Preparation method and application of cerium-based catalyst
Through the preparation method of cerium-based catalyst, the cerium-based oxide precursor is dispersed with a porous support, and the use of chemical dehydrating agents is avoided, and the problems of by-product generation and high energy consumption in the synthesis of dimethyl carbonate are solved, so as to achieve the problem of existing catalysts. High efficiency and low energy consumption catalytic effect.
Patent Information
- Application Number
- CN202411075270.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-12
AI Technical Summary
The existing catalysts need to add chemical dehydrating agents during the synthesis of dimethyl carbonate, resulting in increased energy consumption of by-product generation and separation, affecting production costs and carbon emissions.
By using the preparation method of cerium-based catalyst, the metal oxide precursor is loaded onto the porous support in an extremely short reflux time, and the cerium-based catalyst is formed after calcination, which avoids the need to add a dehydrating agent and improves the catalytic effect.
It has achieved efficient and low-energy synthesis of dimethyl carbonate, with uniform catalyst size, less agglomeration of particles, rich mesoporous structure, high reaction yield, and meets the requirements of green and efficient production.
Smart Images

Figure CN118925708A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of catalyst preparation, and in particular to a preparation method and application of a cerium-based catalyst. Background Art
[0002] Dimethyl carbonate (DMC) is an important chemical raw material, widely used in the production of fine chemicals such as polycarbonate, developer, and coating. Driven by the new energy industry, the consumption of dimethyl carbonate as lithium battery electrolyte continues to increase, accounting for 34% of its total domestic consumption in 2023. Therefore, dimethyl carbonate is not only a fine chemical raw material with important industrial value, but also a key new energy material for achieving green transformation of energy structure and sustainable development.
[0003] The production processes of dimethyl carbonate mainly include phosgene method, transesterification method and methanol oxidation carbonylation method. Phosgene method is a traditional method for synthesizing dimethyl carbonate, but it is highly polluting, highly toxic and has low safety, and has been gradually eliminated. The transesterification method uses propylene oxide, methanol and carbon dioxide as raw materials to produce dimethyl carbonate while producing a large amount of propylene glycol as a by-product. The raw material price is high and the by-product output is large, which seriously affects the economic benefits. Methanol oxidation carbonylation uses methanol, carbon monoxide and oxygen as raw materials. The process is simple and the cost is low, but the mixture of carbon monoxide and oxygen is explosive. Carbon dioxide can be used as a raw material to replace carbon monoxide and oxygen, and dimethyl carbonate can be directly synthesized with methanol, and the above problems can be effectively overcome. The synthesis route of dimethyl carbonate using methanol and carbon dioxide as raw materials is similar to the methanol carbonylation method. The only by-product is water, which has a high atomic economy. While producing dimethyl carbonate, it also realizes the high-value utilization of carbon dioxide and reduces the overall carbon emissions of the process.
[0004] The key to synthesizing dimethyl carbonate from methanol and carbon dioxide is the catalyst. Since the synthesis of dimethyl carbonate is accompanied by the generation of water, which limits the forward reaction and affects the reaction yield, the existing catalysts often need to add chemical dehydrating agents such as 2-cyanopyridine and methyl trichloroacetate during the reaction. Although chemical dehydrating agents can quickly dehydrate, they will generate by-products, increase separation energy consumption, and affect production costs.
[0005] Therefore, it is of great practical significance to develop green and efficient catalysts and promote the development of the process route for directly synthesizing dimethyl carbonate from carbon dioxide and methanol. Summary of the invention
[0006] The invention provides a method for preparing a cerium-based catalyst, which has a simple preparation process, cheap and readily available raw materials, high yield, short synthesis cycle, low energy consumption, and good repeatability of synthesis of different batches of catalysts.
[0007] The present invention also provides a cerium-based catalyst and application thereof. The cerium-based catalyst has uniform size, less particle agglomeration, and a rich mesoporous structure, thus having a good catalytic effect and no need to add a dehydrating agent during the catalytic process.
[0008] The first aspect of the present invention provides a method for preparing a cerium-based catalyst, which comprises the following steps:
[0009] 1) mixing a metal salt solution containing a cerium salt with an inorganic alkali solution, and performing a first stirring and aging treatment to obtain a precursor suspension;
[0010] 2) heating the precursor suspension under reflux at 100-170° C., adding a porous carrier, and performing a second stirring aging treatment to obtain a carrier loaded with the precursor;
[0011] 3) washing, drying and calcining the carrier carrying the precursor to obtain the cerium-based catalyst.
[0012] The preparation method as described above, wherein the metal salt solution further comprises at least one of a zirconium salt, a zinc salt and a copper salt;
[0013] And / or, the inorganic base in the inorganic base solution includes at least one of sodium hydroxide, potassium hydroxide and ammonia water;
[0014] And / or, the porous carrier includes at least one of kaolin, bentonite, diatomaceous earth, MCM-41 molecular sieve, NaY molecular sieve, all-silicon ZSM-5 molecular sieve, Beta molecular sieve and USY molecular sieve.
[0015] The preparation method as described above, wherein the concentration of the metal salt solution is 0.2-0.8 mol / L;
[0016] And / or, the concentration of the inorganic alkali solution is 1-8 mol / L.
[0017] In the preparation method as described above, the molar ratio of the inorganic base in the inorganic base solution to the metal salt in the metal salt solution is 5 to 30.
[0018] In the preparation method as described above, the mass ratio of the porous carrier to the metal salt in the metal salt solution is 3-5.
[0019] In the preparation method as described above, in step 2), the porous carrier is added after the precursor suspension is refluxed for 5 to 90 minutes.
[0020] In the preparation method as described above, the calcination temperature is 400-800° C. and the calcination time is 1-8 hours.
[0021] A second aspect of the present invention provides a cerium-based catalyst, which is obtained according to the above preparation method.
[0022] The third aspect of the present invention provides a method for preparing dimethyl carbonate, which comprises the following steps:
[0023] The catalyst obtained according to the above preparation method or the above catalyst is mixed with methanol, and carbon dioxide is introduced to obtain dimethyl carbonate.
[0024] The method as described above, wherein the mass ratio of the methanol to the catalyst is 5 to 15;
[0025] and / or, the reaction temperature is 100 to 160° C.;
[0026] And / or, the reaction pressure is 2 to 6 MPa.
[0027] The preparation method of the cerium-based catalyst of the present invention synthesizes a metal oxide precursor in a very short reflux time by a rapid reflux method, and adds a porous carrier during the reflux process to grow the metal oxide precursor on the porous carrier, and forms a cerium-based catalyst after calcination. The reflux method has a simple preparation process, the raw material used as the catalyst carrier is cheap and easy to obtain, the yield is high, the synthesis cycle is short, the energy consumption is low, and the synthesis repeatability of different batches of catalysts is good. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.
[0029] Figure 1 is a SEM image of the cerium-based catalyst in Example 2;
[0030] Figure 2a EDS pattern of the cerium-based catalyst in Example 2;
[0031] Figure 2b EDS image of Al element on the surface of the cerium-based catalyst in Example 2;
[0032] Figure 2c EDS image of Si element on the surface of the cerium-based catalyst in Example 2;
[0033] Figure 2d EDS image of Ce element on the surface of the cerium-based catalyst in Example 2;
[0034] Figure 3 TEM image of the cerium-based catalyst in Example 2;
[0035] Figure 4 is the XRD diffraction spectrum of the cerium-based catalyst in Example 2, Example 10 and Example 11;
[0036] Figure 5 is a diagram of N2 adsorption-desorption of the cerium-based catalyst in Example 2, Example 10 and Example 11;
[0037] Figure 6 3 is the pore size distribution diagram of the cerium-based catalyst in Example 2, Example 10 and Example 11. DETAILED DESCRIPTION
[0038] In order to make the purpose, technical solutions and advantages of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0039] The first aspect of the present invention provides a method for preparing a cerium-based catalyst, which comprises the following steps:
[0040] 1) mixing a metal salt solution containing a cerium salt with an inorganic alkali solution, and performing a first stirring and aging treatment to obtain a precursor suspension;
[0041] 2) heating the precursor suspension under reflux at 100-170° C., adding a porous carrier, and performing a second stirring aging treatment to obtain a carrier loaded with the precursor;
[0042] 3) washing, drying and calcining the carrier carrying the precursor to obtain the cerium-based catalyst.
[0043] The preparation method of the cerium-based catalyst of the present invention comprises the following steps:
[0044] Step 1) mixing a metal salt solution containing cerium salt with an inorganic base solution, wherein the cerium salt generates a hydroxide precipitate containing cerium under the action of the inorganic base, and after a first stirring aging treatment for sufficient reaction, a precursor suspension is obtained.
[0045] The cerium salt of the present invention is a soluble metal salt of cerium, such as cerium nitrate and cerium chloride.
[0046] Step 2), heating and refluxing the above-mentioned precursor suspension at 100-170°C, adding a porous carrier, the metal ions in the precursor and the hydroxyl groups on the porous carrier form a chemical reaction, so that the precursor is loaded on the porous carrier to obtain a carrier loaded with the precursor. The porous carrier can effectively disperse the precursor, thereby improving the catalytic activity.
[0047] Step 3), washing the carrier loaded with the precursor until the washing liquid is neutral, then drying to obtain a powder, and calcining the powder to obtain a cerium-based catalyst.
[0048] The preparation method of the cerium-based catalyst of the present invention loads the cerium-based oxide precursor onto a porous carrier by a rapid reflux method. Due to the chemical reaction between the cerium-based oxide precursor and the porous carrier, the porous carrier can effectively disperse the cerium-based oxide precursor, and the porous carrier can remove water generated during the catalytic reaction by physical adsorption, without the need to add additional chemical dehydrating agents, thereby reducing the generation of by-products, so that the catalyst of the present invention has a good catalytic effect.
[0049] In a specific embodiment, the metal salt solution further includes at least one of a zirconium salt, a zinc salt and a copper salt.
[0050] The inventors have found through research that when the metal salt solution is a compound of different metal salts, the catalytic effect of the cerium-based catalyst finally prepared is better.
[0051] Preferably, the metal salt solution is a solution of a double metal salt of a cerium salt and a zirconium salt.
[0052] More preferably, the metal salt solution comprises cerium salt and zirconium salt in a molar ratio of 9:1.
[0053] Furthermore, the inorganic base in the inorganic base solution includes at least one of sodium hydroxide, potassium hydroxide and ammonia water.
[0054] The cerium-based catalysts prepared using different types of inorganic bases in the present invention all have good catalytic performance. Preferably, when the inorganic base is sodium hydroxide, the cerium-based catalyst has the best performance.
[0055] Furthermore, the porous carrier includes at least one of kaolin, bentonite, diatomaceous earth, MCM-41 molecular sieve, NaY molecular sieve, all-silicon ZSM-5 molecular sieve, Beta molecular sieve and USY molecular sieve.
[0056] The inventors have found that different types of porous carriers have different effects on catalyst performance. Suitable porous carriers can effectively disperse cerium-based oxide precursors and adsorb water generated during the catalyst reaction, thereby improving the raw material conversion rate. Preferably, when kaolin is used as a porous carrier, the cerium-based catalyst has the best performance.
[0057] In a specific embodiment, the concentration of the metal salt solution is 0.2 to 0.8 mol / L;
[0058] Furthermore, the concentration of the inorganic alkali solution is 1 to 8 mol / L.
[0059] Preferably, the concentration of the metal salt solution is 0.4 mol / L; the concentration of the inorganic alkali solution is 5 mol / L.
[0060] In another specific embodiment, the molar ratio of the inorganic base in the inorganic base solution to the metal salt in the metal salt solution is 5-30.
[0061] Preferably, the molar ratio of the inorganic base in the inorganic base solution to the metal salt in the metal salt solution is 20.
[0062] Furthermore, the mass ratio of the porous carrier to the metal salt in the metal salt solution is 3-5.
[0063] Preferably, the mass ratio of the porous carrier to the metal salt in the metal salt solution is 4.
[0064] In a specific embodiment, in step 2), the porous carrier is added after the precursor suspension is refluxed for 5 to 90 minutes.
[0065] Preferably, in step 2), the porous carrier is added after the precursor suspension is refluxed for 30 minutes.
[0066] In another specific embodiment, the calcination temperature is 400-800° C., and the calcination time is 1-8 hours.
[0067] Preferably, the calcination temperature is 600° C. and the calcination time is 5 hours.
[0068] When the concentration of the reaction raw materials, the addition ratio and the reaction process conditions are within the above ranges, both the reaction cost and the catalytic effect of the cerium-based catalyst can be taken into consideration.
[0069] A second aspect of the present invention provides a cerium-based catalyst, which is obtained according to the above preparation method.
[0070] In the cerium-based catalyst of the present invention, the cerium-based oxide is effectively dispersed on the porous carrier, the catalyst has uniform size, less particle agglomeration, more mesoporous structures, and good catalytic effect.
[0071] The third aspect of the present invention provides a method for preparing dimethyl carbonate, which comprises the following steps:
[0072] The catalyst obtained according to the above preparation method or the above catalyst is mixed with methanol, and carbon dioxide is introduced to obtain dimethyl carbonate.
[0073] The present invention uses methanol and carbon dioxide as raw materials to synthesize dimethyl carbonate under the action of a cerium-based catalyst. The cerium-based catalyst has a good catalytic effect and a high reaction yield. In addition, no additional chemical dehydrating agent needs to be added during the reaction process, thereby reducing the generation of by-products and meeting the current requirements for green and efficient production.
[0074] In a specific embodiment, the mass ratio of the methanol to the catalyst is 5 to 15; the reaction temperature is 100 to 160° C.; and the reaction pressure is 2 to 6 MPa.
[0075] Preferably, when the mass ratio of methanol to catalyst is 10, the reaction temperature is 140° C., and the reaction pressure is 5 MPa, the yield of dimethyl carbonate is the highest.
[0076] The solution provided by the present invention is further described below in conjunction with specific embodiments.
[0077] Example 1
[0078] The preparation method of the cerium-based catalyst of this embodiment comprises the following steps:
[0079] 1) dissolving cerium nitrate in deionized water to prepare a salt solution with a metal salt concentration of 0.2 mol / L; dissolving sodium hydroxide in deionized water to prepare an alkali solution with an inorganic alkali concentration of 5 mol / L; under continuous stirring, adding the metal salt solution dropwise to the inorganic alkali solution, wherein the amount of sodium hydroxide in the inorganic alkali solution is 20 times the amount of cerium nitrate in the metal salt solution; after the addition is completed, stirring and aging are continued for 30 minutes to obtain a precursor suspension;
[0080] 2) heating the suspension at 150° C. to rapidly reflux; adding kaolin after reflux for 30 min and continuing stirring for 120 min, wherein the mass of kaolin added is 4 times the mass of cerium nitrate;
[0081] 3) Separating kaolin loaded with cerium oxide precursor from the suspension, washing to neutrality, and drying to obtain precursor powder; calcining the precursor powder at 600° C. for 5 h, and grinding to obtain a cerium-based catalyst, which is labeled as CeO2-1 / kaolin-1.
[0082] Example 2
[0083] The preparation method of the cerium-based catalyst in this example is basically the same as that in Example 1, except that the metal salt concentration is 0.4 mol / L of the salt solution, and the cerium-based catalyst obtained in Example 2 is marked as CeO2-2 / kaolin-1.
[0084] Figure 12 is a SEM image of the cerium-based catalyst in Example 2; it can be seen from the image that the catalyst has a short and thick rod-like structure with a relatively large pore structure, and a small amount of CeO2 can be seen growing on the surface of part of the kaolin.
[0085] pass Figure 2a The EDS images in Figure 5-d further illustrate the chemical composition of the CeO2-2 / kaolin-1 catalyst. The image shows that the catalyst contains 52% Al, 43% Si and 5% Ce, and the three elements are evenly distributed on the catalyst.
[0086] Figure 3 TEM image of the cerium-based catalyst in Example 2; it can be seen from the figure that a circle of nanorod-like particles surrounds the surface of kaolin, indicating that CeO2 is successfully loaded onto the surface of kaolin to form a loaded cerium-based oxide catalyst.
[0087] Example 3
[0088] The preparation method of the cerium-based catalyst in this example is basically the same as that in Example 1, except that the metal salt concentration is 0.8 mol / L of the salt solution, and the cerium-based catalyst obtained in this example is marked as CeO2-3 / kaolin-1.
[0089] Example 4
[0090] The preparation method of the cerium-based catalyst in this example is basically the same as that in Example 2, except that the concentration of the inorganic base in step 1) is 1 mol / L, and the cerium-based catalyst obtained in this example is marked as CeO2-4 / kaolin-1.
[0091] Example 5
[0092] The preparation method of the cerium-based catalyst in this example is basically the same as that in Example 2, except that the concentration of the inorganic base in step 1) is 8 mol / L, and the cerium-based catalyst obtained in this example is marked as CeO2-5 / kaolin-1.
[0093] Example 6
[0094] The preparation method of the cerium-based catalyst in this embodiment is basically the same as that in Example 2, except that: in step 1), the amount of sodium hydroxide in the alkaline solution is 5 times the amount of cerium nitrate in the salt solution. The cerium-based catalyst obtained in this embodiment is marked as CeO2-6 / kaolin-1.
[0095] Example 7
[0096] The preparation method of the cerium-based catalyst in this embodiment is basically the same as that in Example 2, except that: in step 1), the amount of sodium hydroxide in the alkaline solution is 20 times the amount of cerium nitrate in the salt solution. The cerium-based catalyst obtained in this embodiment is marked as CeO2-7 / kaolin-1.
[0097] Example 8
[0098] The preparation method of the cerium-based catalyst in this example is basically the same as that in Example 2, except that: in step 2), the suspension is heated at 100° C. to rapidly reflux. The cerium-based catalyst obtained in this example is labeled as CeO2-8 / kaolin-1.
[0099] Example 9
[0100] The preparation method of the cerium-based catalyst in this example is basically the same as that in Example 2, except that: in step 2), the suspension is heated at 160° C. to rapidly reflux. The cerium-based catalyst obtained in this example is labeled as CeO2-9 / kaolin-1.
[0101] Example 10
[0102] The preparation method of the cerium-based catalyst in this example is basically the same as that in Example 2, except that: in step 2), kaolin is added after refluxing for 5 minutes. The cerium-based catalyst obtained in this example is marked as CeO2-10 / kaolin-1.
[0103] Embodiment 11
[0104] The preparation method of the cerium-based catalyst in this example is basically the same as that in Example 2, except that: in step 2), kaolin is added after reflux for 90 minutes. The cerium-based catalyst obtained in this example is marked as CeO2-11 / kaolin-1.
[0105] Figure 4 The XRD diffraction spectra of CeO2-2 / kaolin-1, CeO2-10 / kaolin-1 and CeO2-11 / kaolin-1 catalysts are shown in Figure 2. The diffraction peaks at 2θ=28.5°, 33.1°, 47.5° and 56.3° belong to CeO2, and the diffraction peaks at 2θ=15.8°, 26.4°, 35.0° and 40.6° belong to kaolin, indicating that CeO2 is successfully loaded onto the kaolin carrier to form a loaded cerium-based oxide catalyst.
[0106] Figure 5 Figure 2 shows the N2 adsorption-desorption curves of CeO2-2 / kaolin-1, CeO2-10 / kaolin-1 and CeO2-11 / kaolin-1 catalysts. The catalysts all exhibit typical IV type adsorption-desorption isotherms with hysteresis loops, indicating that CeO2 / kaolin has a mesoporous structure.
[0107] Figure 6 The pore size distribution diagrams of CeO2-2 / kaolin-1, CeO2-10 / kaolin-1 and CeO2-11 / kaolin-1 catalysts are shown in Figure 1. The results show that CeO2 / kaolin catalysts have similar pore size distributions, and the most probable pore size is around 10 nm.
[0108] Example 12
[0109] The preparation method of the cerium-based catalyst in this example is basically the same as that in Example 2, except that the inorganic base in step 1) is potassium hydroxide, and the cerium-based catalyst obtained in this example is marked as CeO2-12 / kaolin-1.
[0110] Embodiment 13
[0111] The preparation method of the cerium-based catalyst in this example is basically the same as that in Example 2, except that the inorganic base in step 1) is aqueous ammonia, and the cerium-based catalyst obtained in this example is marked as CeO2-13 / kaolin-1.
[0112] Embodiment 14
[0113] The preparation method of the cerium-based catalyst in this example is basically the same as that in Example 2, except that the inorganic base in step 1) is a mixture of sodium hydroxide and potassium hydroxide, and the cerium-based catalyst obtained in this example is marked as CeO2-14 / kaolin-1.
[0114] Embodiment 15
[0115] The preparation method of the cerium-based catalyst in this example is basically the same as that in Example 2, except that the inorganic base in step 1) is a mixture of sodium hydroxide and ammonia water, and the cerium-based catalyst obtained in this example is marked as CeO2-15 / kaolin-1.
[0116] Example 16
[0117] The preparation method of the cerium-based catalyst in this example is basically the same as that in Example 2, except that the porous carrier added in step 2) is bentonite, and the cerium-based catalyst obtained in this example is marked as CeO2-2 / bentonite-1 catalyst.
[0118] Embodiment 17
[0119] The preparation method of the cerium-based catalyst in this example is basically the same as that in Example 2, except that the porous carrier added in step 2) is diatomaceous earth, and the cerium-based catalyst obtained in this example is marked as CeO2-2 / diatomaceous earth-1 catalyst.
[0120] Embodiment 18
[0121] The preparation method of the cerium-based catalyst in this example is basically the same as that in Example 2, except that the porous carrier added in step 2) is MCM-41 molecular sieve, and the cerium-based catalyst obtained in this example is marked as CeO2-2 / MCM-41.
[0122] Embodiment 19
[0123] The preparation method of the cerium-based catalyst in this example is basically the same as that in Example 2, except that the porous carrier added in step 2) is NaY molecular sieve, and the cerium-based catalyst obtained in this example is marked as CeO2-2 / MCM-41 catalyst.
[0124] Embodiment 20
[0125] The preparation method of the cerium-based catalyst in this example is basically the same as that in Example 2, except that the porous carrier added in step 2) is a ZSM-5 molecular sieve, and the cerium-based catalyst obtained in this example is marked as CeO2-2 / ZSM-5 catalyst.
[0126] Embodiment 21
[0127] The preparation method of the cerium-based catalyst in this example is basically the same as that in Example 2, except that the porous carrier added in step 2) is Beta molecular sieve, and the cerium-based catalyst obtained in this example is marked as CeO2-2 / Beta catalyst.
[0128] Embodiment 22
[0129] The preparation method of the cerium-based catalyst in this example is basically the same as that in Example 2, except that the porous carrier added in step 2) is USY molecular sieve, and the cerium-based catalyst obtained in this example is marked as CeO2-2 / USY catalyst.
[0130] Embodiment 23
[0131] The preparation method of the cerium-based catalyst in this example is basically the same as that in Example 2, except that the mass of kaolin added in step 2) is 4 times the mass of cerium nitrate. The cerium-based catalyst obtained in this example is marked as CeO2-2 / kaolin-2.
[0132] Embodiment 24
[0133] The preparation method of the cerium-based catalyst in this example is basically the same as that in Example 2, except that the mass of kaolin added in step 2) is 5 times the mass of cerium nitrate. The cerium-based catalyst obtained in this example is marked as CeO2-2 / kaolin-3.
[0134] Embodiment 25
[0135] The preparation method of the cerium-based catalyst in this example is basically the same as that in Example 2, except that the calcination temperature in step 3) is 400° C. The cerium-based catalyst obtained in this example is marked as CeO2-2 / kaolin-4.
[0136] Embodiment 26
[0137] The preparation method of the cerium-based catalyst in this example is basically the same as that in Example 2, except that the calcination temperature in step 3) is 800° C. The cerium-based catalyst obtained in this example is marked as CeO2-2 / kaolin-5.
[0138] Embodiment 27
[0139] The preparation method of the cerium-based catalyst in this example is basically the same as that in Example 2, except that the calcination time in step 3) is 1 h, and the cerium-based catalyst obtained in this example is marked as CeO2-2 / kaolin-6.
[0140] Embodiment 28
[0141] The preparation method of the cerium-based catalyst in this example is basically the same as that in Example 2, except that the calcination time in step 3) is 8 hours, and the cerium-based catalyst obtained in this example is marked as CeO2-2 / kaolin-7.
[0142] Embodiment 29
[0143] The preparation method of the cerium-based catalyst in this embodiment is basically the same as that in Example 2, except that: the metal salt solution in step 1) is a mixed solution of cerium nitrate and zirconium nitrate, the molar ratio of cerium nitrate to zirconium nitrate is 1:1, and the metal salt concentration is 0.4 mol / L. The cerium-based catalyst obtained in this embodiment is marked as Ce 0.5 Zr 0.5 O2 / kaolin-1.
[0144] Embodiment 30
[0145] The preparation method of the cerium-based catalyst in this embodiment is basically the same as that in Example 2, except that: the metal salt solution in step 1) is a mixed solution of cerium nitrate and zinc nitrate, the molar ratio of cerium nitrate to zinc nitrate is 1:1, and the metal salt concentration is 0.4 mol / L. The cerium-based catalyst obtained in this embodiment is marked as Ce 0.5 Zn 0.5 O2 / kaolin-1.
[0146] Embodiment 31
[0147] The preparation method of the cerium-based catalyst in this embodiment is basically the same as that in Example 2, except that: the metal salt solution in step 1) is a mixed solution of cerium nitrate and copper nitrate, the molar ratio of cerium nitrate to copper nitrate is 1:1, and the metal salt concentration is 0.4 mol / L. The cerium-based catalyst obtained in this embodiment is marked as Ce 0.5 Cu 0.5 O2 / kaolin-1.
[0148] Embodiment 32
[0149] The preparation method of the cerium-based catalyst in this embodiment is basically the same as that in Example 2, except that the molar ratio of cerium nitrate to zirconium nitrate is 9:1. The cerium-based catalyst obtained in this embodiment is marked as Ce. 0.9 Zr 0.1 O2 / kaolin-1 catalyst.
[0150] Embodiment 33
[0151] The preparation method of the cerium-based catalyst in this example is basically the same as that in Example 29, except that the molar ratio of cerium nitrate to zirconium nitrate is 1:9, and the cerium-based catalyst obtained in this example is marked as Ce. 0.1 Zr 0.9 O2 / kaolin-1 catalyst.
[0152] Embodiment 34
[0153] This embodiment provides a method for synthesizing dimethyl carbonate using a cerium-based catalyst, comprising the following steps:
[0154] The Ce prepared in Example 32 0.9 Zr 0.1 O2 / kaolin-1 catalyst and methanol were added to the reactor, and carbon dioxide was introduced. The mass of methanol was controlled to be 10 times the mass of the cerium-based catalyst. The reaction temperature was 140°C and the CO2 pressure was 5MPa.
[0155] Embodiment 35
[0156] This embodiment provides a method for synthesizing dimethyl carbonate using a cerium-based catalyst, comprising the following steps:
[0157] The Ce prepared in Example 32 0.9 Zr 0.1 O2 / kaolin-1 catalyst and methanol were added to the reactor, and carbon dioxide was introduced. The mass of methanol was controlled to be 5 times the mass of the cerium-based catalyst. The reaction temperature was 140°C and the CO2 pressure was 5MPa.
[0158] Embodiment 36
[0159] This embodiment provides a method for synthesizing dimethyl carbonate using a cerium-based catalyst, comprising the following steps:
[0160] The Ce prepared in Example 32 0.9 Zr 0.1 O2 / kaolin-1 catalyst and methanol were added to the reactor, and carbon dioxide was introduced. The mass of methanol was controlled to be 15 times the mass of the cerium-based catalyst. The reaction temperature was 140°C and the CO2 pressure was 5MPa.
[0161] Embodiment 37
[0162] This embodiment provides a method for synthesizing dimethyl carbonate using a cerium-based catalyst, comprising the following steps:
[0163] The Ce prepared in Example 32 0.9 Zr 0.1 O2 / kaolin-1 catalyst and methanol were added to the reactor, and carbon dioxide was introduced. The mass of methanol was controlled to be 15 times the mass of the cerium-based catalyst. The reaction temperature was 100°C and the CO2 pressure was 5MPa.
[0164] Embodiment 38
[0165] This embodiment provides a method for synthesizing dimethyl carbonate using a cerium-based catalyst, comprising the following steps:
[0166] The Ce prepared in Example 32 0.9 Zr 0.1 O2 / kaolin-1 catalyst and methanol were added to the reactor, and carbon dioxide was introduced. The mass of methanol was controlled to be 15 times the mass of the cerium-based catalyst. The reaction temperature was 160°C and the CO2 pressure was 5MPa.
[0167] Embodiment 39
[0168] This embodiment provides a method for synthesizing dimethyl carbonate using a cerium-based catalyst, comprising the following steps:
[0169] The Ce prepared in Example 32 0.9 Zr 0.1 O2 / kaolin-1 catalyst and methanol were added to the reactor, and carbon dioxide was introduced. The mass of methanol was controlled to be 15 times the mass of the cerium-based catalyst. The reaction temperature was 160°C and the CO2 pressure was 2MPa.
[0170] Embodiment 40
[0171] This embodiment provides a method for synthesizing dimethyl carbonate using a cerium-based catalyst, comprising the following steps:
[0172] The Ce prepared in Example 32 0.9 Zr0.1 O2 / kaolin-1 catalyst and methanol were added to the reactor, and carbon dioxide was introduced. The mass of methanol was controlled to be 15 times the mass of the cerium-based catalyst. The reaction temperature was 160°C and the CO2 pressure was 6MPa.
[0173] Comparative Example 1
[0174] The method of the cerium-based catalyst in this comparative example comprises the following steps:
[0175] 1) dissolving cerium nitrate in deionized water to prepare a salt solution with a metal salt concentration of 0.4 mol / L; dissolving sodium hydroxide in deionized water to prepare an alkaline solution with an inorganic base concentration of 5 mol / L; under continuous stirring, adding the salt solution dropwise to the alkaline solution, wherein the amount of sodium hydroxide in the alkaline solution is 20 times the amount of cerium nitrate in the salt solution; after the addition is completed, stirring and aging are continued for 30 minutes to obtain a precursor suspension;
[0176] 2) heating the suspension at 150° C. to rapidly reflux;
[0177] 3) Separating a CeO2 precursor from the suspension, washing to neutrality, and drying to obtain a precursor powder; calcining the precursor powder at 600°C for 5 hours, and grinding to obtain a cerium-based catalyst, which is marked as a CeO2 catalyst.
[0178] The relevant data of the catalysts prepared in Examples 1 to 33 and Comparative Example 1 are shown in Table 1, and the relevant data of the reaction process for preparing dimethyl carbonate in Examples 34 to 40 are shown in Table 2.
[0179] Table 1 Data of catalysts prepared in Examples 1 to 33 and Comparative Example 1
[0180]
[0181]
[0182] The following conclusions can be drawn from Table 1:
[0183] 1) It can be seen from Examples 1 to 33 and Comparative Example 1 that the cerium-based catalyst introduced with a porous carrier can effectively improve the raw material conversion rate and product selectivity, and improve the yield. The inventors speculate that the porous carrier can be used as a solid dehydrating agent to remove the water generated in the reaction, thereby promoting the forward reaction and improving the methanol conversion rate and dimethyl carbonate yield.
[0184] 2) By comparing Examples 1 to 3, it can be seen that the cerium-based catalysts prepared using metal salt solutions of different concentrations all have good catalytic performance; when the concentration of the metal salt solution is 0.4 mol / L, the catalyst performance is the best and the yield of dimethyl carbonate is the highest.
[0185] 3) By comparing Examples 2, 4 and 5, it can be seen that the cerium-based catalysts prepared using inorganic alkali solutions of different concentrations all have good catalytic performance; when the concentration of the inorganic alkali solution is 5 mol / L, the catalyst performance is the best and the yield of dimethyl carbonate is the highest.
[0186] 4) By comparing Examples 2, 6 and 7, it can be seen that the cerium-based catalysts prepared using different molar amounts of inorganic bases all have good catalytic performance; when the molar amount of the inorganic base is 20 times the molar amount of the metal salt, the catalyst performance is optimal and the yield of dimethyl carbonate is the highest.
[0187] 5) By comparing Examples 2, 8 and 9, it can be seen that the cerium-based catalysts prepared using different heating reflux temperatures all have good catalytic performance; when the reflux heating temperature is 150°C, the catalyst performance is optimal and the dimethyl carbonate yield is the highest.
[0188] 6) By comparing Examples 2, 10 and 11, it can be seen that the cerium-based catalysts prepared by adding the porous carrier at different reflux times all have good catalytic performance; when the porous carrier is added 30 minutes after the start of reflux, the catalyst performance is the best and the dimethyl carbonate yield is the highest.
[0189] 7) By comparing Examples 2 and 12 to 15, it can be seen that the cerium-based catalysts prepared using alkaline solutions with different inorganic base compositions all have good catalytic performance; when the inorganic base is composed of sodium hydroxide, the catalyst performance is the highest and the yield of dimethyl carbonate is the highest.
[0190] 8) By comparing Examples 2 and 16 to 22, it can be seen that different types of porous carriers have different effects on catalyst performance. A suitable porous carrier can effectively disperse the active components and adsorb the water generated by the reaction, thereby improving the methanol conversion rate. When kaolin is used as a porous carrier, the catalyst performance is optimal and the dimethyl carbonate yield is the highest.
[0191] 9) By comparing Examples 2, 23 and 24, it can be seen that the cerium-based catalysts prepared using different porous carrier masses all have good catalytic performance; when the mass of the porous carrier is 4 times the mass of the metal salt, the catalyst performance is optimal and the dimethyl carbonate yield is the highest.
[0192] 10) By comparing Examples 2, 25 and 26, it can be seen that the cerium-based catalysts prepared at different calcination temperatures all have good catalytic performance; when the calcination temperature is 600°C, the catalyst performance is the best and the dimethyl carbonate yield is the highest.
[0193] 11) By comparing Examples 2, 27 and 28, it can be seen that the cerium-based catalysts prepared using different calcination times all have good catalytic performance; when the calcination time is 5 h, the catalyst performance is the best and the dimethyl carbonate yield is the highest.
[0194] 12) By comparing Examples 2, 29, 30 and 31, it can be seen that zirconium, zinc and copper can be added to cerium oxide to form a bimetallic cerium-based oxide; when the cerium-based oxide is composed of cerium and zirconium bimetallic, the catalyst performance is optimal and the yield of dimethyl carbonate is the highest.
[0195] 13) By comparing Examples 29, 32 and 33, it can be seen that when the molar ratio of cerium nitrate to zirconium nitrate in the bimetallic salt solution is 9:1, the catalyst performance is optimal and the yield of dimethyl carbonate is the highest.
[0196] Table 2 Relevant data during the reaction of preparing dimethyl carbonate in Examples 34 to 40
[0197]
[0198]
[0199] The following conclusions can be drawn from Table 2:
[0200] 1) By comparing Examples 34 to 36, it can be seen that different mass ratios of methanol to cerium-based catalysts all have good dimethyl carbonate yields; when the mass of methanol is 10 times the mass of the cerium-based catalyst, the dimethyl carbonate yield is the highest.
[0201] 2) By comparing Examples 34, 37 and 38, it can be seen that different reaction temperatures all have good dimethyl carbonate yields; when the reaction temperature is 140°C, the dimethyl carbonate yield is the highest.
[0202] 2) By comparing Examples 34, 39 and 40, it can be seen that different CO2 pressures all have good dimethyl carbonate yields; when the CO2 pressure is 5 MPa, the dimethyl carbonate yield is the highest.
[0203] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a cerium-based catalyst, characterized in that: The steps include: 1) mixing a metal salt solution containing a cerium salt with an inorganic alkali solution, and performing a first stirring and aging treatment to obtain a precursor suspension; 2) heating the precursor suspension under reflux at 100-170° C., adding a porous carrier, and performing a second stirring aging treatment to obtain a carrier loaded with the precursor; 3) washing, drying and calcining the carrier carrying the precursor to obtain the cerium-based catalyst.
2. The preparation method according to claim 1, characterized in that: The metal salt solution also includes at least one of a zirconium salt, a zinc salt and a copper salt; And / or, the inorganic base in the inorganic base solution includes at least one of sodium hydroxide, potassium hydroxide and ammonia water; And / or, the porous carrier includes at least one of kaolin, bentonite, diatomaceous earth, MCM-41 molecular sieve, NaY molecular sieve, all-silicon ZSM-5 molecular sieve, Beta molecular sieve and USY molecular sieve.
3. The preparation method according to claim 1 or 2, characterized in that: The concentration of the metal salt solution is 0.2-0.8 mol / L; And / or, the concentration of the inorganic alkali solution is 1-8 mol / L.
4. The preparation method according to any one of claims 1 to 3, characterized in that: The molar ratio of the inorganic base in the inorganic base solution to the metal salt in the metal salt solution is 5 to 30.
5. The preparation method according to any one of claims 1 to 4, characterized in that: The mass ratio of the porous carrier to the metal salt in the metal salt solution is 3-5.
6. The preparation method according to any one of claims 1 to 5, characterized in that: In step 2), the porous carrier is added after the precursor suspension is refluxed for 5 to 90 minutes.
7. The preparation method according to any one of claims 1 to 6, characterized in that: The calcination temperature is 400-800° C., and the calcination time is 1-8 hours.
8. A cerium-based catalyst, characterized in that Obtained according to the preparation method according to any one of claims 1 to 7.
9. A method for preparing dimethyl carbonate, characterized in that: The steps include: The catalyst obtained by the preparation method according to any one of claims 1 to 7 or the catalyst according to claim 8 is mixed with methanol, and carbon dioxide is introduced to obtain dimethyl carbonate.
10. The method according to claim 9, characterized in that The mass ratio of methanol to catalyst is 5 to 15; and / or, the reaction temperature is 100 to 160° C.; And / or, the reaction pressure is 2 to 6 MPa.
Citation Information
Cited By
Method for selectively recovering rare earth La and Ce in waste polishing powder and regenerating CeO2-based catalyst by coupling mechanochemical deconstruction with aluminum salt leaching
CN120006117A