Silver catalyst and preparation method and application thereof

By optimizing the ratio of the organic co-adjuvant and alkali metal additives of rhenium in the silver catalyst, the problem of insufficient activity and selectivity of silver catalysts in the prior art was solved, and a highly efficient silver catalyst was prepared, suitable for ethylene epoxy under high load conditions The chemical reaction significantly improves the performance of the catalyst.

CN118925723APending Publication Date: 2024-11-12CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310538767.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-12
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing silver catalysts have problems with insufficient activity and selectivity in ethylene epoxidation reaction, especially under high load conditions, and fail to effectively optimize the synergistic ratio between silver and additives, affecting the performance of the catalyst.

Method used

By using the organic co-adjuvant of rhenium and optimizing the load ratio between silver and alkali metal, alkali metal and organic co-adjuvant of rhenium and rhenium, a silver catalyst with high activity and selectivity is prepared. The specific steps include preparing the impregnation liquid And a catalyst is obtained through impregnation, leaching, heating and other processes.

Benefits of technology

It improves the activity and selectivity of the catalyst, and is especially suitable for ethylene epoxidation under high load conditions, breaking the previous limit of 85.7% selectivity of silver catalysts and significantly improving the performance of the catalyst.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention belongs to the technical field of silver catalysts, and discloses a silver catalyst and a preparation method and application thereof, and the preparation method comprises the following steps: preparing an impregnation liquid; impregnating the carrier with the impregnation liquid, and then leaching and heating to obtain the silver catalyst, the impregnation liquid comprises a silver-containing compound, an alkali metal auxiliary agent, a rhenium auxiliary agent and an organic co-auxiliary agent of rhenium, and the raw materials for preparing the impregnation liquid enable the content of silver in the prepared silver catalyst to be 15-36wt% based on the total weight of the silver catalyst; in terms of metal, the molar ratio of silver to alkali metal in the auxiliary components in the silver catalyst is 150-800 / 1, preferably 200-650 / 1; the molar ratio of the alkali metal to the rhenium is (0.5-10): 1, preferably (1.0-8.0): 1; the molar ratio of the rhenium to the metal elements of the organic co-additive of rhenium is (5-50): 1, preferably (10-40): 1. The silver catalyst prepared by the method provided by the invention has high activity and selectivity, and is especially suitable for a reaction device for producing ethylene oxide by ethylene epoxidation with high load.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of silver catalysts, and more specifically, to a silver catalyst and a preparation method and application thereof. Background Art

[0002] EO / EG is mainly produced through ethylene epoxidation reaction, and silver catalyst is the core catalyst for producing ethylene oxide / ethylene glycol.

[0003] Silver catalyst is a catalyst used in industry for the production of ethylene oxide (EO) by epoxidation of ethylene. Shell, Dow Chemical (UCC), SD and Sinopec have conducted extensive research on silver catalysts. The current market is dominated by high-selectivity and high-efficiency silver catalysts suitable for high space-time yields, with a demand ratio of more than 99%. Ethylene epoxidation under the action of silver catalysts mainly produces ethylene oxide (EO), while carbon dioxide and water are produced as side reactions. Among them, activity, selectivity and stability are the main performance indicators of silver catalysts. Activity refers to the reaction temperature required when the ethylene oxide production process reaches a certain reaction load. The lower the reaction temperature, the higher the activity of the catalyst; selectivity refers to the ratio of the number of moles of ethylene converted into ethylene oxide in the reaction to the total number of moles of ethylene in the reaction; stability is expressed as the rate of decrease of activity and selectivity. The smaller the rate of decrease, the better the stability of the catalyst. The performance of silver catalysts is not only related to the performance of the carrier used and its preparation method, but also to the composition and preparation method of the catalyst.

[0004] From the perspective of catalyst composition, the active component is metallic silver, and additives are added to improve the selectivity of the product. Patents for the addition of additives have basically covered all elements in the periodic table. However, the additive components of silver catalysts mainly include alkali metals, alkaline earth metals, rare earth metals and precious metals, and the composition of different types of catalysts is also different. One of the more important additives is alkali metals. Literature reports that it can make the silver particles more evenly distributed on the carrier, and can promote the formation of electrophilic oxygen and ethylene epoxidation transition state oxygen heterometallic ring (OMC); there are also literatures introducing that alkali metals can make silver generate more lattice defects on the carrier surface, which is easy to adsorb subsurface oxygen and then generate EO. USP6762311 alkali metals are preferably added in the form of hydroxides, and USP6815395 alkali metals are preferably added in the form of nitrates, and the catalyst performance is improved by impregnating different alumina carriers.

[0005] Another very important additive is rhenium. The difference between high-activity catalysts and medium / high-selectivity and high-efficiency silver catalysts is that the latter catalysts contain rhenium additives, which significantly improves the selectivity of the catalysts. USP 4761394 first reported the use of rhenium (Re) as an additive in silver catalysts. USP4548921 describes the role of rhenium additives in silver catalysts. Re exists as uniformly dispersed metal particles on the carrier, and the active component silver is loaded on the outer surface of rhenium to improve the performance of the silver catalyst. There are also literatures that believe that the rhenium additive competes with the adsorbed oxygen on the catalyst surface and attracts electrons in the silver lattice, resulting in a decrease in the electron density of the adsorbed oxygen and an increase in the selectivity of the product EO. USP7259129 rhenium additives can be added in the form of chlorides, rhenates and perrhenates. CN201010622856.4 and CN201010534019.6 rhenium additives are inorganic compounds containing rhenium, such as perrhenic acid, perrhenates, or mixtures thereof.

[0006] As a co-promoter of the rhenium promoter, it can keep the rhenium promoter at a higher valence state and ensure that the catalyst has a higher selectivity. U.S. Patent 7538235 describes that the co-promoter of the rhenium promoter includes one or more compounds containing tungsten, chromium, molybdenum, and sulfur, preferably a tungsten compound. The co-promoters added in the patent literature are mostly inorganic compounds, and there are basically no reports on organic co-promoters.

[0007] In addition, the loading amount of each auxiliary agent during the preparation of the impregnation solution and the ratio between silver and auxiliary agents and between different auxiliary agents also have an important influence on the synergistic effect and catalyst performance. The amount of alkali metal auxiliary agent added in US10865189 is 10-3000ppm, preferably 15-2000ppm, further preferably 20-1500ppm, and most preferably 50-1000ppm. BASF US2021 / 0046459 Al provides a catalyst for effectively converting ethylene oxidation into ethylene oxide, the catalyst composition comprising 20-45% silver by weight of the catalyst; the cesium loading C (Cs) per kilogram of catalyst is at least 2.0mmol; the rhenium loading C (Re) per kilogram of catalyst is at least 3.0mmol; the tungsten loading c (W) per kilogram of catalyst is at least 1.6mmol. Shell patent EP 3187493 B1 provides a catalyst for olefin epoxidation, which includes a carrier and silver, a rhenium promoter, a first co-promoter and a second co-promoter deposited on the carrier; the rhenium promoter is at least 1.5 mmole / kg and at most 10 mmole / kg relative to the weight of the catalyst in terms of element; the molar ratio of the first co-promoter to the second co-promoter is greater than 1; the catalyst also contains a potassium promoter, and the potassium loading is at least 0.5 mmole / kg relative to the weight of the catalyst.

[0008] The generally accepted mechanism of ethylene epoxidation to produce ethylene oxide is the atomic oxygen mechanism, that is, ethylene reacts with atomic oxygen adsorbed on silver to generate the product ethylene oxide. The additive can adjust the amount and strength of oxygen adsorbed on silver, and thus affect the catalyst performance. The above reference introduces the preferred range of the loading amount of the additive in the catalyst, but does not limit the synergistic ratio between silver and each additive. Summary of the invention

[0009] The object of the present invention is to provide a silver catalyst and a preparation method and application thereof, by using an organic co-promoter of rhenium and optimizing the loading ratio between silver and alkali metal, alkali metal and rhenium, and rhenium and rhenium organic co-promoter metal elements, so that the prepared silver catalyst has better catalyst performance.

[0010] In order to achieve the above object, the first aspect of the present invention provides a method for preparing a silver catalyst, the preparation method comprising the following steps:

[0011] (1) preparing an impregnation solution;

[0012] (2) impregnating the carrier with the impregnation solution, and then leaching and heating to obtain the silver catalyst;

[0013] The impregnation solution comprises: a silver compound, an alkali metal additive, a rhenium additive and an organic co-additive of rhenium. The raw materials of the impregnation solution are prepared so that the silver content of the prepared silver catalyst is 15-36wt% based on the total weight of the silver catalyst; the molar ratio of silver to alkali metal in the silver catalyst is 150-800 / 1, preferably 200-650 / 1, the molar ratio of alkali metal to rhenium is 0.5-10 / 1, preferably 1.0-8.0 / 1; the molar ratio of rhenium to the metal element of the organic co-additive of rhenium is 5-50 / 1, preferably 10-40 / 1.

[0014] The second aspect of the present invention provides a silver catalyst prepared by the above preparation method.

[0015] The third aspect of the present invention provides the use of the above silver catalyst in catalyzing the epoxidation of ethylene to produce ethylene oxide.

[0016] The technical solution of the present invention has the following beneficial effects:

[0017] The silver catalyst prepared according to the method of the present invention has high activity and selectivity and is particularly suitable for a reaction device for producing ethylene oxide by epoxidation of ethylene with a high load.

[0018] Other features and advantages of the present invention will be described in detail in the following detailed description. DETAILED DESCRIPTION

[0019] The preferred embodiments of the present invention will be described in more detail below. Although the preferred embodiments of the present invention are described below, it should be understood that the present invention can be implemented in various forms and should not be limited to the embodiments set forth herein.

[0020] The first aspect of the present invention provides a method for preparing a silver catalyst, the preparation method comprising the following steps:

[0021] (1) preparing an impregnation solution;

[0022] (2) impregnating the carrier with the impregnation solution, and then leaching and heating to obtain the silver catalyst;

[0023] The impregnation solution comprises: a silver compound, an alkali metal additive, a rhenium additive and an organic co-additive of rhenium. The raw materials of the impregnation solution are prepared so that the silver content of the prepared silver catalyst is 15-36wt% based on the total weight of the silver catalyst; the molar ratio of silver to alkali metal in the silver catalyst is 150-800 / 1, preferably 200-650 / 1, the molar ratio of alkali metal to rhenium is 0.5-10 / 1, preferably 1.0-8.0 / 1; the molar ratio of rhenium to the metal element of the organic co-additive of rhenium is 5-50 / 1, preferably 10-40 / 1.

[0024] In the present invention, the inventors have conducted in-depth research on the preparation of domestically produced high-efficiency silver-containing rhenium catalysts, that is, by selecting a carrier with suitable physical properties and the original catalyst preparation process, the addition amount of alkali metal additives, rhenium additives and co-additives in the impregnation solution is adjusted so that the loading amount between silver and alkali metal, alkali metal and rhenium, and rhenium and its co-additives in the prepared finished catalyst is in a certain ratio to further improve the performance of the high-efficiency silver catalyst. The silver amine solution is prepared in a traditional way, and according to the physical properties of the carrier, the addition amount of the additive is strictly controlled in the process of preparing the impregnation solution. After the catalyst is leached and thermally decomposed, there is an optimal ratio range between the active component silver and the loading amount of each additive, and the prepared silver catalyst has good performance.

[0025] In the present invention, alkali metal additives and rhenium additives are the two most important additives in the silver catalyst. The discovery of each additive has qualitatively improved the performance of the silver catalyst. In particular, the addition of rhenium additives has broken the limit of 85.7% of ethylene oxide selectivity of the silver catalyst, which is of great significance in the development history of silver catalysts. Previously, patent documents only limited the composition of the active component silver and the additives in the catalyst, and the optimal ratio range between silver and the additives was not reported.

[0026] The auxiliary agents used in the present invention include alkali metal auxiliary agents, rhenium auxiliary agents and co-auxiliaries thereof. The auxiliary agents with a synergistic ratio in the catalyst can achieve the best effect of its auxiliary catalytic effect and improve the performance of the prepared silver catalyst.

[0027] In the present invention, the impregnation solution preferably comprises: a silver compound, an alkali metal additive, a rhenium additive, an organic co-additive of rhenium and a solvent, wherein the solvent is water and / or an organic solvent; and the organic solvent is preferably an organic amine.

[0028] According to the present invention, preferably, the raw materials of the impregnation solution are prepared so that in the prepared silver catalyst, the content of alkali metal in each auxiliary component, calculated as metal, is 50 to 3000 ppm, preferably 100 to 2500 ppm; the content of rhenium is 25 to 1500 ppm, preferably 50 to 1200 ppm; the content of organic co-auxiliary metal element of rhenium is 5 to 300 ppm, preferably 10 to 250 ppm.

[0029] In the present invention, the contents of the alkali metal, rhenium and rhenium co-promoter metal element are all based on the total weight of the silver catalyst.

[0030] According to the present invention, preferably, the organic co-adjuvant of rhenium is an organic complex of chromium, preferably including at least one of chromium picolinate, chromium nicotinate, yeast chromium, chromium methionine and chromium propionate.

[0031] In the present invention, the organic co-promoter of rhenium is more fully dissolved in the silver amine solution, has a better coordination effect on rhenium, and further improves the catalyst performance.

[0032] According to the present invention, preferably, the alkali metal auxiliary agent is at least one of compounds of lithium, sodium, potassium, rubidium and cesium.

[0033] According to the present invention, preferably, the rhenium auxiliary agent is at least one of rhenium oxide, perrhenic acid and perrhenate, preferably perrhenic acid and / or perrhenate, and more preferably at least one of perrhenic acid, cesium perrhenate and ammonium perrhenate.

[0034] According to the present invention, preferably, the carrier is an α-alumina carrier;

[0035] The α-alumina carrier is preferably prepared by a method comprising the following steps: uniformly mixing inert α-A12O3 powder, pseudo-monohydrate alumina, a pore-forming agent, a silicon-containing compound and a zirconium-containing compound to obtain a mixture, and then kneading, extruding, drying and calcining the mixture, an extrusion aid and a cellulose solution binder to obtain the α-alumina carrier.

[0036] In the present invention, the carrier used in the present invention is preferably a porous α-alumina, the α-alumina content in the carrier is more than 90%, and preferably includes the following preparation steps:

[0037] 1) preparing a solid mixture having the following composition:

[0038] a) α-A12O3 having a particle size of 1 to 5 μm in an amount of 75% to 95% based on the total weight of the solid mixture;

[0039] b) 2.0% to 15% of pseudo-alumina monohydrate having a particle size of less than 75 μm, based on the total weight of the solid mixture;

[0040] c) a pore-forming agent in an amount of 2.0% to 15% based on the total weight of the solid mixture;

[0041] d) a silicon-containing compound in an amount of 0.1% to 1.5% by weight based on the total weight of the solid mixture;

[0042] e) a zirconium-containing compound in an amount of 0.2% to 2.0% by weight based on the total weight of the solid mixture;

[0043] II) The mixed material of step I) is transferred into a kneader and the following auxiliary agents are added:

[0044] h) an extrusion aid in an amount of 0.5% to 10% based on the total weight of the mixture in step I);

[0045] i) using 20% ​​to 40% of a cellulose polymer colloidal solution as a binder based on the total weight of the mixture in step I);

[0046] III) The kneaded material of step II) is extruded into strips, dried and calcined at 1200-1450°C to prepare a finished α-A12O3 carrier.

[0047] The porous alumina carrier prepared by this method has the following characteristics: the crushing strength of the carrier is 40 to 150 N / grain, preferably 50 to 140 N / grain; the specific surface area is 0.5 to 2.5 m 2 / g, preferably 0.7 to 2.0 m 2 / g; the pore volume is 0.30-0.65 ml / g, preferably 0.35-0.60 ml / g.

[0048] According to the present invention, preferably, in step (2), the carrier is impregnated with the impregnation liquid under the condition that the vacuum degree is less than 10 mmHg;

[0049] Heating is carried out in an air stream or a nitrogen-oxygen mixture with an oxygen content of not more than 21% by volume.

[0050] According to the present invention, preferably, the preparation method further comprises step (3): repeatedly performing step (2) on the prepared silver catalyst.

[0051] In the present invention, the impregnation solution formula is designed according to the catalyst composition and the physical properties of the carrier, and the obtained impregnation solution is used to twice impregnate the carrier under the condition of vacuum degree less than 10 mmHg to prepare the silver catalyst product. The impregnation time of the alumina carrier is preferably 10 to 60 minutes, and then drained and thermally decomposed.

[0052] In the present invention, the alkali metal auxiliary agent may be applied to the support before, simultaneously with or after the impregnation of silver, or may be impregnated on the support after the silver compound is reduced.

[0053] In the present invention, the rhenium-containing promoter and the organic co-promoter of rhenium can be applied to the support before, at the same time or after the silver is impregnated, or can be impregnated on the support after the silver compound is reduced. The activity, selectivity and stability of the activity and selectivity of the obtained silver catalyst can be further improved by adding the rhenium promoter and the organic co-promoter of rhenium.

[0054] The second aspect of the present invention provides a silver catalyst prepared by the above preparation method.

[0055] The third aspect of the present invention provides the use of the above silver catalyst in catalyzing the epoxidation of ethylene to produce ethylene oxide.

[0056] The invention will be further described below with reference to the embodiments, but the scope of the invention is not limited to these embodiments.

[0057] The silver catalyst used in the following examples and comparative examples was tested for its initial performance and stability using a laboratory reactor (hereinafter referred to as "micro-reactor") evaluation device. The reactor used in the micro-reactor evaluation device is a stainless steel tube with an inner diameter of 4 mm, and the reactor is placed in a heating jacket. The catalyst loading volume is 1 ml, and there is an inert filler at the bottom so that the catalyst bed is located in the constant temperature zone of the heating jacket.

[0058] Determination of initial activity and selectivity

[0059] The activity and selectivity determination conditions used in the present invention are as follows:

[0060] Reaction gas composition (mol%)

[0061] <![CDATA[Ethylene (C2H4)]]> 28.0%±1.0 <![CDATA[Oxygen (O2)]]> 7.4%±0.2 <![CDATA[Carbon dioxide (CO2)]]> <1.0% Inhibitor Ethylene Dichloride 0.1ppm~2.0ppm <![CDATA[Stabilizing gas (N2)]]> margin Reaction pressure 2.1MPa airspeed 6000 / h EO concentration at reactor outlet (mol%) 2.50%

[0062] When the above reaction conditions are stably reached, the gas composition at the reactor inlet and outlet is continuously measured. The selectivity is calculated according to the following formula after volume shrinkage correction is performed on the measured results:

[0063]

[0064] Among them, ΔEO is the difference in ethylene oxide concentration between the outlet gas and the inlet gas, and the average of more than 10 groups of test data is taken as the test result of the day.

[0065] The carriers used in the following examples and comparative examples were prepared by the following method:

[0066] Put 500g of inert α-A12O3 powder of 1-5μm, 50g of pseudo monohydrate alumina less than 75μm, 50g of petroleum coke, 3.0g of calcium silicate and 5.0g of zirconium dioxide into a mixer and mix them evenly. Then transfer them into a kneader, add 25g of vaseline and 160g of 2.5% methyl cellulose colloidal aqueous solution, and knead them into a paste that can be extruded. Extrusion molding is a single-hole column with an outer diameter of 8.0mm, a length of 6.0mm, and an inner diameter of 3.0mm. Dry it at 100℃ for more than 2 hours to reduce the free water content to less than 10%. Put the above kneaded carrier into a bell kiln, raise it from room temperature to 1400℃ after 33 hours, and calcine it at 1400℃ for 4 hours to obtain a carrier (α-alumina carrier) of a white silver catalyst. The carrier crushing strength is 68N / grain; the specific surface area is 1.16m 2 / g; pore volume is 0.44ml / g.

[0067] Catalyst Preparation Comparative Example 1

[0068] 19.85 g of ethylenediamine was dissolved in 35.92 g of deionized water. Silver oxalate was slowly added to the mixture under stirring. The temperature was kept below 40° C. to dissolve all the silver oxalate. The amount of silver oxalate added was such that the silver content in the silver catalyst was 24 wt % (based on the total weight of the silver catalyst). 0.055 g of cesium nitrate and deionized water were then added to make the total mass of the solution reach 100 g to prepare an impregnation solution for standby use.

[0069] Catalyst Preparation Comparative Example 2

[0070] 19.85 g of ethylenediamine was dissolved in 35.92 g of deionized water. Silver oxalate was slowly added to the mixture under stirring. The temperature was kept below 40° C. to dissolve all the silver oxalate. The amount of silver oxalate added was such that the silver content in the silver catalyst was 24 wt % (based on the total weight of the silver catalyst). 0.074 g of cesium nitrate, 0.251 g of perrhenic acid and deionized water were then added to make the total mass of the solution reach 100 g to prepare an impregnation solution for standby use.

[0071] Catalyst Preparation Comparative Example 3

[0072] 19.85 g of ethylenediamine was dissolved in 35.92 g of deionized water. Silver oxalate was slowly added to the mixture under stirring. The temperature was kept below 40° C. to dissolve all the silver oxalate. The amount of silver oxalate added was such that the silver content in the silver catalyst was 24 wt % (based on the total weight of the silver catalyst). Then 0.174 g of cesium nitrate, 0.093 g of perrhenic acid, 0.003 g of ammonium chromate and deionized water were added to make the total mass of the solution reach 100 g to prepare an impregnation solution for standby use.

[0073] Catalyst Preparation Example 1

[0074] 19.85 g of ethylenediamine was dissolved in 35.92 g of deionized water, and silver oxalate was slowly added to the mixture under stirring. The temperature was kept below 40° C. to dissolve all the silver oxalate. The amount of silver oxalate added was such that the silver content in the silver catalyst was 24 wt % (based on the total weight of the silver catalyst). Then, 0.074 g of cesium nitrate, 0.186 g of perrhenic acid, 0.004 g of chromium propionate and deionized water were added to make the total mass of the solution reach 100 g, and an impregnation solution was prepared for standby use.

[0075] Catalyst Preparation Example 2

[0076] 19.85 g of ethylenediamine was dissolved in 35.92 g of deionized water. Silver oxalate was slowly added to the mixture under stirring. The temperature was kept below 40° C. to dissolve all the silver oxalate. The amount of silver oxalate added was such that the silver content in the silver catalyst was 24 wt % (based on the total weight of the silver catalyst). Then 0.110 g of cesium nitrate, 0.136 g of perrhenic acid, 0.004 g of chromium propionate and deionized water were added to make the total mass of the solution reach 100 g to prepare an impregnation solution for standby use.

[0077] Catalyst Preparation Example 3

[0078] 19.85 g of ethylenediamine was dissolved in 35.92 g of deionized water. Silver oxalate was slowly added to the mixture under stirring. The temperature was kept below 40° C. to dissolve all the silver oxalate. The amount of silver oxalate added was such that the silver content in the silver catalyst was 24 wt % (based on the total weight of the silver catalyst). Then 0.174 g of cesium nitrate, 0.093 g of perrhenic acid, 0.006 g of chromium propionate and deionized water were added to make the total mass of the solution reach 100 g to prepare an impregnation solution for standby use.

[0079] Catalyst Preparation Example 4

[0080] 19.85 g of ethylenediamine was dissolved in 35.92 g of deionized water. Silver oxalate was slowly added to the mixture under stirring. The temperature was kept below 40° C. to dissolve all the silver oxalate. The amount of silver oxalate added was such that the silver content in the silver catalyst was 24 wt % (based on the total weight of the silver catalyst). Then 0.174 g of cesium nitrate, 0.093 g of perrhenic acid, 0.008 g of chromium propionate and deionized water were added to make the total mass of the solution reach 100 g to prepare an impregnation solution for standby use.

[0081] Catalyst Preparation Example 5

[0082] 19.85 g of ethylenediamine was dissolved in 35.92 g of deionized water. Silver oxalate was slowly added to the mixture under stirring. The temperature was kept below 40° C. to dissolve all the silver oxalate. The amount of silver oxalate added was such that the silver content in the silver catalyst was 24 wt % (based on the total weight of the silver catalyst). Then 0.221 g of cesium nitrate, 0.051 g of perrhenic acid, 0.006 g of chromium propionate and deionized water were added to make the total mass of the solution reach 100 g to prepare an impregnation solution for standby use.

[0083] Catalyst Preparation Example 6

[0084] 19.85 g of ethylenediamine was dissolved in 35.92 g of deionized water. Silver oxalate was slowly added to the mixture under stirring. The temperature was kept below 40° C. to dissolve all the silver oxalate. The amount of silver oxalate added was such that the silver content in the silver catalyst was 24 wt % (based on the total weight of the silver catalyst). Then 0.331 g of cesium nitrate, 0.043 g of perrhenic acid, 0.009 g of chromium propionate and deionized water were added to make the total mass of the solution reach 100 g to prepare an impregnation solution for standby use.

[0085] Catalyst Preparation Example 7

[0086] 19.85 g of ethylenediamine was dissolved in 35.92 g of deionized water, and silver oxalate was slowly added to the mixture under stirring. The temperature was kept below 40° C. to dissolve all the silver oxalate. The amount of silver oxalate added was such that the silver content in the silver catalyst was 24 wt % (based on the total weight of the silver catalyst). Then 0.331 g of cesium nitrate, 0.043 g of perrhenic acid, 0.008 g of chromium picolinate and deionized water were added to make the total mass of the solution reach 100 g, and the mixture was prepared into an impregnation solution for standby use.

[0087] Take 20g of the carrier sample respectively, put it into a vacuum container, evacuate to above 10mmHg, introduce the above impregnation solution, keep it for 30min, and filter out the excess solution. The impregnated carrier is heated in an air flow of 350℃ for 10min, and after cooling, it is made into a primary impregnation catalyst; repeat the above steps for secondary impregnation to obtain the finished catalyst. The activity and selectivity of the catalyst sample are measured under the above process conditions using a microreactor evaluation device, and the space-time yield is 295gEO / mlCat. / h. The experimental results are listed in Table 1 below.

[0088] Table 1 Effect of additive composition on the performance of silver catalyst

[0089]

[0090] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments.

Claims

1. A method for preparing a silver catalyst, characterized in that: The preparation method comprises the following steps: (1) preparing an impregnation solution; (2) impregnating the carrier with the impregnation solution, and then leaching and heating to obtain the silver catalyst; The impregnation solution comprises: a silver compound, an alkali metal additive, a rhenium additive and an organic co-additive of rhenium. The raw materials of the impregnation solution are prepared so that the silver content of the prepared silver catalyst is 15-36wt% based on the total weight of the silver catalyst; the molar ratio of silver to alkali metal in the silver catalyst is 150-800 / 1, preferably 200-650 / 1, the molar ratio of alkali metal to rhenium is 0.5-10 / 1, preferably 1.0-8.0 / 1; the molar ratio of rhenium to the metal element of the organic co-additive of rhenium is 5-50 / 1, preferably 10-40 / 1.

2. The preparation method according to claim 1, wherein The raw materials of the impregnation solution are prepared so that in the prepared silver catalyst, the content of alkali metal in each auxiliary component is 50-3000ppm, preferably 100-2500ppm; the content of rhenium is 25-1500ppm, preferably 50-1200ppm; the content of organic co-auxiliary metal element of rhenium is 5-300ppm, preferably 10-250ppm.

3. The preparation method according to claim 1, wherein The organic co-adjuvant of rhenium is an organic complex of chromium, preferably including at least one of chromium picolinate, chromium nicotinate, yeast chromium, chromium methionine and chromium propionate.

4. The preparation method according to claim 1, wherein The alkali metal additive is at least one of compounds of lithium, sodium, potassium, rubidium and cesium.

5. The preparation method according to claim 1, wherein The rhenium auxiliary agent is at least one of rhenium oxide, perrhenic acid and perrhenate, preferably perrhenic acid and / or perrhenate, and more preferably at least one of perrhenic acid, cesium perrhenate and ammonium perrhenate.

6. The preparation method according to claim 1, wherein The carrier is an α-alumina carrier; The α-alumina carrier is preferably prepared by a method comprising the following steps: uniformly mixing inert α-A12O3 powder, pseudo-monohydrate alumina, a pore-forming agent, a silicon-containing compound and a zirconium-containing compound to obtain a mixture, and then kneading, extruding, drying and calcining the mixture, an extrusion aid and a cellulose solution binder to obtain the α-alumina carrier.

7. The preparation method according to claim 1, wherein In step (2), the carrier is impregnated with the impregnation liquid under the condition that the vacuum degree is less than 10 mmHg; Heating is carried out in an air stream or a nitrogen-oxygen mixture with an oxygen content of not more than 21% by volume.

8. The preparation method according to claim 1, wherein The preparation method further comprises step (3): repeatedly performing step (2) on the prepared silver catalyst.

9. The silver catalyst prepared by the preparation method according to any one of claims 1 to 8.

10. Use of the silver catalyst according to claim 9 in catalyzing the epoxidation of ethylene to produce ethylene oxide.

Citation Information

Patent Citations

  • Preparation method of silver catalyst for producing ethylene oxide through ethylene oxidation, silver catalyst and application

    CN115364854A

  • Preparation method of silver catalyst for producing ethylene oxide through ethylene oxidation, silver catalyst and application

    CN115487809A