Gamma crystal form manganese-based catalyst recycled from waste lithium battery positive electrode material and preparation method and application thereof

By recovering γ-crystalline manganese-based catalysts from waste lithium batteries, the problem of recycling and utilization of manganese-based catalysts in the prior art was solved, and T-γ-MnO2 catalyst with high catalytic activity was prepared, thereby achieving efficient degradation of VOCs and lithium Recycling and utilization of battery resources.

CN118925744APending Publication Date: 2024-11-12JIANGSU UNIV OF TECH

Patent Information

Application Number
CN202410979456.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The prior art is difficult to effectively recycle and utilize manganese-based catalysts in waste lithium batteries, and catalytic oxidation technology has low treatment efficiency for volatile organic compounds (VOCs) at low temperatures.

Method used

By recovering the gamma crystal manganese-based catalyst from the positive electrode material of the waste lithium battery, and preparing the gamma crystal manganese-based catalyst using steps such as soaking, calcining, leaching of acid solution, and hydrothermal reaction, to form a T-γ with high catalytic activity -MnO2 catalyst.

Benefits of technology

The specific surface area and pore volume of the catalyst are improved, the low-temperature redox capacity and the catalytic activity of VOCs are enhanced, and the recycling and utilization of waste lithium battery resources and the efficient degradation of VOCs are achieved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118925744A_ABST
    Figure CN118925744A_ABST
Patent Text Reader

Abstract

The embodiment of the invention relates to a gamma crystal form manganese-based catalyst recycled from a waste lithium battery positive electrode material and a preparation method and application thereof, and belongs to the technical field of waste and old material recycling. The method for recycling the gamma crystal form manganese-based catalyst from the positive electrode material of the waste lithium battery comprises the following steps: S1, putting the waste ternary lithium battery into a NaCl solution to be fully soaked; s2, the battery is disassembled and classified, a positive electrode material is cut after being dried, and is roasted, crushed and sieved to obtain positive electrode active powder; s3, leaching the positive electrode active powder, and filtering to obtain a clarified leachate; s4, the pH of the leachate is adjusted, ammonium sulfite / sodium sulfite and deionized water are added, and a suspension A is obtained; and S5, carrying out a hydrothermal reaction on the turbid liquid A, carrying out solid-liquid separation after the reaction is finished, washing, drying, and calcining to obtain the gamma crystal form manganese-based catalyst. The catalyst has relatively high catalytic efficiency in the process of catalyzing decomposition of VOCs (Volatile Organic Compounds).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The embodiments of the present application relate to the technical field of waste material recycling, and in particular to a γ-crystalline manganese-based catalyst recovered from waste lithium battery positive electrode materials, and a preparation method and application thereof. Background Art

[0002] The share of lithium manganese oxide batteries in the electric bicycle field has increased year by year due to their low cost, good fast charging performance, outstanding low-temperature performance and other advantages. The resulting waste lithium batteries have also become a new "urban mine". Waste lithium manganese oxide batteries are rich in metal elements such as manganese (Mn) and lithium (Li). If they can be effectively recycled, it can not only avoid heavy metal pollution, but also bring considerable economic benefits. Volatile organic compounds (VOCs) are one of the main sources of air pollutants and are also secondary organic aerosols (SOAs) and ozone (O 3 ). Therefore, effective control of VOCs emissions is crucial to solving the problem of air pollution. Among the many VOCs treatment technologies, catalytic oxidation is considered to be one of the most promising technologies because it can completely convert VOCs at a lower temperature, high activity and low cost. For catalytic oxidation, catalysts are the key to large-scale promotion and application. The synthesis of various VOCs oxidation catalysts has become the focus of many researchers. Summary of the invention

[0003] In view of this, the embodiments of the present application provide a γ-crystalline manganese-based catalyst recovered from the positive electrode material of waste lithium batteries, and a preparation method and application thereof. The method utilizes the manganese-based transition metal in the waste ternary lithium battery to synthesize the manganese dioxide catalyst, which can effectively overcome the defects of the above-mentioned prior art.

[0004] The first aspect of the embodiment of the present application provides a method for recovering a γ-crystalline manganese-based catalyst from a waste lithium battery positive electrode material, comprising the following steps:

[0005] S1. Soak the used ternary lithium battery in a NaCl solution;

[0006] S2, using tools to saw open the battery shell, disassemble and classify the batteries, wherein the positive electrode material is dried, cut, roasted, crushed and sieved to obtain positive electrode active powder;

[0007] S3, selecting an acid solution and a reducing agent to leach the positive electrode active powder, and obtaining a clarified leachate after filtering;

[0008] S4, adding alkali metal hydroxide to the clarified leachate, stirring evenly, adjusting the pH of the leachate, and then adding ammonium sulfite and deionized water, stirring evenly, to obtain a suspension A;

[0009] S5, subjecting the suspension A to a hydrothermal reaction, and after the reaction is completed, performing solid-liquid separation, washing, drying, and calcining to obtain a γ-crystalline manganese-based catalyst.

[0010] Specifically, a method for recovering a γ-crystalline manganese-based catalyst from a waste lithium battery positive electrode material comprises the following steps:

[0011] S1. Soak the used ternary lithium battery in a NaCl solution to fully discharge it to ensure the safety of the subsequent disassembly process;

[0012] S2. Using tools to saw open the battery casing, disassemble the battery and classify it into positive electrode materials and the remaining parts. The positive electrode materials are naturally dried in a fume hood, then cut into small square pieces, and baked in a muffle furnace to remove the binder PVDF. The baked positive electrode sheets are crushed by a grinder and sieved to obtain positive electrode active powder;

[0013] S3, using an acid solution and a reducing agent to leach the positive electrode active powder, so that the main metal elements are transferred from the solid to the solution. After the leaching is completed, the mixed solution is filtered through a filter membrane to obtain a clarified leachate;

[0014] S4, adding alkali metal hydroxide to the clarified leachate, stirring evenly, adjusting the pH of the leachate to 3-6, then adding ammonium sulfite / sodium sulfite and deionized water, stirring evenly, to obtain a suspension A;

[0015] S5, placing the suspension A in a reactor with a polytetrafluoroethylene liner, placing the reactor in a blast drying oven for hydrothermal reaction, filtering the obtained sample after the reaction, and then rinsing with deionized water until the filtrate is neutral, placing the obtained filter residue in a blast drying oven for drying, and then placing the dried sample in a muffle furnace for calcination, grinding after calcination, and obtaining a γ-crystalline manganese-based catalyst T-γ-MnO 2 .

[0016] In some embodiments that may include the above embodiments, in step S3, the leaching conditions are: the leaching temperature is 60-80°C, the leaching time is 1-5h, and the solid-liquid ratio is 20:1.

[0017] In some embodiments that may include the above embodiments, in step S5, the hydrothermal reaction temperature is 80-100°C, and the hydrothermal reaction time is 20-30h. The hydrothermal reaction temperature is preferably 80°C, 90°C or 100°C, etc.; the hydrothermal reaction time is preferably 20h, 25h or 30h, etc.

[0018] In some embodiments that may include the above embodiments, in step S5, the drying temperature is 55-80°C and the drying time is 8-24h. The drying temperature is preferably 50°C, 60°C, 70°C or 80°C, etc.; the drying time is preferably 8h, 10h, 12h or 24h, etc.

[0019] In some embodiments that may include the above embodiments, in step S5, the calcination heating rate is 2-6°C / min, the calcination temperature is 300-450°C, and the calcination time is 1-3h. The calcination heating rate is preferably 2°C / min, 4°C / min, or 6°C / min, etc.; the calcination temperature is preferably 300°C, 350°C, 400°C, or 450°C, etc.; the calcination time is preferably 1h, 2h, or 3h, etc.

[0020] In some embodiments that may include the above embodiments, in step S3, the acid solution is at least one of nitric acid, sulfuric acid, hydrochloric acid, and phosphoric acid; or

[0021] The reducing agent is at least one of hydrogen peroxide, sodium bisulfite and glucose.

[0022] In some embodiments that may include the above embodiments, in step S4, the alkali metal hydroxide is sodium hydroxide and / or potassium hydroxide; or

[0023] The ammonium sulfite and the Mn in the clarified leaching solution 2+ The molar ratio is 1:1.

[0024] In some embodiments that may include the above embodiments, in step S2, the battery is disassembled and classified into a positive electrode material and a remaining part, wherein the remaining part includes a negative electrode material, an iron shell, a separator and an electrolyte.

[0025] The second aspect of the embodiment of the present application further provides a γ-crystal manganese-based catalyst, and the γ-crystal manganese-based catalyst is recovered by the above method.

[0026] The third aspect of the embodiments of the present application also provides the use of the above-mentioned γ-crystalline manganese-based catalyst in the treatment of VOCs in industrial tail gas.

[0027] The T-γ-MnO recovered in this embodiment of the present invention 2 The catalyst concentration in toluene was 1000 ppm and the space velocity was 60,000 mL·g -1 ·h -1 Under the conditions of 2 The conversion rate of toluene catalytic oxidation 90 and T 50 239℃ and 233℃ respectively; at 1000ppm chlorobenzene concentration and 60,000mL·g -1 ·h -1Under the conditions of 2 The conversion rate of toluene catalytic oxidation 90 and T 50 312℃ and 290℃ respectively; at a formaldehyde concentration of 1000ppm and a space velocity of 60,000mL·g -1 ·h -1 Under the conditions of 2 The conversion rate of toluene catalytic oxidation 90 and T 50 The temperature of α-MnO prepared from pure substances is 130℃ and 86℃ respectively. 2 In comparison, T 90 and T 50 Both have decreased significantly, and at the same time, the resource utilization of waste lithium batteries can be realized, which has good application prospects.

[0028] Compared with the prior art, the embodiments of the present application have the following beneficial effects:

[0029] 1. T-γ-MnO in the examples of this application 2 The catalyst is a manganese-based catalyst with a γ-crystal structure, and the number of mesopores in the catalyst is significantly increased, the specific surface area and pore volume are also greatly improved, and the adsorbed oxygen species are more abundant, so it has better low-temperature redox ability and VOCs catalytic activity;

[0030] 2. T-γ-MnO in the examples of this application 2 The synthesis of the catalyst is based on the recycling of waste lithium batteries, and adopts the idea of ​​treating waste with waste to degrade VOCs. The catalyst has a high catalytic efficiency in the process of catalyzing the decomposition of VOCs. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0032] Figure 1 The figure is a graph showing the conversion rates of toluene, chlorobenzene and formaldehyde of the catalysts prepared in Example 1 and Comparative Example 1;

[0033] Figure 2 The XRD patterns of the catalysts prepared in Example 1 and Comparative Example 1;

[0034] Figure 3 The SEM, TEM and HRTEM images of the catalysts prepared in Example 1 and Comparative Example 1 are shown. DETAILED DESCRIPTION

[0035] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0036] Unless otherwise specified, the experimental methods used in the examples of this application are all conventional methods.

[0037] In the following examples and comparative examples, unless otherwise specified, all raw materials can be obtained by commercial purchase or conventional methods.

[0038] Example 1

[0039] The method of recovering a γ-crystalline manganese-based catalyst from a waste lithium battery positive electrode material in this embodiment comprises the following steps:

[0040] (1) placing the waste ternary lithium battery (nickel-cobalt-manganese ternary lithium battery) cell in a 5% (v%) NaCl solution to fully discharge it;

[0041] (2) using a tool to saw open the battery shell, disassemble the battery and classify it into positive electrode material and remaining parts (negative electrode material, iron shell, separator and electrolyte); the positive electrode material is naturally dried in a fume hood, then cut into small square pieces, and calcined at 600°C in a muffle furnace to remove PVDF; the calcined positive electrode pieces are crushed by a pulverizer and sieved to finally obtain positive electrode active powder;

[0042] (3) Place the above positive electrode active powder in 100 mL 4 mol·L -1 H 2 SO 4 and 5 ml 30% HO 2 O 2 In the process, the leaching temperature is 70°C, the leaching time is 2h, the solid-liquid ratio is 20:1, and after the leaching is completed, the mixed solution is filtered through a filter membrane to obtain a clarified leachate;

[0043] (4) adding sodium hydroxide to 20 mL of the clarified leachate, stirring evenly, adjusting the pH of the clarified leachate to 3, then adding 0.98 g of sodium sulfite and a certain amount of deionized water to make the solution 100 mL, stirring evenly, and obtaining a mixed suspension A;

[0044] (5) The obtained suspension A is placed in a reactor with a polytetrafluoroethylene liner, and the reactor is placed in a forced air drying oven at 90°C for reaction for 24 hours. After the reaction is completed, the obtained sample is filtered and then rinsed with deionized water until the filtrate is neutral. The obtained filter residue is placed in a forced air drying oven at 60°C for drying for 24 hours. The dried sample is then placed in a muffle furnace, the heating rate is controlled to be 5°C / min, and calcined at 350°C for 2 hours. After calcination, the sample is ground to obtain T-γ-MnO 2 catalyst.

[0045] Example 2

[0046] The method for recovering a γ-crystalline manganese-based catalyst from waste lithium battery positive electrode materials provided in this embodiment can refer to Example 1, except that in step S3, the leaching conditions are: the leaching temperature is 60° C., and the leaching time is 5 h.

[0047] Example 3

[0048] The method for recovering a γ-crystalline manganese-based catalyst from waste lithium battery positive electrode materials provided in this embodiment can refer to Example 1, except that in step S3, the leaching conditions are: the leaching temperature is 80° C., and the leaching time is 1 hour.

[0049] Example 4

[0050] The method for recovering a γ-crystalline manganese-based catalyst from waste lithium battery positive electrode materials provided in this embodiment can refer to Example 1, except that in step S5, the hydrothermal reaction temperature is 80° C. and the hydrothermal reaction time is 30 h.

[0051] Example 5

[0052] The method for recovering a γ-crystalline manganese-based catalyst from waste lithium battery positive electrode materials provided in this embodiment can refer to Example 1, except that in step S5, the hydrothermal reaction temperature is 100° C. and the hydrothermal reaction time is 20 h.

[0053] Example 6

[0054] The method for recovering γ-crystalline manganese-based catalyst from waste lithium battery positive electrode materials provided in this embodiment can refer to Example 1, except that in step S5, the calcination heating rate is 2°C / min, the calcination temperature is 300°C, and the calcination time is 3h.

[0055] Example 7

[0056] The method for recovering γ-crystalline manganese-based catalyst from waste lithium battery positive electrode materials provided in this embodiment can refer to Example 1, except that in step S5, the calcination heating rate is 6°C / min, the calcination temperature is 450°C, and the calcination time is 1h.

[0057] Example 8

[0058] The method for recovering a γ-crystalline manganese-based catalyst from anode materials of waste lithium batteries provided in this embodiment can refer to Example 1, except that the reducing agent is glucose.

[0059] Comparative Example 1

[0060] The γ-crystalline manganese-based catalyst (γ-MnO 2 ), comprising the following steps:

[0061] (1) Take 0.98g sodium sulfite and 0.726g MnSO 4 ·H 2 O was dissolved in 100 mL of ultrapure water and stirred continuously for 30 min to obtain a stable suspension;

[0062] (2) The suspension was transferred to a reactor with a polytetrafluoroethylene liner, and the reactor was placed in a blast drying oven at 90°C for reaction for 24 hours. After the reaction, the obtained sample was filtered and then rinsed with deionized water until the filtrate was neutral. The obtained filter residue was placed in a blast drying oven at 60°C for drying for 24 hours. The dried sample was placed in a muffle furnace, the heating rate was controlled to be 5°C / min, and calcined at 350°C for 2 hours. After calcination, the γ-MnO was ground. 2 catalyst.

[0063] Activity test

[0064] The catalytic performance of different VOCs oxidation was studied in a fixed bed experimental device. The reactor is a quartz tube with an inner diameter of 6mm. The reaction temperature is controlled by a program temperature control device, and the temperature is measured by a self-prepared thermocouple. In the experiment, the initial concentration of various VOCs was set to about 1000ppm. High-purity liquid toluene was placed in an ice water bath. Toluene gas was formed by bubbling and then mixed with air in a buffer bottle for dilution. The catalyst dosage was 0.06g, and the particle size was 40-60 mesh, which was obtained by screening. The gas flow rate of each channel was controlled by a mass flow meter, and the total gas flow rate was controlled at 60mL min -1 The reaction gas hourly space velocity was set to 60000 mL·g -1 ·h -1 The test results are as follows: Figure 1 As shown in Table 1.

[0065] Table 1 Physical properties and catalytic performance of different catalysts

[0066]

[0067] Ⅰ The catalytic oxidation performance of toluene, Ⅱ The catalytic oxidation performance of chlorobenzene, ⅢIt has catalytic oxidation properties for formaldehyde.

[0068] Depend on Figure 1 As shown in Table 1, within the reaction temperature range of 180-300 °C, the 2D sheet-like structure of T-γ-MnO 2 The toluene conversion rate, chlorobenzene conversion rate and formaldehyde conversion rate of the 1D rod-shaped tunnel structure of γ-MnO 2 Among them, T-γ-MnO 2 Toluene conversion rate T 90 and T 50 At 239℃ and 233℃, γ-MnO 2 The conversion rate of toluene catalytic oxidation 90 and T 50 275℃ and 254℃; T-γ-MnO 2 Chlorobenzene conversion rate T 90 and T 50 At 312℃ and 290℃,γ-MnO 2 T of chlorobenzene conversion rate in catalytic oxidation 90 and T 50 340℃ and 319℃; T-γ-MnO 2 Formaldehyde conversion rate T 90 and T 50 At 130℃ and 86℃,γ-MnO 2 The conversion rate of formaldehyde in catalytic oxidation 90 and T 50 is 162℃ and 127℃. This indicates that T-γ-MnO 2 The catalyst has better catalytic activity for various VOCs at both high and low temperatures.

[0069] T-γ-MnO 2 The three doped metal elements Co, Ni and Li play an effect of strengthening the physical and chemical properties of the catalyst, making the sheet-like structure of T-γ-MnO 2 The number of mesopores increases significantly, and the specific surface area and pore volume also increase greatly. Therefore, T-γ-MnO 2 Outperforms γ-MnO 2 toluene catalytic activity.

[0070] Table 1 also shows that T-γ-MnO 2 ,γ-MnO 2 Physical properties of T-γ-MnO 2 ,γ-MnO 2 The specific surface areas are 79.4 and 26.4 m 2 ·g -1 .T-γ-MnO 2It has a larger specific surface area and pore volume, which is also related to its extremely low crystallinity. The higher specific surface area can provide more reaction sites, which is conducive to the reaction and can make the catalyst have higher catalytic performance.

[0071] In summary, the γ-crystalline manganese-based catalyst prepared by the present application based on the recycling of waste lithium batteries has a significantly increased number of mesopores, greatly improved specific surface area and pore volume, and has excellent VOCs catalytic activity.

[0072] Characterization Test

[0073] Figure 2 It shows that T-γ-MnO 2 ,γ-MnO 2 The XRD spectrum of the sample matches well with PDF#14-0644, indicating that γ-MnO was successfully prepared by using pure material in Comparative Example 1 and waste ternary lithium batteries in Example 1. 2 In addition, compared with Comparative Example 1, the MnO synthesized in Example 1 2 The diffraction peaks of are relatively weaker and broader, indicating that its crystallinity is lower and there may be more lattice defects.

[0074] Figure 3 (A1, A2) is γ-MnO 2 SEM spectrum of γ-MnO 2 It is composed of randomly stacked nanorods with smooth surfaces, and the diameter and length of a single nanorod are approximately 50-100nm and 1-2μm, respectively. Figure 3 (B1, B2) is T-γ-MnO 2 SEM spectrum of T-γ-MnO 2 It has a 2D flake structure with an average diameter of about 243nm. The TEM spectra of each sample are shown in Figure 3 (A3, B3), γ-MnO 2 、T-γ-MnO 2 Rod-like and sheet-like structures were observed in the samples, verifying the inference of SEM. HRTEM was used to further observe the lattice characteristics of each sample, such as Figure 3 (A4, B4) as shown. Figure 3 The lattice fringes in (A4 area) are clear and uniform, and the spacing between the two fringes is 0.24 nm, which is consistent with the γ-MnO 2 The interplanar spacing of the (131) plane is consistent. Figure 3 The lattice spacing of 0.24 nm in (B4 region) indicates that the main exposed crystal plane is T-γ-MnO 2 (131) crystal plane.

[0075] The waste ternary lithium battery (nickel-cobalt-manganese ternary lithium battery) powder, γ-MnO prepared in Comparative Example 12 and T-γ-MnO prepared in Example 1 2 The catalyst powder was soaked in aqua regia and heated to 110°C until the catalyst powder was completely dissolved. The obtained solution was filtered through a 0.45 um filter membrane, and the filtrate was fixed to 1 L and then tested for the metal ion composition and content in the solution using a plasma emission spectrometer. The results are shown in Table 2.

[0076] Table 2 ICP-OES results of clarified leachate and catalysts

[0077] sample Mn Co Ni Li <![CDATA[TLB leaching solution Ⅰ > 5350 872 1950 955 <![CDATA[γ-MnO 2 Ⅱ ]]> 56.2 — — — <![CDATA[T-γ-MnO 2 Ⅱ ]]> 45.0 4.17 10.38 2.18

[0078] In Table 2, the unit of Ⅰ is mg·L -1 ; ⅡThe unit is mass percentage (wt.%).

[0079] It can be seen from Table 2 that compared with γ-MnO 2 It contains a small amount of Ni, Co, and Li doping, from which it can be inferred that T-γ-MnO 2 The three doped metal elements have the effect of enhancing the physical and chemical properties of the catalyst.

[0080] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present application.

Claims

1. A method for recovering a γ-crystalline manganese-based catalyst from anode materials of waste lithium batteries, characterized in that: The following steps are involved: S1. Soak the used ternary lithium battery in a NaCl solution; S2, using tools to saw open the battery shell, disassemble and classify the batteries, wherein the positive electrode material is dried, cut, roasted, crushed and sieved to obtain positive electrode active powder; S3, selecting an acid solution and a reducing agent to leach the positive electrode active powder, and obtaining a clarified leachate after filtering; S4, adding alkali metal hydroxide to the clarified leachate, stirring evenly, adjusting the pH of the leachate, and then adding ammonium sulfite / sodium sulfite and deionized water, stirring evenly, to obtain a suspension A; S5, subjecting the suspension A to a hydrothermal reaction, and after the reaction is completed, performing solid-liquid separation, washing, drying, and calcining to obtain a γ-crystalline manganese-based catalyst.

2. The method for recovering a γ-crystalline manganese-based catalyst from anode materials of waste lithium batteries according to claim 1, characterized in that: In step S3, the leaching conditions are: leaching temperature is 60-80°C, leaching time is 1-5h, and solid-liquid ratio is 20:

1.

3. The method for recovering a γ-crystalline manganese-based catalyst from anode materials of waste lithium batteries according to claim 1, characterized in that: In step S5, the hydrothermal reaction temperature is 80-100° C., and the hydrothermal reaction time is 20-30 h.

4. The method for recovering a γ-crystalline manganese-based catalyst from anode materials of waste lithium batteries according to claim 1, characterized in that: In step S5, the drying temperature is 55-80°C and the drying time is 8-24h.

5. The method for recovering a γ-crystalline manganese-based catalyst from anode materials of waste lithium batteries according to claim 1, characterized in that: In step S5, the calcination heating rate is 2-6°C / min, the calcination temperature is 300-450°C, and the calcination time is 1-3h.

6. The method for recovering a γ-crystalline manganese-based catalyst from anode materials of waste lithium batteries according to claim 1, characterized in that: In step S3, the acid solution is at least one of nitric acid, sulfuric acid, hydrochloric acid, and phosphoric acid; or The reducing agent is at least one of hydrogen peroxide, sodium bisulfite and glucose.

7. The method for recovering a γ-crystalline manganese-based catalyst from anode materials of waste lithium batteries according to claim 1, characterized in that: In step S4, the alkali metal hydroxide is sodium hydroxide and / or potassium hydroxide; or The ammonium sulfite and the Mn in the clarified leaching solution 2+ The molar ratio is 1:

1.

8. The method for recovering a γ-crystalline manganese-based catalyst from anode materials of waste lithium batteries according to claim 1, characterized in that: In step S2, the battery is disassembled and classified into a positive electrode material and a remaining part, wherein the remaining part includes a negative electrode material, an iron shell, a separator and an electrolyte.

9. A γ-crystalline manganese-based catalyst, characterized in that: The gamma crystalline manganese-based catalyst is recovered by the method described in any one of claims 1 to 8.

10. Use of the gamma-crystalline manganese-based catalyst according to claim 9 in treating VOCs in industrial tail gas.

Citation Information

Patent Citations

  • Method and applications thereof for recovering MnO* from anode material of wasted lithium manganate battery

    CN101538655A

  • Preparation method of super-capacitor manganese oxide material

    CN101950682A

  • Preparation method and use of nano-manganese oxide by utilizing waste battery

    CN104261480A

  • Method for preparing sigma and gamma-MnO2 from lithium ion battery anode wastes

    CN106517343A

  • Method for leaching metals in anode material of waste lithium ion battery

    CN108486376A

Cited By

  • Preparation method of modified manganese slag catalyst for catalyzing VOCs (Volatile Organic Compounds)

    CN120515437A