol and 2.118 g of oleic acid, heat and stir at 80° C. for 60 min to form a clear liquid, and cool to room temperature, wherein the molar ratio of menthol to oleic acid is 1:3.

[0154] Activated carbon sample: coal-based granular carbon, specific surface area 678m 2 / g, mesopore content is 62.9%, and BJH adsorption average pore diameter is 5.3nm.

[0155] Preparation of adsorption materials:

[0156] (1) Activated carbon pretreatment: The activated carbon was heated at 200 °C for 10 h under nitrogen environment;

[0157] (2) Add 5 g of pretreated activated carbon to the prepared low eutectic solvent, wherein the weight ratio of the pretreated activated carbon to the low eutectic solvent is about 1:0.5, and then ultrasonicate at 200 W and 28 kHz ultrasonic frequency for 90 min, and then dry in a vacuum drying oven at a pressure of 0.8 kPa, a temperature of 80°C, and a time of 24 h to obtain adsorbent material S9.

[0158] Example 10

[0159] Preparation of low eutectic solvent: Weigh 0.391 g of menthol and 2.118 g of oleic acid, heat and stir at 80° C. for 60 min to form a clear liquid, and cool to room temperature, wherein the molar ratio of menthol to oleic acid is 1:3.

[0160] Activated carbon sample: wood granular carbon, specific surface area 1163m 2 / g, mesopore content is 20.8%, and BJH adsorption average pore diameter is 2.5nm.

[0161] Preparation of adsorption materials:

[0162] (1) Activated carbon pretreatment: The activated carbon was heated at 200 °C for 10 h under nitrogen environment;

[0163] (2) Add 5 g of pretreated activated carbon to the prepared low eutectic solvent, wherein the weight ratio of the pretreated activated carbon to the low eutectic solvent is about 1:0.5, and then ultrasonicate at 200 W and 28 kHz ultrasonic frequency for 90 min, and then dry in a vacuum drying oven at a pressure of 0.8 kPa, a temperature of 80°C, and a time of 24 h to obtain an adsorbent material S10.

[0164] Comparative Example 1

[0165] Activated carbon sample: coconut shell granular carbon, specific surface area of ​​734m 2 / g, mesopore content is 46.8%, and BJH adsorption average pore diameter is 3.2nm.

[0166] Activated carbon pretreatment: The activated carbon was heated at 400°C for 8 h under a nitrogen environment to obtain pretreated activated carbon D1.

[0167] Comparative Example 2

[0168] Hydrogen bond donor: 2.121 g of n-hexanoic acid, heated and stirred at 90°C for 50 min, and cooled to room temperature.

[0169] Activated carbon sample: wood granular carbon, specific surface area 853m 2 / g, mesopore content is 35.6%, and BJH adsorption average pore diameter is 2.8nm.

[0170] Preparation of materials:

[0171] (1) Activated carbon pretreatment: The activated carbon was heated at 300 °C for 6 h under nitrogen environment;

[0172] (2) 5 g of pretreated activated carbon was added to n-hexanoic acid, wherein the weight ratio of the pretreated activated carbon to n-hexanoic acid was about 1:0.4, and then ultrasonicated at 200 W and 28 kHz for 60 min, followed by drying in a vacuum drying oven at a pressure of 1.0 kPa, a temperature of 100° C., and a time of 72 h to obtain material D2.

[0173] Comparative Example 3

[0174] Hydrogen bond acceptor: 1.525 g of menthol, heated and stirred at 70°C for 30 min, and cooled to room temperature.

[0175] Activated carbon sample: coal-based granular carbon, specific surface area 779m 2 / g, mesopore content is 47.1%, and BJH adsorption average pore diameter is 3.1nm.

[0176] Preparation of materials:

[0177] (1) Activated carbon pretreatment: The activated carbon was heated at 500 °C for 3 h under nitrogen environment;

[0178] (2) 5 g of pretreated activated carbon was added to menthol, wherein the weight ratio of the pretreated activated carbon to menthol was about 1:0.3, and then ultrasonicated at 200 W and 28 kHz for 45 min, followed by drying in a vacuum drying oven at a pressure of 3 kPa, a temperature of 60° C., and a time of 36 h to obtain material D3.

[0179] Comparative Example 4

[0180] Preparation of low eutectic solvent: Weigh 1.349 g of choline chloride and 1.160 g of urea, heat and stir at 80° C. for 60 min to form a clear liquid, and cool to room temperature.

[0181] Activated carbon sample: coconut shell granular carbon, specific surface area 965m 2 / g, mesopore content is 43.9%, and BJH adsorption average pore diameter is 2.8nm.

[0182] Preparation of adsorption materials:

[0183] (1) Activated carbon pretreatment: The activated carbon was heated at 200 °C for 10 h under nitrogen environment;

[0184] (2) Add 5 g of pretreated activated carbon to the prepared low eutectic solvent, wherein the weight ratio of the pretreated activated carbon to the low eutectic solvent is about 1:0.5, and then ultrasonicate at 200 W and 28 kHz ultrasonic frequency for 90 min, and then dry in a vacuum drying oven at a pressure of 0.8 kPa, a temperature of 80°C, and a time of 24 h to obtain adsorbent material D4.

[0185] Comparative Example 5

[0186] Preparation of low eutectic solvent: Weigh 1.252 g of tetraoctylammonium chloride and 0.868 g of n-hexanoic acid, heat and stir at 90° C. for 50 min to form a clear liquid, and cool to room temperature, wherein the molar ratio of tetraoctylammonium chloride to n-hexanoic acid is 1:3.

[0187] Activated carbon sample: wood granular carbon, specific surface area 853m 2 / g, mesopore content is 35.6%, and BJH adsorption average pore diameter is 2.8nm.

[0188] Preparation of adsorption materials:

[0189] The activated carbon in this comparative example was not pretreated, wherein the weight ratio of the activated carbon to the low eutectic solvent was about 1:0.4, and then ultrasonicated at 200 W and 28 kHz ultrasonic frequency for 60 min, and then dried in a vacuum drying oven at a pressure of 1.0 kPa, a temperature of 100° C., and a time of 72 h to obtain adsorbent material D5.

[0190] Test Example 1

[0191] The materials prepared in Examples 1-10 and Comparative Examples 1-5 were tested for ethane and propane adsorption performance using a high-pressure adsorption capacity tester. Nitrogen was used as the carrier gas during the test, and the test gas systems were ethane + nitrogen and propane + nitrogen, respectively, wherein the alkane composition was 10% vol, and the total gas flow rate was 50 ml / min. The results are shown in Table 1.

[0192] Table 1

[0193]

[0194] It can be seen from Table 1 that the adsorption material of the present invention exhibits excellent adsorption performance for ethane and propane.

[0195] Test Example 2

[0196] The adsorbent material S5 after the adsorption performance test in Test Example 1 was desorbed under a vacuum environment with a desorption pressure of 3.5 kPa and a desorption time of 15 minutes to obtain a regenerated material C1.

[0197] The ethane and propane adsorption performance of material C1 was tested using a high-pressure adsorption capacity tester. Nitrogen was used as the carrier gas in the test process, and the test gas systems were ethane + nitrogen and propane + nitrogen, respectively, in which the alkane composition was 10% vol, and the total gas flow rate was 50 ml / min. When the adsorption temperature was 10°C and the adsorption pressure was 0.9 MPa, the adsorption capacities of ethane and n-butane were 118.27 and 346.75, respectively. The data were basically consistent with the experimental results of the adsorption material S5 in Test Example 1, verifying that the adsorption material prepared by the present invention can achieve desorption and regeneration under vacuum conditions, and there is basically no loss in adsorption capacity.

[0198] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. An adsorption material, characterized in that: The adsorption material comprises: activated carbon and a deep eutectic solvent supported on the activated carbon; Wherein, the deep eutectic solvent contains at least one pair of hydrogen bond acceptor-hydrogen bond donor; The hydrogen bond acceptor is selected from one or more of tetrabutylammonium bromide, tetraoctylammonium chloride, menthol and thymol; the hydrogen bond donor is an organic acid; In the deep eutectic solvent, the ratio of the amount of the hydrogen bond acceptor substance to the amount of the hydrogen bond donor substance is 1:1-5.

2. The adsorption material according to claim 1, characterized in that The organic acid is selected from levulinic acid and / or C6-C18 fatty acid; Preferably, the C6-C18 fatty acid is selected from one or more of n-hexanoic acid, oleic acid, n-decanoic acid and n-octanoic acid.

3. The adsorption material according to claim 2, characterized in that When the deep eutectic solvent contains tetrabutylammonium bromide-oleic acid, the molar ratio of tetrabutylammonium bromide to oleic acid in the tetrabutylammonium bromide-oleic acid is 1:3-5.

4. The adsorption material according to claim 2 or 3, characterized in that: When the deep eutectic solvent contains tetraoctylammonium chloride-n-hexanoic acid, the molar ratio of tetraoctylammonium chloride to n-hexanoic acid in the tetraoctylammonium chloride-n-hexanoic acid is 1:3-5.

5. The adsorption material according to claim 2, characterized in that When the deep eutectic solvent contains menthol-n-decanoic acid, the molar ratio of menthol to n-decanoic acid in the menthol-n-decanoic acid is 1:1-3.

6. The adsorption material according to claim 2, characterized in that: When the deep eutectic solvent contains thymol-octanoic acid, the amount of thymol to octanoic acid in the thymol-octanoic acid is 1:1-3.

7. The adsorbent material according to claim 2, characterized in that: When the deep eutectic solvent contains menthol-oleic acid, the molar ratio of menthol to oleic acid in the menthol-oleic acid is 1:1-3.

8. The adsorbent material according to claim 1 or 2, characterized in that: The activated carbon is coconut shell charcoal, wood charcoal or coal charcoal; Preferably, the specific surface area of ​​the activated carbon is 600-1200m 2 / g; Preferably, the mesoporous content of the activated carbon is 10-70%; Preferably, the BJH adsorption average pore size of the activated carbon is 2.5-6 nm.

9. The adsorbent material according to claim 1, characterized in that: The deep eutectic solvent is supported on the pores of the activated carbon.

10. A method for preparing an adsorbent material, characterized in that: The method comprises the following steps: (1) pre-treating the activated carbon; (2) mixing the pretreated activated carbon and the deep eutectic solvent, ultrasonicating, and then drying; Wherein, the deep eutectic solvent contains at least one pair of hydrogen bond acceptor-hydrogen bond donor; The hydrogen bond acceptor is selected from one or more of tetrabutylammonium bromide, tetraoctylammonium chloride, menthol and thymol; the hydrogen bond donor is an organic acid; In the deep eutectic solvent, the ratio of the amount of the hydrogen bond acceptor substance to the amount of the hydrogen bond donor substance is 1:1-5.

11. The method according to claim 10, characterized in that The organic acid is selected from levulinic acid and / or C6-C18 fatty acid; Preferably, the C6-C18 fatty acid is selected from one or more of n-hexanoic acid, oleic acid, n-decanoic acid and n-octanoic acid.

12. The adsorbent material according to claim 10 or 11, characterized in that: The activated carbon is coconut shell charcoal, wood charcoal or coal charcoal. Preferably, the specific surface area of ​​the activated carbon is 600-1200m 2 / g; Preferably, the mesoporous content of the activated carbon is 10-70%; Preferably, the BJH adsorption average pore size of the activated carbon is 2.5-6 nm.

13. The method according to claim 10, characterized in that In step (1), the pretreatment method is heat treatment; Preferably, the heat treatment conditions include: temperature of 200-800° C.; time of 1-12 h; and inert atmosphere.

14. The method according to claim 10 or 11, characterized in that In step (2), the weight ratio of the pretreated activated carbon to the low eutectic solvent is 1:0.05-0.

5.

15. The method according to any one of claims 10 to 14, characterized in that: In step (2), the ultrasonic conditions include: ultrasonic power of 200-500W; ultrasonic frequency of 28-40kHz; and time of 30-60min.

16. The method according to claim 10, characterized in that In step (2), the drying conditions include: pressure of 0.1-5 kPa, temperature of 60-150° C., and time of 12-72 h.

17. The method according to claim 10, characterized in that The preparation method of the low eutectic solvent comprises: mixing a hydrogen bond donor and a hydrogen bond acceptor and stirring the mixture at 20 to 100° C. for 10 to 100 minutes.

18. An adsorbent material prepared by the method according to any one of claims 10 to 17.

19. Use of the adsorption material according to any one of claims 1 to 9 or the adsorption material according to claim 18 in adsorbing VOCs.

20. A method for adsorbing VOCs, characterized in that: The method comprises: mixing and contacting the adsorption material according to any one of claims 1 to 5 or the adsorption material according to claim 13 with a gas containing VOCs; Wherein, the temperature of the mixed contact is 0-60°C and the pressure is 0.1-1MPa.