Monolithic metal net catalyst for CO catalytic oxidation and preparation method and application thereof

The integrated metal mesh catalyst prepared by electrochemical synthesis solves the problems of poor stability of existing catalysts and high cost of precious metal catalysts, and realizes efficient CO catalytic oxidation, which has the advantages of small pressure drop, stability and mechanical strength. It is suitable for In terms of energy efficiency improvement and cost reduction.

CN118925728APending Publication Date: 2024-11-12EAST CHINA UNIV OF SCI & TECH
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410965288.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Among the existing CO catalytic oxidation catalysts, the preparation of the integral catalyst has problems such as weak support binding force and poor stability, and the high price of precious metal catalysts, which limits its large-scale application.

Method used

The integrated metal mesh catalyst was prepared by electrochemical synthesis method, and Cu-Co hydroxide precursor was electrochemically deposited by ultrapure water ultrasonic precursor, and heated up and activated in an inert gas to form Cu-Co oxide surface. Mesh metal catalyst.

Benefits of technology

It has achieved an integrated metal mesh catalyst with small pressure drop, stable chemical properties, high mechanical strength and good mass transfer effect. It is suitable for CO catalytic oxidation, improving energy efficiency and reducing reaction costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118925728A_ABST
    Figure CN118925728A_ABST
Patent Text Reader

Abstract

The invention relates to an integral metal net catalyst for CO catalytic oxidation and a preparation method and application thereof, and the preparation method comprises the following steps: ultrasonically pretreating a Cu net by using ultrapure water, and drying to obtain a clean material. Next, a Co (NO3) 2 solution or a mixed solution of the Co (NO3) 2 solution and NaNO3 is used as an electrolyte, and a catalyst precursor is prepared by an electrochemical synthesis method and setting current and positive and negative electrode alternating conditions; and finally, washing and drying the precursor, introducing gas, and activating at a specific temperature to obtain the metal mesh catalyst. Compared with the prior art, the preparation process is simple, preparation reaction conditions are easy to control, and the preparation method is efficient. The integral Cu net catalyst has the advantages of small pressure drop, stable chemical performance, high mechanical strength and good mass transfer effect. In addition, other metal nets can be used for replacement in later exploration, the exploration performance is high, the application range is wide, and good application and popularization are achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of catalysts, and in particular to an integral metal mesh catalyst for CO catalytic oxidation and a preparation method and application thereof. Background Art

[0002] CO is usually a colorless, non-irritating gas. The explosion limit when mixed with air is 12.5%-72.4%. After entering the human body, CO has a high affinity with hemoglobin in the blood, which inhibits the binding of hemoglobin to oxygen. Even at extreme levels, it can cause hypoxic shock, and in severe cases, death. Carbon monoxide is also a precursor of ground-level ozone and can cause serious respiratory problems. CO has a wide range of sources. Exhaust gas emitted by cars, gas emitted by power plants and factories, fuel cells, and daily use of coal gas will release a large amount of carbon monoxide, causing environmental pollution. Therefore, the elimination of low concentrations of CO has attracted widespread attention. Commonly used technologies for gas purification include filtration, adsorption, catalysis, and plasma. At present, the most widely used method for eliminating low concentrations of CO in the air is catalytic oxidation.

[0003] The preparation of efficient catalysts at room temperature is the core of catalytic oxidation. At present, catalysts for CO catalytic oxidation are mainly divided into two categories: precious metal catalysts and non-precious metal catalysts, and different types of catalysts have their own strengths. Precious metal catalysts show excellent catalytic performance such as high efficiency, good stability and high activity in the CO oxidation process, but their high prices limit their large-scale application. In contrast, non-precious metal catalysts have gradually become a research hotspot because of their economy and good treatment effects. Therefore, the applicant believes that there is an urgent need to prepare a non-precious metal catalyst, which is of great significance and good industrial application prospects for CO catalytic oxidation.

[0004] Compared with traditional catalysts, compared with traditional powdered or granular catalysts, monolithic catalysts show the advantages of small pressure drop, stable chemical properties, high mechanical strength and good mass transfer effect. However, how to prepare high-performance monolithic electrocatalysts is a problem that needs to be solved urgently. CN108953462A discloses an integrated metal-non-metal composite catalyst and preparation method for CO hydrogenation to methanol. The invention adopts a wet coating process to prepare an integrated Cu, MoOx bifunctional catalyst for CO hydrogenation to methanol. However, the catalyst used in this patent is still in a dispersed granular state, has weak binding force with the carrier, and has poor stability. CN105102455A also discloses the structure of an integrated anode or cathode substrate, but it does not explain the specific operating process, nor does it propose evaluation indicators for its performance. Based on the above reasons, the applicant designed and proposed a method of using a whole metal mesh as a carrier to replace the existing porous carrier to solve such problems. Summary of the invention

[0005] The purpose of the present invention is to overcome the defects of the above-mentioned prior art and provide an integral metal mesh catalyst for CO catalytic oxidation and its preparation method and application, which exhibits the advantages of small pressure drop, stable chemical properties, high mechanical strength and good mass transfer effect.

[0006] Therefore, it is widely used in catalytic combustion, catalytic degradation of VVCs, selective catalytic reduction of NOx, exhaust gas treatment and other fields to improve energy efficiency and reduce reaction costs.

[0007] The purpose of the present invention can be achieved by the following technical solutions:

[0008] The first aspect of the present invention provides an electrochemical synthesis method of a monolithic metal mesh catalyst for CO catalytic oxidation, comprising the following steps:

[0009] S1: Ultrasonic pretreatment of the Cu mesh with ultrapure water for t0, and drying to obtain a clean Cu mesh material;

[0010] S2: Using Co(NO3)2 aqueous solution or NaNO3 and Co(NO3)2 mixed aqueous solution as electrolyte, using two Cu meshes as positive and negative electrodes, using electrochemical synthesis method, presetting current I1, I2, positive and negative electrode alternation time t1, t2, cycle alternation number x, to obtain catalyst precursor;

[0011] S3: Wash and dry the prepared catalyst precursor, prepare a sample and put it into a reactor, introduce gas, preset the starting temperature T0, heat it to T1, heat it up at a rate of ν0, heat it up for a time of t3, stabilize it for a time of t4, and complete the activation of the Cu mesh metal catalyst to obtain an integral metal mesh catalyst.

[0012] Furthermore, in S1, the ultrasonic pretreatment time t0 is 5-60 min.

[0013] Furthermore, in S2, the concentration of the NaNO3 solution is 0.01-2 mol / L, and the concentration of Co(NO3)2 is 0.01-2 mol / L.

[0014] Furthermore, in S2, the values ​​of the preset currents I1 and I2 are 100 mA-1000 mA, the values ​​of the positive and negative pole alternation times t1 and t2 are 10 s-100 s, and the number of cycle alternations x is 100 times-500 times.

[0015] Furthermore, in S2, the catalyst precursor is Cu-Co hydroxide.

[0016] Furthermore, in S3, the process of washing the catalyst precursor includes: washing the prepared Cu-Co hydroxide precursor with ultrapure water, ultrasonicating it for 3-10 minutes, and then drying it in a drying oven for 3-12 hours.

[0017] Furthermore, in S3, the gas is Ar or O2.

[0018] Furthermore, in S3, the preset starting temperature T0 is 10℃-40℃, the temperature rises to T1 is 100℃-500℃, the heating rate ν0 does not exceed 10℃ / min, the heating time t3 is the ratio of the rising temperature to the heating rate, t3 is calculated by the determined heating rate, and the stabilization time t4 is 60min-90min.

[0019] The second aspect of the present invention provides a monolithic metal mesh catalyst as described above, wherein the monolithic metal mesh catalyst is a Cu mesh metal catalyst having a surface of Cu—Co oxide.

[0020] A third aspect of the present invention provides a use of the above-mentioned integral metal mesh catalyst in CO catalytic oxidation.

[0021] Compared with the prior art, the present invention has the following technical advantages:

[0022] (1) The catalyst prepared in the present invention is a monolithic catalyst, which has the advantages of small pressure drop, stable chemical properties, high mechanical strength and good mass transfer effect. It still has high activity after the water content test and has certain water resistance and stability.

[0023] (2) The preparation method used in the present invention has a short preparation cycle compared to traditional preparation methods, such as the impregnation method, the sol-gel method, etc., and a large amount of catalyst can be prepared in a single time. In addition, the preparation variables can be easily controlled, and repeated samples can be easily achieved in subsequent repeated experiments, which has a high prospect for industrial application. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is a data diagram for comparing the activities of the catalysts of the present invention at different charge amounts.

[0025] Figure 2 This is a comparative data diagram of the activity of different contents of Co metal doped in the present invention.

[0026] Figure 3 This is a stability data diagram of the catalyst with the best activity in the present invention under water-containing conditions.

[0027] Figure 4 This is a physical picture of sample preparation in the present invention. DETAILED DESCRIPTION

[0028] The integral Cu mesh metal catalyst used for CO catalytic oxidation in the present invention is synthesized by an electrochemical method. In this patent, the preparation current, time and number of cycles are specifically regulated to explore the influence on the activity.

[0029] In a specific implementation, the preparation current is controlled within the range of 100mA-1000mA, the time is controlled within the range of 10s-100s, and the number of cycles is controlled within the range of 100-500 times.

[0030] In specific implementation, the method for electrochemically synthesizing a monolithic Cu mesh composite metal catalyst in the present invention comprises the following steps:

[0031] S1: Ultrasonic pretreatment of the Cu mesh with ultrapure water for t0, and drying to obtain a clean Cu mesh material;

[0032] S2: Using a certain concentration of Co(NO3)2 or a mixture of a certain concentration of NaNO3 and Co(NO3)2 as the electrolyte, two Cu meshes as the positive and negative electrodes, and using an electrochemical synthesis method to preset currents I1 and I2, positive and negative electrode alternation times t1 and t2, and cycle alternation times x, to obtain a catalyst precursor;

[0033] S3: Wash and dry the prepared catalyst precursor, prepare a sample and place it in a reactor, introduce an inert gas, preset the starting temperature T0, heat it to T1, heat it up at a rate of ν0, heat it up for a time of t2, stabilize it for a time of t3, and complete the activation of the Cu mesh metal catalyst.

[0034] In a specific implementation, the metal mesh catalyst is a Cu mesh metal catalyst.

[0035] In specific implementation, the ultrasonic pretreatment time t0 in S1 is 3-8 min, preferably t0 is 5 min.

[0036] In specific implementation, the concentration of NaNO3 in S2 is 0.01-1 mol / L, and the concentration of Co(NO3)2 is 0.01-1 mol / L. Preferably, the concentration of Co(NO3)2 is 0.05M.

[0037] In specific implementation, the preset currents I1 and I2 in S2 are 100mA-1000mA, the positive and negative alternating times t1 and t2 are 10s-100s, and the number of cycle alternations x is 100-500 times. Preferably, I1 is 180mA, I2 is 240mA, the positive and negative alternating times t1 and t2 are 40s, and the number of cycle alternations x is 400 times.

[0038] In a specific implementation, the catalyst precursor described in S2 is a Cu-Co hydroxide precursor.

[0039] In the specific implementation, in S3, the prepared Cu-Co hydroxide precursor needs to be washed with ultrapure water, and then ultrasonicated for 3-8 minutes and placed in a drying oven for drying for 3-12 hours.

[0040] In a specific implementation, the gas described in S3 is Ar or O2.

[0041] In specific implementation, the preset starting temperature T0 in S3 is 10°C-40°C, the temperature rises to T1 is 100°C-500°C, the heating rate v0 does not exceed 10°C / min, the heating time t3 is the ratio between the heating rate and the rising temperature, which can be calculated by the determined heating rate, and the stabilization time t4 is 60min-90min. Preferably, T1 is 300°C; the stabilization time t4 is 60min.

[0042] The present invention provides a monolithic metal mesh catalyst for CO catalytic oxidation, a preparation method thereof, and a use thereof. The nano multilayer composite material composed of Cu and Co not only promotes the forward movement of the chemical equilibrium of the multiphase catalytic reaction, but also improves the physical properties of the catalyst itself, thereby achieving a synergistic effect between Cu and Co, greatly increasing the conductivity and mass transfer capacity of the substrate, and avoiding the agglomeration phenomenon of conventional catalytic materials. At the same time, the preparation method of the monolithic metal mesh catalyst provided by the present invention is simple and easy, low in cost, flexible and diverse in operation, and has a wide range of application, which can effectively expand the field of its practical application.

[0043] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. Any features such as preparation means, materials, structures or composition ratios not clearly described in this technical solution are regarded as common technical features disclosed in the prior art.

[0044] Example 1

[0045] In this embodiment, 0.05M Co(NO3)2 aqueous solution was used as the electrolyte, and the preparation was carried out under the conditions of positive electrode current of 180mA, negative electrode current of -240mA, time of 40s and 30s respectively, and cycle number of 300 times.

[0046] The preparation process of this embodiment includes:

[0047] S1: Ultrasonic pretreatment of the Cu mesh with ultrapure water for 5 min, and drying to obtain a clean Cu mesh material;

[0048] S2: 0.05M Co(NO3)2 aqueous solution was used as the electrolyte, and two Cu meshes were used as the positive and negative electrodes. Figure 4 , using the electrochemical synthesis method, the preset current I1=180mA, I2=240mA, the positive and negative electrode alternation time is 40s and 30s, the cycle alternation number is 300 times, and the catalyst precursor is obtained;

[0049] S3: Wash and dry the prepared catalyst precursor, prepare a sample and place it in a reactor, introduce inert gas, set the starting temperature at 25°C, heat it to 300°C, heat it up at a rate of ν0 = 10°C / min, heat it up for t2 = 30min, stabilize it for 60min, and complete the activation of the Cu mesh metal catalyst.

[0050] Example 2

[0051] Different from Example 1, in this example, 0.1M Co(NO3)2 aqueous solution is used as the electrolyte, and the preparation is carried out under the conditions of positive electrode current of 180mA, negative electrode current of -240mA, time of 40s and 30s respectively, and cycle number of 300 times.

[0052] Example 3

[0053] Different from Example 1, in this example, 0.03M Co(NO3)2 aqueous solution is used as the electrolyte, and the preparation is carried out under the conditions of positive electrode current of 180mA, negative electrode current of -240mA, time of 40s and 30s respectively, and cycle number of 300 times.

[0054] Example 4

[0055] Different from Example 1, in this example, 0.015M Co(NO3)2 aqueous solution is used as the electrolyte, and the preparation is carried out at a positive electrode current of 180mA, a negative electrode current of -240mA, a time of 40s and 30s respectively, and a cycle number of 300 times.

[0056] Example 5

[0057] Different from Example 1, in this example, 0.1M NaNO3 and 0.05M Co(NO3)2 aqueous solution are used as electrolyte, and the preparation is carried out under the conditions of positive electrode current of 180mA, negative electrode current of -240mA, time of 40s and 30s respectively, and number of cycles of 300 times.

[0058] Example 6

[0059] Different from Example 1, in this example, 0.05M Co(NO3)2 aqueous solution is used as the electrolyte, and the preparation is carried out under the conditions of positive electrode current of 180mA, negative electrode current of -240mA, time of 20s and 15s respectively, and cycle number of 300 times.

[0060] Example 7

[0061] Different from Example 1, in this example, 0.05M Co(NO3)2 aqueous solution is used as the electrolyte, and the preparation is carried out under the conditions of positive electrode current of 180mA, negative electrode current of -240mA, time of 30s and 22.5s respectively, and number of cycles of 300 times.

[0062] Verification Example 1

[0063] The prepared 180mA catalyst was cut into small discs with a diameter of 4mm and a mass of about 50mg. The catalyst was filled into a quartz tube with an outer diameter of 6mm and reacted in a small fixed bed reactor. The test gas was: 1% CO, 20% O2, Ar as carrier gas, and the total gas flow rate was 50mL min -1 The post-reaction gas was passed into a mass spectrometer to detect the amounts of CO and CO2 at reaction temperatures of 100, 120, and 140°C for subsequent conversion rate calculations.

[0064] Table 1: Catalyst performance data at 180 mA in each example and in the examples under the above catalyst evaluation conditions

[0065]

[0066] The experimental results show that when the Co content is within a certain range, the activity of the catalyst is significantly improved at a lower temperature, and can be almost fully utilized at a high temperature, and presents a volcano-shaped distribution with a maximum activity point. The catalyst prepared by the present invention has a short preparation cycle and improved activity. In addition, by using different charge amounts, see Figure 2 The comparison of the catalyst activity shows that the activity of the catalyst gradually increases with the increase of the charge. The reason is that the increase of the charge makes the Cu mesh electrolyzed and the deposited substances increase, which in turn increases the catalytic active sites and improves the activity. In addition, the water stability test of the catalyst with the best activity is carried out, see Figure 3 It can be found that after the catalyst was tested under water conditions for 20 hours, its activity can still be restored to its original level after water removal, indicating that the catalyst has good stability.

[0067] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.

Claims

1. An electrochemical synthesis method of a monolithic metal mesh catalyst for CO catalytic oxidation, characterized in that: The following steps are involved: S1: Ultrapure water is used to ultrasonically pretreat the Cu mesh for t0, and then dried to obtain a clean Cu mesh material; S2: Using Co(NO3)2 aqueous solution or NaNO3 and Co(NO3)2 mixed aqueous solution as electrolyte, using two Cu meshes as positive and negative electrodes, using electrochemical synthesis method, presetting current I1, I2, positive and negative electrode alternation time t1, t2, cycle alternation number x, to obtain catalyst precursor; S3: Wash and dry the prepared catalyst precursor, prepare a sample and put it into a reactor, introduce gas, preset the starting temperature T0, heat it to T1, heat it up at a rate of ν0, heat it up for a time of t3, stabilize it for a time of t4, and complete the activation of the Cu mesh metal catalyst to obtain an integral metal mesh catalyst.

2. The electrochemical synthesis method of a monolithic metal mesh catalyst for CO catalytic oxidation according to claim 1, characterized in that: In S1, the ultrasonic pretreatment time t0 is 5-60 min.

3. The electrochemical synthesis method of a monolithic metal mesh catalyst for CO catalytic oxidation according to claim 1, characterized in that: In S2, the concentration of the NaNO3 solution is 0.01-2 mol / L, and the concentration of Co(NO3)2 is 0.01-2 mol / L.

4. The electrochemical synthesis method of a monolithic metal mesh catalyst for CO catalytic oxidation according to claim 1, characterized in that: In S2, the values ​​of the preset currents I1 and I2 are 100mA-1000mA, the values ​​of the positive and negative pole alternation times t1 and t2 are 10s-100s, and the number of cycle alternations x is 100 times-500 times.

5. The electrochemical synthesis method of a monolithic metal mesh catalyst for CO catalytic oxidation according to claim 1, characterized in that: In S2, the catalyst precursor is Cu-Co hydroxide.

6. The electrochemical synthesis method of a monolithic metal mesh catalyst for CO catalytic oxidation according to claim 1, characterized in that: In S3, the process of washing the catalyst precursor includes: washing the prepared Cu-Co hydroxide precursor with ultrapure water, ultrasonicating for 3-10 minutes, and then putting it into a drying oven for drying for 3-12 hours.

7. The electrochemical synthesis method of a monolithic metal mesh catalyst for CO catalytic oxidation according to claim 1, characterized in that: In S3, the gas is Ar or O2.

8. The electrochemical synthesis method of a monolithic metal mesh catalyst for CO catalytic oxidation according to claim 1, characterized in that: In S3, the preset starting temperature T0 is 10℃-40℃, the temperature rises to T1 is 100℃-500℃, the heating rate ν0 does not exceed 10℃ / min, the heating time t3 is the ratio of the rising temperature to the heating rate, t3 is calculated by the preset heating rate, and the stabilization time t4 is 60min-90min.

9. An integral metal mesh catalyst as claimed in any one of claims 1 to 8, characterized in that: The monolithic metal mesh catalyst is a Cu mesh metal catalyst with a surface of Cu-Co oxide.

10. Use of the monolithic metal mesh catalyst as claimed in claim 9 in catalytic oxidation of CO.

Citation Information

Patent Citations

  • Integral cobalt-manganese based binary catalyst preparation method, product and application thereof

    CN109569646A

  • Preparation method and application of copper-cobalt oxide loaded carbon nanofiber composite material

    CN112275288A

  • Copper-cobalt oxide / carbon nano tube / foamed nickel composite electrode for heterogeneous electro-Fenton system, and application thereof

    CN113998760A

  • Co3O4 nanosheet-loaded stainless steel mesh as well as preparation method and application thereof

    CN114164471A

  • Foam metal loaded nickel ferrite monolithic catalyst as well as preparation method and application thereof

    CN116422334A