Catalyst for dehydrogenation of liquid organic hydrogen energy carrier and preparation method thereof
By performing ascorbic acid reduction treatment and Pt ion in situ anchoring on Ce-Mg-Al hydrotalcite, Pt/CeO2-MgO-Al2O3 catalyst is formed, which solves the problem of insufficient dispersion of active components in the prior art and improves detachment The activity and stability of hydrogen catalysts reduce production costs and achieve efficient hydrogen release.
Patent Information
- Application Number
- CN202411104426.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-12
AI Technical Summary
The existing liquid organic hydrogen energy carrier dehydrogenation catalysts have problems such as insufficient dispersion of active components, low utilization rate and low activity. In particular, the dispersion method of Pt particles has not been effectively solved, resulting in high hydrogen storage costs.
Ce-Mg-Al hydrotalcite is used as a support to form Ce3+ by ascorbic acid reduction treatment, and the Pt ions are anchored in situ using its oxygen vacant position to form a Pt/CeO2-MgO-Al2O3 catalyst, which significantly improves the dispersion and metal of Pt - Carrier interaction, inhibiting the aggregation and loss of active components.
It significantly improves the dehydrogenation activity and stability of the catalyst, reduces the amount of precious metals, and achieves efficient hydrogen release rate and good industrial application prospects.
Smart Images

Figure CN118925718A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of chemical hydrogen storage, and in particular relates to a method for preparing a dehydrogenation catalyst for a liquid organic hydrogen energy carrier. Background Art
[0002] Fossil energy is one of the main sources of energy in the world and plays an important role in the economic development and scientific and technological progress of many countries and regions. However, the large-scale exploitation and utilization of fossil energy have brought about increasingly serious environmental pollution, climate change and other problems. Therefore, developing clean energy and improving energy utilization efficiency, and gradually reducing dependence on fossil energy have become the trend and direction of development in the global energy field today. With the development of hydrogen production technology, hydrogen energy, as a clean energy source with abundant and renewable sources, has attracted much attention. However, due to the large volume of hydrogen, in order to store enough hydrogen, it is necessary to find a carrier with high hydrogen storage density. Currently, commonly used hydrogen storage methods include compressed hydrogen, liquid hydrogen and solid hydrogen, but their hydrogen storage density is not ideal, resulting in high hydrogen storage costs and limited use. Organic liquid hydrogen storage is a new type of hydrogen storage technology. Its basic principle is to react hydrogen with organic liquid to form a liquid organic hydrogen energy carrier, thereby realizing the storage and transportation of hydrogen. When hydrogen is needed, the liquid organic hydrogen energy carrier can release hydrogen through dehydrogenation reaction. The difficulty of this technology lies in how to achieve rapid dehydrogenation. The key to solving this problem lies in the development of efficient dehydrogenation catalysts and their simple preparation processes.
[0003] There are many types of dehydrogenation catalysts, including platinum, iridium, molybdenum, iron, cobalt, nickel and other metals and their supported catalysts [Documents ACS Energy Lett. 2022, 7, 3734, CN115106120A and CN114797912A], and their preparation methods mainly include impregnation loading method, coprecipitation method, sol-gel method, physical mixing method, etc., among which impregnation loading method is the most commonly used method [CN115703064A]. These preparation methods are difficult to achieve uniform and highly dispersed active components on the carrier, and it is inevitable that some active components will agglomerate together, and some active components will be lost during the reaction. In order to further improve the dehydrogenation activity of the catalyst, the previous studies mainly adopted measures such as optimizing the catalyst preparation method and process conditions, regulating the size and morphology of the catalyst particles, and improving the carrier and its acidity and alkalinity. For example, in CN106622228A, in order to inhibit the carbon deposition and deactivation of the catalyst, alkaline MgO was introduced into the Al2O3 carrier to improve the stability of the catalyst, but the catalyst needs to be loaded with a higher Pt to obtain a higher hydrogen production rate; CN 114797850 A discloses a cyclohexane dehydrogenation catalyst and its preparation method and application, using activated carbon as a carrier to prepare a Pt-aid / carbon dehydrogenation catalyst. The literature [C hin J Chem Eng 2020, 28, 2337] reported that the decrease in the dehydrogenation activity of the catalyst was mainly due to the agglomeration of the active components during the reaction, resulting in an increase in the particle size and a decrease in the number of active sites. CN109331823A uses an alkali precipitation method to prepare a Ce-doped Mg-Al hydrotalcite containing Pt in one step, and then obtains the target catalyst by roasting and hydrogen reduction. However, these preparation methods do not fundamentally solve the dispersion problem of Pt particles, and there are still problems such as insufficient dispersion of active components, low utilization rate, and low activity. Summary of the invention
[0004] Therefore, in order to reduce the usage of active components and improve the activity of the catalyst, the present invention discloses a catalyst for dehydrogenation of a liquid organic hydrogen energy carrier and a preparation method thereof.
[0005] The preparation method comprises the following steps: using Ce-Mg-Al hydrotalcite as a carrier precursor, reducing the Ce-Mg-Al hydrotalcite with ascorbic acid before calcining the Ce-Mg-Al hydrotalcite, so that more Ce 3+ , and then the Pt / CeO2-MgO-Al2O3 catalyst was prepared by in-situ Pt ion anchoring, filtration, calcination and hydrogen reduction.
[0006] This method mainly uses ascorbic acid to convert Ce in Ce(OH)4 4+ Reduction to Ce 3+, and then use its selective adsorption and reducibility to anchor the active component Pt on the oxygen vacancies, significantly improving the dispersion of Pt, and Pt and CeO2 can form a strong metal-support interaction, inhibiting the agglomeration of the active component during the preparation process and the loss of the active component during the reaction process. The operation method is simple and easy, and the obtained catalyst shows excellent catalytic activity and stability in the dehydrogenation reaction of liquid organic hydrogen energy carriers, and has good industrial application prospects.
[0007] The preparation method of the liquid organic hydrogen energy carrier dehydrogenation catalyst of the present invention firstly creates vacancies on the carrier precursor, and reduces the vacancies with ascorbic acid to make part of Ce 4+ Restore to Ce 3+ Defective oxygen vacancies are generated, and then the active components are anchored in situ on the oxygen vacancies by utilizing the adsorption and reducibility of the oxygen vacancies, promoting the formation of a strong metal-carrier interaction, effectively improving the dispersion of the active components and playing the role of catalytic active centers. The inventive method is simple and easy to implement, can significantly improve the utilization rate of metal components and inhibit the agglomeration of active components during catalyst preparation, i.e., the reaction process. The obtained catalyst exhibits excellent hydrogen release rate and stability in the dehydrogenation reaction of organic hydrogen carrier cycloalkanes.
[0008] Further, the reduction treatment of Ce-Mg-Al hydrotalcite with ascorbic acid includes stirring the uncalcined Ce-Mg-Al hydrotalcite in ascorbic acid for reaction, the ascorbic acid is preferably used in the form of a solution, such as a 1-10 mmol / L aqueous solution, preferably a 2-5 mmol / L aqueous solution, and the ascorbic acid is added at a mass ratio of ascorbic acid to Ce-Mg-Al hydrotalcite of 0.02-1:1, preferably 0.05-0.3:1, more preferably 0.1-0.25:1. The ascorbic acid treatment reduces part of the Ce-Mg-Al hydrotalcite. 4+ Restore to Ce 3+ , which is conducive to the adsorption of Pt ions.
[0009] Furthermore, the reduction treatment temperature is 5-60°C, preferably 10-50°C, more preferably 15-45°C, more preferably 20-30°C, for example 25°C, and the reduction time is more than 0.5 h, for example 0.5-10 hours, preferably 0.5-6 h, and the treated carrier is rich in oxygen vacancies.
[0010] Furthermore, the oxygen vacancy characteristics are utilized to adsorb Pt ions, and then an oxidation-reduction reaction immediately occurs to anchor Pt on the support.
[0011] Further, the in-situ anchoring of Pt ions includes adding the reduced hydrotalcite-like substance to a Pt salt (preferably a soluble Pt salt) solution, such as a chloroplatinic acid acetone solution, and standing at a temperature of 0 to 60 °C for more than 0.5 h, such as 0.5 to 12 h, preferably 0.5 to 4 h. The concentration of the platinum salt is generally 0.001-0.05 g / mL, preferably 0.005-0.02 g / mL. The loading amount of Pt in the catalyst is regulated by controlling the amount of chloroplatinic acid acetone solution added, which is generally 0.1 to 0.5 wt%, preferably 0.3 to 0.4 wt%, that is, 0.3 to 2 mL of chloroplatinic acid acetone solution is added to 20 mL of acetone, preferably 0.4 to 1.5 mL.
[0012] Furthermore, the calcination temperature is 300-600°C, preferably 350-550°C, and the calcination time is 1-6 h, preferably 2-5 h.
[0013] Furthermore, the hydrogen reduction comprises reducing the calcined catalyst precursor in a hydrogen atmosphere at a reduction temperature of 200-550°C, preferably 250-500°C, preferably 300-500°C, and a reduction time of more than 1 h, such as 1-10 h, preferably 1-5 h.
[0014] Preferably, the Ce-Mg-Al type hydrotalcite is prepared by a co-precipitation method, comprising the following steps: (1) Add soluble aluminum salt, magnesium salt and cerium salt into water, preferably deionized water, to prepare a metal salt mixed solution A, and then prepare an alkali solution B. Under stirring conditions, the mixed solution A and B are simultaneously added dropwise to a flask. When the pH value of the suspension reaches a range of 9.5 to 10.5, the addition is stopped, and the reaction is continued for more than 0.5 h, preferably 0.5 to 2 h; (2) The suspension obtained in step (1) is transferred into a hydrothermal reactor and crystallized at 90-110°C (preferably 95-105°C) for more than 10 h, for example, 10-24 h, preferably 10-15 h. The obtained precipitate is separated, washed and dried to obtain Ce-Mg-Al hydrotalcite.
[0015] Furthermore, the soluble aluminum salt is one or more of aluminum sulfate, aluminum nitrate or aluminum chloride.
[0016] Furthermore, the soluble magnesium salt is one or more of magnesium sulfate, magnesium nitrate or magnesium chloride, wherein Mg 2+ / Al 3+ The molar ratio is 1.
[0017] Furthermore, the soluble cerium salt is one or both of cerium nitrate and cerium chloride.
[0018] Among them, Ce 3+ / Mg2+ / Al 3+ The molar ratio is 0.01-0.50:0.5-10:1, preferably 0.03-0.40:0.8-5:1, more preferably 0.05-0.30:1-4:1, more preferably 0.10-0.25:2-3:1.
[0019] The alkali solution B can be a sodium hydroxide solution, a potassium hydroxide solution, or a mixed solution of sodium hydroxide and sodium carbonate. Preferably, the alkali solution B is a mixed alkali solution of sodium hydroxide and sodium carbonate. The mass ratio of sodium hydroxide to sodium carbonate can be 2-10:1, preferably 5-8:1, and the concentration of the alkali solution can be 1-30wt%, preferably 2-10wt%.
[0020] The drying can be carried out in an oven at 80-130° C. for 1-24 h, preferably at 100-120° C. for 2-12 h, for example 10 h.
[0021] The present invention further relates to a dehydrogenation catalyst for a liquid organic hydrogen energy carrier prepared by the above method.
[0022] The present invention also relates to the use of the above-mentioned catalyst for dehydrogenation of liquid organic hydrogen energy carrier in the dehydrogenation reaction of liquid organic hydrogen energy carrier, wherein the organic hydrogen energy carrier is cyclohexane, methylcyclohexane, ethylcyclohexane or decalin.
[0023] The beneficial effects of the present invention are: The catalyst preparation method of the present invention uses ascorbic acid to innovatively perform reduction treatment on Ce-Mg-Al hydrotalcite before calcination, thereby forming more Ce on the surface of Ce-Mg-Al hydrotalcite. 3+ , and then utilize the adsorption and reduction characteristics of unsaturated sites to anchor Pt on the carrier, and use filtration to separate the precipitate. The excess or unanchored Pt ions remain in the solution. Compared with the reduction treatment after calcination of Ce-Mg-Al hydrotalcite, the use of precious metals is significantly reduced, the production cost is effectively reduced, and the dispersion of Pt and the formation of strong metal-carrier interaction are promoted. The obtained catalyst exhibits excellent dehydrogenation activity and stability in the dehydrogenation reaction of cycloalkanes. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 The present invention is a flow chart of the preparation process of the Pt / CeO2-MgO-Al2O3 catalyst.
[0025] Figure 2 TEM image (a) and HR-TEM image (b) of the Pt / CeO2-MgO-Al2O3 catalyst of Example 1. DETAILED DESCRIPTION
[0026] The present invention is illustrated in detail by the following examples.
[0027] The reagents used in the examples were all analytically pure and the water was ultrapure water. Preparation Example 1
[0028] Weigh 9.4 g of aluminum nitrate and press Al 3+ / Mg 2+ / Ce 3+ The molar ratio is 5:15:1. A certain amount of magnesium nitrate and cerium nitrate are weighed and dissolved in 200 mL of deionized water to prepare a metal salt mixed solution A; 12.0 g of NaOH and 2.0 g of anhydrous Na2CO3 are weighed and dissolved in 250 mL of deionized water to prepare an alkali mixed solution B. At room temperature and vigorous stirring, the metal salt mixed solution A and the alkali mixed solution B are simultaneously dripped into a three-necked flask at a rate of 4 mL / min using a constant pressure titration funnel, and the pH value of the suspension in the three-necked flask is controlled within the range of 9.5-10.5. The addition of the alkali mixed solution B is stopped, and the reaction is continued for 30 min. The suspension is transferred to a hydrothermal reactor and crystallized at 95 °C for 10 h. The suspension is then filtered, and the filtered solid is washed and dried to obtain Ce-Mg-Al hydrotalcite. Preparation Example 2
[0029] According to the preparation process of hydrotalcite in Preparation Example 1, only Al 3+ / Mg 2+ / Ce 3+ The molar ratio was adjusted to 20:20:1. Preparation Example 3
[0030] According to the preparation process of hydrotalcite in Preparation Example 1, only Al 3+ / Mg 2+ / Ce 3+ The molar ratio was adjusted to 5:20:1. Preparation Example 4
[0031] According to the preparation process of hydrotalcite in Preparation Example 1, only Al 3+ / Mg 2+ / Ce 3+ The molar ratio was adjusted to 10:30:3. Example 1
[0032] Weigh 1 g of the Ce-Mg-Al hydrotalcite obtained in Preparation Example 1, add 3 mmol / L ascorbic acid solution at a mass ratio of ascorbic acid / Ce-Mg-Al hydrotalcite of 0.15, stir the mixture at room temperature 25 °C for 2 h, and then filter to obtain Ce-Mg-Al hydrotalcite rich in oxygen vacancies. Then add the hydrotalcite to 20 mL of acetone, and add 1 mL of chloroplatinic acid acetone solution (concentration of 0.01 g / mL). After standing at room temperature 25 °C for 3 h, the filtered solid is dried at 200 °C for 4 h, and then calcined at 500 °C for 4 h to obtain a catalyst precursor (loading amount of 0.38 wt%).
[0033] 0.5 g of the above catalyst precursor was weighed and filled into a fixed bed reaction tube. It was reduced in a hydrogen atmosphere at 350 °C for 4 h, and then the hydrogen was stopped and methylcyclohexane was introduced instead for dehydrogenation performance test. The feed flow rate was 0.1 mL / min. Chromatographic analysis showed that the conversion rate was 99.5% and the selectivity for toluene was 99.9%. After 12 h of continuous reaction, the dehydrogenation activity did not change. Example 2
[0034] Weigh 1 g of the Ce-Mg-Al hydrotalcite obtained in Preparation Example 1, add 5 mmol / L ascorbic acid solution at a mass ratio of ascorbic acid / Ce-Mg-Al hydrotalcite of 0.05, stir the reaction at 60 °C for 0.5 h, and then filter to obtain Ce-Mg-Al hydrotalcite rich in oxygen vacancies. Then add the hydrotalcite to 20 mL of acetone, and add 1.8 mL of chloroplatinic acid acetone solution (concentration of 0.005 g / mL). After standing at 0 °C for 4 h, the filtered solid is dried at 200 °C for 4 h, and then calcined at 600 °C for 1 h to obtain a catalyst precursor (loading of 0.34 wt%).
[0035] 0.5 g of the above catalyst precursor was weighed and filled into a fixed bed reaction tube. It was reduced in a hydrogen atmosphere at 500 °C for 1 h, and then the hydrogen was stopped and methylcyclohexane was introduced instead for dehydrogenation performance test. The feed flow rate was 0.1 mL / min. Chromatographic analysis showed that the conversion rate was 90.1% and the selectivity for toluene was 99.9%. After 15 h of continuous reaction, the dehydrogenation activity did not change. Example 3
[0036] Weigh 1 g of the Ce-Mg-Al hydrotalcite obtained in Preparation Example 1, add 2 mmol / L ascorbic acid solution at a mass ratio of ascorbic acid / Ce-Mg-Al hydrotalcite of 0.3, stir the mixture at 5 °C for 6 h, and then filter to obtain Ce-Mg-Al hydrotalcite rich in oxygen vacancies. Then add the hydrotalcite to 20 mL of acetone, and add 0.7 mL of chloroplatinic acid acetone solution (concentration of 0.015 g / mL). After standing at 60 °C for 0.5 h, the filtered solid is dried at 200 °C for 4 h, and then calcined at 300 °C for 6 h to obtain a catalyst precursor (loading of 0.4 wt%).
[0037] 0.5 g of the above catalyst precursor was weighed and filled into a fixed bed reaction tube. It was reduced in a hydrogen atmosphere at 350 °C for 4 h, and then the hydrogen was stopped and cyclohexane was introduced instead for dehydrogenation performance test. The feed flow rate was 0.1 mL / min. Chromatographic analysis showed that the conversion rate was 99.1% and the selectivity for benzene was 99.9%. After 18 h of continuous reaction, the dehydrogenation activity did not change. Example 4
[0038] Weigh 1 g of the Ce-Mg-Al hydrotalcite obtained in Preparation Example 1, add 2.5 mmol / L ascorbic acid solution at a mass ratio of ascorbic acid / Ce-Mg-Al hydrotalcite of 0.2, stir the mixture at 30 °C for 2 h, and then filter to obtain Ce-Mg-Al hydrotalcite rich in oxygen vacancies. Then add the hydrotalcite to 20 mL of acetone, and add 0.4 mL of chloroplatinic acid acetone solution (concentration of 0.02 g / mL). After standing at 40 °C for 2 h, the filtered solid is dried at 200 °C for 4 h, and then calcined at 500 °C for 4 h to obtain a catalyst precursor (loading amount of 0.3 wt%).
[0039] 0.5 g of the above catalyst precursor was weighed and filled into a fixed bed reaction tube. It was reduced in a hydrogen atmosphere at 250 °C for 5 h. Then the hydrogen was stopped and hexylcyclohexane was introduced instead for dehydrogenation performance test. The feed flow rate was 0.1 mL / min. Chromatographic analysis showed that the conversion rate was 74.1% and the selectivity of ethylbenzene was 99.9%. After 12 h of continuous reaction, the dehydrogenation activity did not change. Example 5
[0040] Weigh 1 g of the Ce-Mg-Al hydrotalcite obtained in Preparation Example 1, add 4 mmol / L ascorbic acid solution at a mass ratio of ascorbic acid / Ce-Mg-Al hydrotalcite of 0.1, stir the mixture at 40 °C for 2 h, and then filter to obtain Ce-Mg-Al hydrotalcite rich in oxygen vacancies. Then add the hydrotalcite to 20 mL of acetone, and add 0.8 mL of chloroplatinic acid acetone solution (concentration of 0.012 g / mL). After standing at 50 °C for 1.5 h, the filtered solid is dried at 200 °C for 4 h, and then calcined at 600 °C for 2 h to obtain a catalyst precursor (loading amount of 0.36 wt%).
[0041] 0.5 g of the above catalyst precursor was weighed and filled into a fixed bed reaction tube. It was reduced in a hydrogen atmosphere at 450 °C for 2 h, and then the hydrogen was stopped and decalin was introduced instead for dehydrogenation performance test. The feed flow rate was 0.1 mL / min. Chromatographic analysis showed that the conversion rate was 86.7% and the selectivity of biphenyl was 99.9%. After the reaction was continued for 12 h, the dehydrogenation activity did not change. Example 6
[0042] The same as Example 1, except that the hydrotalcite of Preparation Example 2 was used instead of the hydrotalcite of Preparation Example 1. Example 7
[0043] The same as Example 1, except that the hydrotalcite of Preparation Example 3 was used instead of the hydrotalcite of Preparation Example 1. Example 8
[0044] The same as Example 1, except that the hydrotalcite of Preparation Example 4 was used instead of the hydrotalcite of Preparation Example 1. Comparative Example 1
[0045] The same as Example 1, except that the Ce-Mg-Al hydrotalcite was first calcined at 600°C to convert it into Ce-Mg-Al oxide, and then treated with ascorbic acid, and the Ce-Mg-Al hydrotalcite was immersed in a 5 mmol / L ascorbic acid solution at 50°C for hydrothermal reaction for 4 h. Under the same reaction conditions, the conversion rate of methylcyclohexane was reduced to 80.7%. Comparative Example 2
[0046] The same as Example 1, except that the untreated hydrotalcite-like substance was not treated with ascorbic acid and was directly added to 20 mL of chloroplatinic acid solution. Under the same reaction conditions, the conversion rate of methylcyclohexane was reduced to 65.2%. Comparative Example 3
[0047] The same as Example 1, except that the same amount of sodium borohydride was used instead of ascorbic acid for reduction treatment. Under the same reaction conditions, the conversion rate of methylcyclohexane was reduced to 75.6%.
[0048] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the scope of protection of the invention.
Claims
1. A method for preparing a catalyst for dehydrogenation of a liquid organic hydrogen energy carrier, Features: The preparation method comprises: reducing uncalcined Ce-Mg-Al hydrotalcite with ascorbic acid, and then preparing Pt / CeO by in-situ anchoring of Pt ions, filtering, calcining and reducing with hydrogen. 2 -MgO-Al 2 O 3 catalyst.
2. The preparation method according to claim 1, It is characterized in that The ascorbic acid is added at a mass ratio of ascorbic acid to Ce-Mg-Al hydrotalcite of 0.05 to 0.3:1; and / or The reduction treatment of the Ce-Mg-Al type hydrotalcite by using ascorbic acid comprises stirring the Ce-Mg-Al type hydrotalcite in ascorbic acid for reaction.
3. The preparation method according to claim 1 or 2, It is characterized in that The ascorbic acid reduction treatment temperature is 5-60°C, and the reduction time is 0.5-6 h.
4. The preparation method according to any one of claims 1 to 3, It is characterized in that The in-situ anchoring of Pt ions comprises adding the reduced hydrotalcite-like substance into a Pt salt solution and leaving it to stand at a temperature of 0 to 60° C. for more than 0.5 h, such as 0.5 to 12 h, preferably 0.5 to 4 h.
5. The preparation method according to any one of claims 1 to 4, It is characterized in that The calcination temperature is 300-600°C, and the calcination time is 1-6 h.
6. The preparation method according to any one of claims 1 to 5, It is characterized in that The catalyst precursor is reduced in a hydrogen atmosphere at a reduction temperature of 250-500° C. for a reduction time of 1-5 h.
7. The preparation method according to any one of claims 1 to 6, It is characterized in that The Ce-Mg-Al hydrotalcite is prepared by a co-precipitation method, comprising the following steps: (1) Add soluble aluminum salt, magnesium salt and cerium salt into water, preferably deionized water, to prepare a metal salt mixed solution A, and then prepare an alkali solution B. Under stirring conditions, the mixed solution B is added dropwise to the mixed solution A. When the pH value of the suspension reaches a range of 9.5 to 10.5, the addition is stopped, and the reaction is continued for more than 0.5 h, preferably 0.5 to 2 h; (2) The suspension obtained in step (1) is transferred into a hydrothermal reactor and crystallized at 90-110° C. (preferably 95-105° C.) for more than 10 h, for example, 10-24 h, preferably 10-15 h. The obtained precipitate is separated, optionally washed, and dried to obtain Ce-Mg-Al hydrotalcite.
8. The preparation method according to claim 7, It is characterized in that The soluble aluminum salt is one or more of aluminum sulfate, aluminum nitrate or aluminum chloride; and / or The soluble magnesium salt is one or more of magnesium sulfate, magnesium nitrate or magnesium chloride; and / or The soluble cerium salt is one or both of cerium nitrate and cerium chloride; and / or Among them, Ce 3+ / Mg 2+ / Al 3+ The molar ratio is 0.01-0.50:0.5-10:1, preferably 0.03-0.40::0.8-5:1, more preferably 0.05-0.30: 1-4:1, more preferably 0.10-0.25:2-3:1; and / or The alkali solution B is a sodium hydroxide solution, a potassium hydroxide solution, or a mixed solution of sodium hydroxide and sodium carbonate. Preferably, the alkali solution B is a mixed alkali solution of sodium hydroxide and sodium carbonate, the mass ratio of sodium hydroxide to sodium carbonate is 2-10:1, preferably 5-8:1, and the concentration of the alkali solution can be 1-30wt%, preferably 2-10wt%.
9. A catalyst for dehydrogenation of a liquid organic hydrogen energy carrier obtained by the preparation method according to any one of claims 1 to 8.
10. Use of the catalyst for dehydrogenation of a liquid organic hydrogen energy carrier according to claim 9 for dehydrogenation of a liquid organic hydrogen energy carrier, wherein the liquid organic hydrogen energy carrier is cyclohexane, methylcyclohexane, ethylcyclohexane or decalin.
Citation Information
Patent Citations
Cycloalkane dehydrogenation catalyst, preparation method thereof and application
CN106622228A
Hydrocarbon dehydrogenation catalyst as well as preparation method and application thereof
CN109331823A
Aromatic nitro compound hydrogenation catalyst as well as preparation method and application thereof
CN118320819A
Cited By
Method for catalyzing dehydrogenation of methylcyclohexane by using composite catalyst
CN120887770A
A method for dehydrogenation of methylcyclohexane catalyzed by a composite catalyst
CN120887770B