Preparation method and application of novel Fe-coated S-1 catalytic material

The Fe@S-1 catalytic material was prepared by hydrothermal method of zero-valent Fe in the limited domain in silicon molecular sieve, and the oxidation and agglomeration of nano-iron particles in electrocatalysis was solved, the removal rate and catalytic activity of nitrate were improved, and the removal rate and catalytic activity of nitrate were achieved. Efficient electrocatalytic reduction effect.

CN118925782AActive Publication Date: 2024-11-12CHANGCHUN INST OF TECH

Patent Information

Application Number
CN202410985784.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-12
Estimated Expiration
2044-07-23

AI Technical Summary

Technical Problem

In electrocatalysis, nanoferrous particles have problems such as oxide film formation, high surface energy leading to agglomeration, reduced active sites and poor catalytic activity, which cannot be compared with high-active precious metals, and the center position of the d-band of zero-valent iron affects nitrate. adsorption efficiency.

Method used

The Fe@S-1 catalytic material was prepared by hydrothermal method. By limiting the sub-nano zero-valent Fe in the silicon molecular sieve, avoiding the agglomeration of iron particles, regulating the center position of the d-band of Fe, improving the adsorption performance of nitrates, and preparing green A non-contamination catalyst.

Benefits of technology

The removal rate of nitrate is significantly improved, the deactivation of the catalyst is delayed, and the efficient electrocatalytic reduction effect is achieved, and good cycle stability and high specific surface area are demonstrated.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118925782A_ABST
    Figure CN118925782A_ABST
Patent Text Reader

Abstract

The invention is applicable to the technical field of environmental engineering water treatment, and provides a preparation method and application of a novel Fe-coated S-1 catalytic material, and the preparation method comprises the following steps: mixing 4.06 g of tetrapropylammonium hydroxide with 32mL of ultrapure water; continuously stirring for 10 minutes, adding 2.6 g of tetraethoxysilane, and stirring for 6 hours to obtain a mixture 1; mixing 0.909 g of iron nitrate nonahydrate, 0.4 mL of ethidene diamine and 4mL of ultrapure water, and stirring for 10 minutes to obtain a mixture 2; dropwise adding the mixture 2 into the mixture 1, stirring for 30 minutes under a precipitation-free condition, then putting into a high-pressure kettle, and carrying out hydrothermal synthesis for 4 days at 170 DEG C; and centrifugally separating and collecting the product, washing with ethanol for 3 times, washing with ultrapure water for 3 times, drying at 80 DEG C for 12 hours, and calcining the product in a hydrogen-argon mixed atmosphere at 550 DEG C for 8 hours to fully reduce. The catalytic material is green and pollution-free and can improve the adsorption performance on nitrate, so that the electro-catalytic removal rate of the nitrate is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of environmental engineering water treatment, and in particular relates to a preparation method of a novel Fe@S-1 catalytic material and application thereof. Background Art

[0002] The diversification and extensive use of nitrogen-containing substances in industry and agriculture have disrupted the nitrogen balance in the environment, leading to the accumulation of nitrate (NO3 – ) pollution is becoming increasingly serious. Survey data on nitrates in deep and shallow groundwater in 52 basin-scale groundwater systems across the country show that among the shallow aquifers in 36 major basins, 90% of the survey points in 25 basins exceed my country's drinking water quality standards; among the deep or karst aquifers in 37 major basins, nitrates in aquifers in 10 basins exceed the standard. The increase in nitrate concentrations seriously affects the aquatic ecosystem, leading to eutrophication and hypoxia of water bodies. In addition, excessive nitrate concentrations in drinking water increase the risk of infection with diseases such as methemoglobinemia, diabetes, spontaneous abortion, thyroid disease, and gastric cancer. Therefore, water bodies with excessive nitrates need to be urgently treated.

[0003] Electrocatalysis is an emerging technology for treating excessive nitrate in water, which is favored by the public due to its mild operating conditions and good efficiency. Among them, the catalytic activity of the cathode catalyst material greatly affects the nitrate removal efficiency. Nano-iron-based catalysts have become an ideal catalytic material for electrocatalytic reduction of nitrates due to their unique advantages (cheap and easy to obtain, green and harmless, and excellent catalytic performance).

[0004] However, when nano-iron particles are directly used for electrocatalytic removal of nitrate, there are several problems:

[0005] (1) At room temperature, nano-iron particles will be oxidized in the air, and a dense oxide film will easily form on the surface, which will hinder the catalytic reaction.

[0006] (2) The surface energy of nano-iron particles is high and they are easy to agglomerate, resulting in a reduction in active sites and thus lowering the catalytic activity.

[0007] (3) Conventional iron catalysts have poor activity and cannot compete with more active precious metals (such as ruthenium).

[0008] These problems are related to the size, valence state and d-band center of the iron particles. For example, the size of nano-iron particles is crucial to their performance. Smaller particles usually have a larger specific surface area and are therefore more likely to interact with other particles. Zero-valent iron exists in the form of pure elemental metal. Compared with high-valent iron in conventional catalysts, it does not form chemical bonds with other elements. There are abundant active sites on the surface that can adsorb and catalyze reactions. These sites contribute to the electrocatalytic reduction and removal of nitrates. The closer the d-band center of iron is to the Fermi level, the stronger the adsorption of nitrates, thereby improving the efficiency of electrocatalytic removal of nitrates. Therefore, a new type of iron-based sub-nano catalyst structure is proposed to solve the problems encountered when using nano-iron particles as catalytic materials by regulating the size, valence state and d-band center of iron particles. Summary of the invention

[0009] The purpose of the embodiments of the present invention is to provide a preparation method of a novel Fe@S-1 catalytic material and its application, aiming to solve the problems raised in the above background technology.

[0010] The embodiment of the present invention is implemented as follows: a method for preparing a novel Fe@S-1 catalytic material, wherein the preparation of the Fe@S-1 catalyst is carried out by a hydrothermal method, specifically comprising the following steps:

[0011] Step 1, 4.06 g of tetrapropylammonium hydroxide was mixed with 32 mL of ultrapure water; after continuous stirring on a magnetic stirrer for 10 min, 2.6 g of ethyl orthosilicate was added and stirred for 6 h to obtain a clear mixture 1;

[0012] Step 2, 0.909 g of ferric nitrate nonahydrate, 0.4 mL of ethylenediamine and 4 mL of ultrapure water were mixed and stirred for 10 minutes to obtain a mixture 2;

[0013] Step 3, adding mixture 2 dropwise to mixture 1, stirring for 30 min without precipitation, and then placing in an autoclave for hydrothermal synthesis at 170° C. for 4 days;

[0014] Step 4: The obtained product was centrifuged and collected, washed with ethanol three times, washed with ultrapure water three times, dried at 80°C for 12 hours, and the collected product was calcined at 550°C in a hydrogen-argon mixed gas atmosphere for 8 hours for full reduction. The obtained powder was ground and named Fe@S-1.

[0015] In a further technical solution, in step 4, the volume ratio of hydrogen to argon in the hydrogen-argon mixed gas is V H2 :V Ar =5:95.

[0016] Another object of an embodiment of the present invention is to provide an application of a new Fe@S-1 catalytic material, wherein the Fe@S-1 catalytic material is applied to the electrocatalytic treatment of nitrates, and an electrode sheet and a platinum sheet prepared using Fe@S-1 are used as a cathode and an anode, respectively.

[0017] A further technical solution is a method for preparing an electrode sheet based on Fe@S-1, comprising the following steps:

[0018] Firstly, Fe@S-1 composite material, conductive carbon black and polyvinylidene fluoride in a mass ratio of 8:1:1 were weighed, and then the mixture was dissolved in N,N-dimethylformamide, and the concentration of the mixture was controlled to be 10 g / L to prepare catalyst ink. The ink was then coated on a 1.0 cm × 2.0 cm carbon cloth to ensure that both sides were evenly coated, and then dried at 60°C for 30 minutes to obtain a working electrode sheet.

[0019] The present invention provides a method for preparing a novel Fe@S-1 catalytic material and its application. The method confines sub-nanometer zero-valent Fe in a silicon molecular sieve to reduce the leaching of iron metal and ensure an extremely low content of iron ions in the treated water, thereby preparing a green and pollution-free material. The direct contact between zero-valent Fe and a highly corrosive environment is blocked, thereby delaying and preventing the deactivation of the catalyst. In addition, nano-confinement can avoid the agglomeration of small-sized iron particles, move the d-band center of Fe upward, and effectively overlap the 3d orbital of Fe with the 2p orbital of O of nitrate, thereby improving the adsorption performance of nitrate, thereby improving the removal rate of nitrate. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 A preparation flow chart of a novel Fe@S-1 catalytic material provided in an embodiment of the present invention;

[0021] Figure 2 This is a technical schematic diagram of the electrocatalytic removal of nitrate from water based on Fe@S-1 catalytic material;

[0022] Figure 3 It is a diagram of the reaction device based on Fe@S-1 catalytic material;

[0023] Figure 4 SEM images of Fe@S-1 and Fe / S-1, where a is Fe@S-1 and b is Fe / S-1;

[0024] Figure 5 TEM images of Fe@S-1 and Fe / S-1, where a is Fe@S-1 and b is Fe / S-1;

[0025] Figure 6 is the EDX image of Fe@S-1;

[0026] Figure 7is the XPS spectrum of Fe@S-1;

[0027] Figure 8 BET results of Fe@S-1 and S-1, where a is Fe@S-1 and b is S-1;

[0028] Fig. 9 Electrochemical impedance spectra of Fe@S-1, Fe / S-1 and S-1;

[0029] Fig.10 Linear sweep voltammetry curves (vs. RHE) of different materials;

[0030] Fig.11 is the Tafel slope (vs. RHE) of different materials;

[0031] Fig.12 The degradation effect of nitrate and the yield and conversion rate of ammonia nitrogen in the process of electrocatalytic reduction of nitrate;

[0032] Fig.13 is the change in nitrite concentration during the degradation process;

[0033] Fig.14 is the cycle performance of Fe@S-1 catalyst;

[0034] Fig.15 The electrocatalytic degradation effect of nitrate on different materials;

[0035] Fig.16 The effect of different current density on the electrocatalytic reduction of nitrate;

[0036] Fig.17 The effect of different pH on the electrocatalytic reduction of nitrate;

[0037] Fig.18 The effect of different initial nitrate concentrations on the electrocatalytic reduction of nitrate;

[0038] Fig.19 The effects of different ions and concentrations on the electrocatalytic reduction of nitrate;

[0039] Fig. 20 Electrocatalytic reduction of NO3 by Fe@S-1 - The reaction path of

[0040] Fig.21 is the reaction process and the change in Gibbs free energy of the reaction;

[0041] Fig. 22 Adsorption of NO3 by Fe@S-1 and Fe / S-1 - The overall differential charge and adsorption energy of , where a is Fe@S-1 and b is Fe / S-1;

[0042] Fig.23 is the Fe d orbital partial wave state density of Fe@S-1 and Fe / S-1, where a is Fe@S-1 and b is Fe / S-1. DETAILED DESCRIPTION

[0043] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0044] The specific implementation of the present invention is described in detail below in conjunction with specific embodiments.

[0045] like Figure 1 As shown, a method for preparing a novel Fe@S-1 catalytic material provided by an embodiment of the present invention, wherein the preparation of the Fe@S-1 catalyst is carried out by a hydrothermal method, specifically comprising the following steps:

[0046] Step 1, 4.06 g of tetrapropylammonium hydroxide was mixed with 32 mL of ultrapure water; after continuous stirring on a magnetic stirrer for 10 min, 2.6 g of ethyl orthosilicate was added and stirred for 6 h to obtain a clear mixture 1;

[0047] Step 2, 0.909 g of ferric nitrate nonahydrate, 0.4 mL of ethylenediamine and 4 mL of ultrapure water were mixed and stirred for 10 minutes to obtain a mixture 2;

[0048] Step 3, adding mixture 2 dropwise to mixture 1, stirring for 30 min without precipitation, and then placing in an autoclave for hydrothermal synthesis at 170° C. for 4 days;

[0049] Step 4: The obtained product was centrifuged and collected, washed with ethanol three times, washed with ultrapure water three times, dried at 80°C for 12 hours, and the collected product was calcined at 550°C in a hydrogen-argon mixed gas atmosphere for 8 hours for full reduction. The obtained powder was ground and named Fe@S-1.

[0050] Another embodiment of the present invention provides an application of a novel Fe@S-1 catalytic material, wherein the Fe@S-1 catalytic material is applied to the electrocatalytic treatment of nitrates. The technical principle of electrocatalytic removal of nitrates in water based on the Fe@S-1 catalytic material is as follows: Figure 2 The electrocatalytic reduction of nitrate was tested in a single-chamber electrolytic cell using a two-electrode system. Figure 3 shown; specifically:

[0051] The electrode sheet and platinum sheet prepared by Fe@S-1 were used as cathode and anode respectively, and the distance between the two plates was controlled to be 0.5-2.0cm; the electrolyte was a nitrate solution with a concentration of 50mg / L (in terms of N) prepared by using NaNO3. The reason for choosing a concentration of 50mg / L is that the concentration of nitrate in the nitrate-contaminated groundwater actually collected is 55mg / L, which is approximately 50mg / L in the simulation experiment. The nitrate content of the water sample at each time point was measured using ion chromatography, and the nitrate removal rate was calculated.

[0052] In an embodiment of the present invention, the electrocatalytic removal of nitrates was carried out in a single-chamber electrolytic cell (50 mL) using a GPS305D DC regulated power supply. In the two-electrode system, the platinum sheet was used as the anode and the electrode sheet prepared by Fe@S-1 was used as the cathode. 30 mL of the electrolyte contained 50 mg / L nitrate (in terms of N) and 0.21 g Na2SO4. A current of 50 mA was applied to the system, and samples were taken every 30 min. The nitrate content of the water samples at each time point was measured using ion chromatography, and the nitrate removal rate was calculated. Under optimal conditions, 94.6% of nitrates can be degraded within 3 h. At the same time, the Fe@S-1 catalyst has good cyclic stability, and there is still a degradation rate of 92.3% after repeated use for 5 times.

[0053] As shown in Table 1, the nitrate reduction performance of different electrocatalytic materials was compared. The nitrate removal rate of the catalytic material Fe@S-1 prepared by this method reached 94.6%, and in just 3 hours, which is much lower than the time required for other catalytic materials. The nitrate removal efficiency is much higher than other iron-based and metal catalysts, and the ammonia selectivity is also 56%. This shows the excellent performance of Fe@S-1 and the amazing nitrate removal efficiency.

[0054] Table 1. Reduction of NO3 by different electrocatalytic materials - Performance comparison

[0055]

[0056] As a preferred embodiment of the present invention, the preparation method of the working electrode based on Fe@S-1 comprises the following steps:

[0057] Firstly, Fe@S-1 composite material, conductive carbon black and polyvinylidene fluoride in a mass ratio of 8:1:1 were weighed, and then the mixture was dissolved in N,N-dimethylformamide, and the concentration of the mixture was controlled to be 10 g / L to prepare catalyst ink. The ink was then coated on a 1.0 cm × 2.0 cm carbon cloth (CC) to ensure that both sides were evenly coated, and then dried at 60°C for 30 minutes to obtain a working electrode sheet.

[0058] Several specific examples are provided below to verify the feasibility of this method:

[0059] Embodiment 1:

[0060] 1. Preparation of catalytic materials:

[0061] (1) Preparation of S-1 silicon molecular sieve:

[0062] The preparation of silicon molecular sieve S-1 is carried out by hydrothermal method. The specific operation process is as follows: 4.06g of tetrapropylammonium hydroxide is mixed with 32mL of ultrapure water. After continuous stirring on a magnetic stirrer for 10 minutes, 2.6g of ethyl orthosilicate is added and stirred for 6 hours to obtain a clear mixture. Then it is placed in an autoclave and hydrothermally synthesized at 170°C for 4 days. The obtained product is centrifuged and collected, washed with ethanol 3 times, washed with ultrapure water 3 times, and dried at 80°C for 12 hours. The collected product is ground into powder and named S-1. S-1 is the prepared silicon molecular sieve reference material.

[0063] (2) Preparation of Fe@S-1 catalyst

[0064] The preparation of Fe@S-1 catalyst was carried out by hydrothermal method, and the specific operation process was as follows: 4.06g of tetrapropylammonium hydroxide was mixed with 32mL of ultrapure water. After continuous stirring on a magnetic stirrer for 10 minutes, 2.6g of tetraethyl orthosilicate was added and stirred for 6 hours to obtain a clear mixture 1. 0.909g of ferric nitrate nonahydrate, 0.4mL of ethylenediamine, and 4mL of ultrapure water were mixed and stirred for 10 minutes to obtain mixture 2, and mixture 2 was added dropwise to mixture 1, stirred for 30 minutes without precipitation, and then placed in an autoclave for hydrothermal synthesis at 170°C for 4 days. The obtained product was centrifuged and collected, washed with ethanol 3 times, washed with ultrapure water 3 times, dried at 80°C for 12 hours, and the collected product was heated at 550°C in a hydrogen-argon mixture (V H2 :V Ar =5:95) atmosphere for 8 h to fully reduce the product, and the obtained powder was ground and named Fe@S-1.

[0065] (3) Preparation of Fe / S-1 catalyst

[0066] The Fe / S-1 catalyst was prepared by a similar method, except that the iron-ethylenediamine-water mixture was not added first. After the S-1 molecular sieve was prepared, 0.1 g of the ground molecular sieve was mixed with the iron-ethylenediamine-water mixture by impregnation, then dried at 80°C for 12 hours, ground again, calcined at 550°C in a hydrogen-argon mixed gas atmosphere for 8 hours, fully reduced, and the product was collected and ground again. The powder product was named Fe / S-1. Fe / S-1 is a non-confined control material prepared.

[0067] 2. Characterization of Catalysts

[0068] 1) Scanning electron microscopy (SEM)

[0069] SEM images of Fe@S-1 catalyst and Fe / S-1 catalyst are shown in Figure 2. Figure 4 a and Figure 4 As shown in b. Figure 4 a It can be clearly observed that the Fe@S-1 catalyst has a round and irregular appearance, with only a portion of the hexagonal structure remaining. This is the effect caused by the confinement of Fe in the S-1 molecular sieve, which results in a rough surface, blurred edges, and distorted morphology of the molecular sieve. Figure 4 b shows the SEM image of Fe / S-1, which clearly shows that it has sharp edges and corners, regular shape, and a very standard hexagonal structure, which is highly similar to the SEM image of S-1 molecular sieve, and does not show the influence of the interaction between iron and molecular sieve. At the same time, it can be seen from the SEM image that the size of a single Fe@S-1 and a single Fe / S-1 is relatively close, with a size of about 200nm to 1μm.

[0070] 2) Transmission electron microscopy (TEM)

[0071] TEM images such as Figure 5 a and Figure 5 As shown in b. Figure 5 The surface of Fe@S-1 in a is clean and tidy, and there is no Fe residue on the surface of the zeolite, but the shape is round and irregular as in the SEM image. This proves that the Fe in Fe@S-1 has successfully entered the interior of the molecular sieve, and the interaction between the two causes morphological distortion. Figure 5 In b, the TEM image of Fe / S-1 clearly shows that there are clusters of particles on the surface of the zeolite. These are the Fe elements gathered on the surface of the zeolite. Because Fe cannot enter the zeolite and only stays on its surface, the internal structure of the zeolite is not affected, and a clear and angular regular hexagonal structure can still be seen.

[0072] 3) Energy dispersive X-ray spectroscopy (EDX)

[0073] The element distribution of Fe@S-1 samples was determined by EDX, such as Figure 6 As shown. It can be seen that O, Si and Fe elements are evenly distributed in almost the same position, indicating that Fe is successfully confined into the S-1 molecular sieve. Among them, O and Si elements are more dense, because they are the components of the molecular sieve. The Fe element is more dispersed than the former two, which indicates that the Fe confined into the molecular sieve will not gather together to form clusters, which is beneficial to increase the reaction contact area and improve the catalyst activity.

[0074] 4) X-ray Photoelectron Spectroscopy (XPS)

[0075] The valence state of Fe was carefully analyzed by XPS. The results are as follows: Figure 7 As shown. In the XPS Fe 2p spectrum, there is a peak at 707.4eV and a peak at 721.4eV, which correspond to zero-valent Fe. This also proves that the Fe@S-1 catalyst with zero-valent Fe has been successfully synthesized.

[0076] 5) Fully automatic physical adsorption test (BET)

[0077] pass Figure 8 From the BET results, it can be seen that Fe@S-1 and S-1 are type IV isotherms, and an adsorption hysteresis loop appears in the middle section, which corresponds to a system in which capillary condensation occurs in the porous adsorbent. The adsorption hysteresis loop is an H3 type hysteresis loop. The pores reflected by the H3 type include flat slit structures, cracks, and wedge structures, etc., and no adsorption saturation is shown in the higher relative pressure area. The most probable pore size of Fe@S-1 is 38.260nm, while the most probable pore size of S-1 is 83.697nm. The pore size of Fe@S-1 is reduced, indicating that zero-valent iron is successfully confined into the silicon molecular sieve. And the BET area of ​​Fe@S-1 is 187.289m 2 / g is much higher than the BET area of ​​S-1, 26.668m 2 / g, Fe@S-1 has a higher specific surface area and more active sites, which is more conducive to improving the catalytic activity.

[0078] 6) Electrochemical impedance spectroscopy (EIS)

[0079] In order to obtain the electrochemical performance of Fe@S-1 catalyst, the catalytic materials Fe@S-1, Fe / S-1, and S-1 were applied to carbon cloth (1.0×2.0 cm) to obtain working electrodes (Fe@S-1 / CC, Fe / S-1 / CC, and S-1 / CC). The electrochemical characterization of Fe@S-1 catalyst and other catalysts was carried out by electrochemical workstation. EIS results are shown in Figure 2. Fig. 9 As shown, the semicircle diameter of Fe@S-1 / CC in the high-frequency region is smaller than that of Fe / S-1 / CC, indicating that the electrochemical impedance of Fe@S-1 / CC is smaller, which means that the charge transfer rate of Fe@S-1 catalyst is higher and more conducive to the electrocatalytic reduction of nitrate.

[0080] 7) Linear Sweep Voltammetry (LSV)

[0081] The LSV curves of Fe@S-1 / CC, Fe / S-1 / CC, S-1 / CC and CC were determined by LSV. Fig.10 As shown. It can be seen that the Fe@S-1 catalyst has a higher linear sweep voltammetry current. Fig.10From the electrochemical impedance spectrum, it can be found that the Fe@S-1 catalyst has a smaller impedance and a larger current, which indicates that the Fe@S-1 catalyst has excellent conductivity, which is conducive to the transfer of electrons from the cathode to the Fe@S-1 catalyst surface, thereby significantly improving the catalytic activity of the electrocatalytic reduction process.

[0082] 8) Tafel curve

[0083] The Tafel curves of Fe@S-1 / CC, Fe / S-1 / CC, S-1 / CC and CC were measured. The results are as follows: Fig.11 The Tafel slope indicates the change in overpotential required when the current changes tenfold, so the smaller the absolute value of the slope, the better. The smaller the slope, the smaller the voltage rise and the lower the energy consumption. Fig.11 It can be seen that the absolute value of the Tafel slope of the Fe@S-1 catalyst is the smallest, followed by Fe / S-1 and S-1, and the absolute value of the Tafel slope of pure carbon cloth is the largest, which indicates that the reaction kinetics of the Fe@S-1 catalyst is faster and has the best catalytic activity.

[0084] Embodiment 2:

[0085] (1) Nitrate degradation effect and ammonia nitrogen production and conversion rate during electrocatalytic reduction of nitrate

[0086] All electrocatalytic nitrate removal experiments were conducted in a single-chamber electrolytic cell (50 mL) using a GPS305D DC regulated power supply. In the two-electrode system, a platinum sheet was used as the anode, and the prepared Fe@S-1 catalytic material was coated on a 1.0×2.0 cm carbon cloth as the cathode, and the distance between the two plates was controlled to be 0.5-2.0 cm. 30 mL of electrolyte contained 50 mg / L NO3 - (in terms of N) and 0.21g Na2SO4. A 50mA current was applied to the system, and samples were taken every 30min. The NO3 content of the water samples at each time point was measured using ion chromatography. - content, and calculate NO3 - The removal rate was determined by Nessler's reagent spectrophotometry, and the ammonia nitrogen concentration in the reaction process was determined, and the ammonia nitrogen conversion rate was calculated. The experimental conditions and operating steps were kept unchanged and the experiment was repeated three times to obtain the nitrate degradation effect and the ammonia nitrogen production and conversion rate during the electrocatalytic reduction of nitrate.

[0087] pass Fig.12It can be seen that after 3 hours of reaction, the degradation rate of nitrate by Fe@S-1 catalyst has reached 94.6%, showing excellent nitrate removal ability. In addition, it can be seen that the ammonia nitrogen conversion rate has been fluctuating around 50%, indicating that 56% of the nitrate degraded at the end of the reaction is converted into ammonia nitrogen, and the remaining 44% is converted into N2. N2 contains two N atoms, so the generation reaction of N2 is a secondary reaction and is always limited by the secondary reaction. Since NO3 - Many intermediates (such as NO2 - ) carries a negative charge and is easily repelled by the electric field, making it difficult to accumulate on the cathode, thereby inhibiting the occurrence of the secondary reaction to generate N2, so more ammonia nitrogen is produced relative to N2.

[0088] (2) Changes in nitrite concentration during degradation

[0089] The rate of nitrate reduction to nitrite is the core of the nitrate reduction process and controls the entire nitrate reduction kinetics. However, nitrite is much more harmful than nitrate. Therefore, a qualified electrochemical reduction and degradation of nitrate reaction process should not have nitrite residue. Fig.13 The concentration change of nitrite during the electrochemical degradation process was measured by ion chromatography. It can be seen that the nitrite concentration at the initial 0h and the final 3h is 0, and only a very small amount of nitrite is generated as an intermediate product in the middle process. This shows that there will be no nitrite residue after the degradation is completed, and it will not cause secondary pollution and other problems.

[0090] (3) Catalyst cycle performance

[0091] During the use of Fe@S-1 catalyst, if the catalyst is passivated due to the influence of internal and external environment, the reaction efficiency will be greatly reduced, affecting the continuous progress of the catalytic reaction. In order to further characterize the stability of Fe@S-1 catalyst, 5 cycle experiments were carried out. During the experiment, the electrode sheet was carefully cleaned and dried after each electrocatalytic degradation, and then the electrode sheet was continued to be put into the electrocatalytic reduction system to repeatedly degrade new nitrate. The experimental conditions were 50mg / L (in terms of N) nitrate, 0.05A current (25mA / cm 2 The experimental results are shown in Figure 2. Fig.14 As shown. Fig.14 It can be seen that the nitrate degradation rates of the Fe@S-1 catalyst within 3 h after being reused for 5 times were 94.6%, 91.8%, 93.2%, 93.1%, and 92.5%, respectively. The degradation rate did not decrease significantly, indicating that the Fe@S-1 catalyst has good cyclic stability.

[0092] (4) Nitrate electrocatalytic degradation effect of different materials

[0093] In order to explore the influence of confinement effect on the electrocatalytic reduction degradation process of nitrate, the operation steps and other degradation conditions in Example 1 were kept unchanged, and 1.0×2.0 cm Fe@S-1, Fe / S-1, S-1 and CC were used as cathodes to carry out degradation experiments. The degradation rate of nitrate when using different materials was measured after 4 hours of degradation. The experimental conditions and operation steps were kept unchanged, and the experiment was repeated three times to obtain the degradation rate of nitrate when using different materials. The results are shown in the figure. Fig.15 shown.

[0094] from Fig.15 It can be seen that the degradation rate of nitrate by Fe@S-1 catalyst has reached 94.6% after 3h of reaction, while the degradation rate of nitrate by Fe / S-1 catalyst after 4h of reaction is only 72.3%. As for the degradation rates of nitrate by S-1 molecular sieve alone and carbon cloth alone after 4h, they are 36.9% and 35.6% respectively. S-1 molecular sieve itself has no catalytic activity, and like carbon cloth, it can only rely on cathode current to reduce nitrate in solution, so the degradation effect is highly similar. Fe@S-1 catalyst removed up to 94.6% of nitrate in just 3 hours, showing an amazing removal efficiency, which is much higher than other similar catalysts, such as Fe(20%)@NC prepared by Duan, which can only remove 83% of nitrate in 24 hours. Therefore, Fe@S-1 is an excellent catalytic material for electrocatalytic reduction of nitrate.

[0095] Example 3:

[0096] In the electrocatalytic reduction process, current density is undoubtedly an important factor affecting the reaction. In order to verify the effect of current density on the electrocatalytic reduction of nitrate, the current density was controlled to 0 mA / cm 2 , 5mA / cm 2 , 15mA / cm 2 , 25mA / cm 2 、35mA / cm 2 , 50mA / cm 2 The degradation experiment was carried out by keeping the operation steps and other degradation conditions in Example 1 unchanged, and then the experiment was repeated three times with the experimental conditions and operation steps completely unchanged. The results are as follows: Fig.16 shown.

[0097] from Fig.16 It can be seen that the current density is 25mA / cm 2 The degradation effect is the best when the current density is from 0mA / cm 2 Up to 25mA / cm 2During the process, the degradation effect continued to improve, but the increase was getting smaller and smaller. 2 The degradation effect decreased slightly when the current was too high. This may be because the voltage in the reaction system was too high when the current was too high, resulting in a large number of side reactions. The higher current density may have accelerated the cathode hydrogen evolution reaction, thereby + The Fe@S-1 catalyst surface provides more active sites, which affects the electrocatalytic reduction of nitrate. Therefore, the optimal current density for electrocatalytic removal of nitrate using the catalytic material Fe@S-1 is 25 mA / cm 2 .

[0098] Example 4:

[0099] In order to explore the effect of the initial pH of the reaction system on the electrocatalytic reduction degradation of nitrate, in order to avoid side reactions, the pH of the reaction system was adjusted using appropriate amounts of H2SO4 and NaOH. Under different conditions of pH 3, 5, 7, 9, and 11, the degradation experiment was carried out while keeping the operating steps and other degradation conditions in Example 1 unchanged. Then, the experiment was repeated three times while keeping the experimental conditions and operating steps completely unchanged. The results are as follows: Fig.17 shown.

[0100] from Fig.17 It can be seen that the degradation effect is best under the condition of pH = 7, and 94.6% of nitrate can be degraded after 3 hours of reaction. There is a slight effect at pH = 5, but the degradation effect at pH = 7 can be achieved after 4 hours of degradation. At pH = 3, 9, and 11, the degradation rate at 4 hours finally dropped to about 90%, indicating that pH has a certain effect on the degradation process. This may be because pH will change the existence form of Fe@S-1 catalyst, but Fe@S-1 is an iron-based catalyst confined on a molecular sieve, and the Fe in it has strong stability because of the protection of the molecular sieve, so the effect of pH on the degradation effect is not significant. This shows that the electrocatalytic reduction system of the Fe@S-1 catalyst weakens the interference of pH. Therefore, the optimal pH value for electrocatalytic removal of nitrate using the catalytic material Fe@S-1 is 7.

[0101] Example 5:

[0102] In order to explore the effect of initial nitrate concentration on the electrocatalytic reduction degradation process of nitrate, the electrocatalytic degradation test was carried out under the conditions of controlling the nitrate concentration to be 5 mg / L, 10 mg / L, 20 mg / L, and 50 mg / L (all in terms of N), and the degradation experiment was carried out while keeping the operating steps and other degradation conditions in Example 1 unchanged. Then, the experiment was repeated three times while keeping the experimental conditions and operating steps completely unchanged. The results are as follows: Fig.18 shown.

[0103] from Fig.18 It can be seen that different initial concentrations within a certain range do not affect the nitrate degradation effect. After 3 hours of reaction, about 95% of nitrate was removed in the reaction system with different concentrations. Subsequent experiments were carried out under the condition of an initial concentration of 50 mg / L.

[0104] Example 6:

[0105] In order to explore the effect of different initial chloride ion concentrations, initial carbonate concentrations and initial carbonate concentrations on the electrocatalytic reduction degradation process of nitrate, the electrocatalytic degradation test was carried out under the conditions of controlling the ion concentrations to be 0, 5mmol / L and 20mmol / L, and the degradation experiment was carried out while keeping the operating steps and other degradation conditions in Example 1 unchanged. Then, the experiment was repeated three times while keeping the experimental conditions and operating steps completely unchanged. The results are as follows Fig.19 shown.

[0106] from Fig.19 It can be seen that different initial chloride ion concentrations have a certain effect on the nitrate degradation effect. After 4 hours of reaction, the nitrate removal rates under the conditions of 5mmol / L and 20mmol / L chloride ions were 89.7% and 88.4%, respectively. This may be because Cl - The presence of will cause side reactions in the reaction system to generate Cl2, thus affecting the removal effect of nitrate. Different initial carbonate concentrations have a certain effect on the nitrate degradation effect. After 4 hours of reaction, the nitrate removal rates under the conditions of 5mmol / L and 20mmol / L carbonate were 92.1% and 80.4%, respectively. This may be because carbonate will also bring side reactions, affecting the degradation effect of nitrate. At the same time, adding carbonate will further affect the pH of the reaction system, so it has a greater impact on the degradation effect than chloride ions. Different initial bicarbonate concentrations have a very small effect on the nitrate degradation effect. After 4 hours of reaction, the nitrate removal rates under the conditions of 5mmol / L and 20mmol / L carbonate were 94.5% and 92.8%, respectively. This may be because although bicarbonate will also bring side reactions and slightly affect the degradation effect of nitrate, bicarbonate is a pH buffer and has little effect on pH. At the same time, the added bicarbonate reaction requires very few electrons, so it has little effect on the degradation effect. Therefore, different ions and concentrations in water have little effect on the electrocatalytic performance of Fe@S-1 in removing nitric acid.

[0107] Example 7:

[0108] Based on the previous characterization results, density functional theory (DFT) calculations were performed to investigate the reaction mechanism and reveal the reasons for the high performance of Fe@S-1 in nitrate reduction using Fe atoms as active sites in the model. -The reaction path, such as Fig. 20 , 21 shown.

[0109] (1) Electrocatalytic reduction of NO3 - Reaction path and reaction Gibbs free energy change

[0110] The reduction of nitrate to ammonia is accompanied by the transfer of nine protons and eight electrons. Fig. 20 The reaction pathway is used for the electrocatalytic reduction of nitrate to ammonia on Fe sites. The first step is NO3 - adsorption, this is NO3 - No electron transfer is required when adsorbed onto the catalyst Fe@S-1, followed by the gradual reduction of *NO3, which generates *NO2, *ON, *ONH, *ONH2, *O, *OH in sequence and finally desorbs to obtain the catalyst *. The specific reaction formula is as follows:

[0111] *+NO3 - +9H + →*NO3+9H +

[0112] *NO3+9H + →*NO2+7H + +H2O

[0113] *NO2+7H + +H2O→*NO+5H + +2H2O

[0114] *ON+5H + +2H2O → *ONH + 4H + +2H2O

[0115] *ONH+4H + +2H2O→*ONH2+3H + +2H2O

[0116] *ONH2+3H + +2H2O→*O+2H + +NH3+2H2O

[0117] *O+2H + +NH3+2H2O→*OH+H + +NH3+2H2O

[0118] *OH+H + +NH3+2H2O→*+3H2O+NH3

[0119] Fig.21The following is the Gibbs free energy change diagram of Fe@S-1 and Fe / S-1 with nitrate reduction. The reaction path is further calculated to calculate the free energy of each intermediate on the Fe site. The lower energy indicates that NO3 - It is easier to adsorb on the Fe@S-1 site to form *NO3. Then the NO bond of *NO3 breaks and gradually reacts with H + Combined to form *NO2, *ON, *ONH, *ONH2, *O and *OH. The high energy of the lowest unoccupied molecular π* orbital of nitrate limits charge injection, so the rate-limiting step in the electrocatalytic removal of nitrate is the nitrite formation process, which limits the overall electrocatalytic removal of nitrate efficiency. However, the rate of formation of *ON on Fe@S-1 is the rate-limiting step, and the energy barrier for the reduction of *ON to *ONH of Fe@S-1 is much smaller than that of Fe / S-1, so the removal efficiency of Fe@S-1 is higher. Based on DFT calculations, it can be seen that Fe@S-1 has a high adsorption capacity for nitrate ions, and for NO3 - The reduction reaction has no large energy barrier and thus has significant electrocatalytic activity.

[0120] Fig. 22 a and Fig. 22 b shows NO3 - The difference in charge between Fe / S-1 and Fe@S-1. Green represents a decrease in electron cloud density, and yellow represents an increase in electron cloud density. The electron-accepting ability of Fe@S-1 is higher than that of Fe / S-1, and the Fe-O bond length of Fe@S-1 is shorter than that of Fe / S-1. The shorter the bond length, the stronger the bond, and the more stable the molecule formed. In addition, the adsorption energies of Fe@S-1 and Fe / S-1 are calculated. The adsorption energies of Fe@S-1 on NO3 - The adsorption capacity of Fe@S-1 is also stronger than that of Fe / S-1. Therefore, Fe@S-1 is more likely to absorb NO3 - Adsorption occurs and electrocatalytic reduction reaction occurs.

[0121] The partial wave state density of the Fe atomic d orbital of Fe / S-1 and Fe@S-1 was calculated respectively. The energy band was projected along the ordinate axis to obtain the state density. The flatter the energy band, the sharper the state density peak; the wider the energy band, the flatter the state density and the stronger the delocalization. Fig.23 a and Fig.23b, it can be seen that the larger the span of Fe@S-1 state density is, the flatter it is, that is, the wider the energy band is, the stronger and more stable the bonding ability is, which is consistent with the differential charge result. According to the d orbital partial wave state density, the d band centers of Fe / S-1 and Fe@S-1 are calculated to be -1.227 and -1.012 eV respectively. The relationship between the position of the d band center and the position of the Fermi level can predict the reaction activity of the catalyst. The closer to the Fermi level, the better the catalytic effect of the material, so the catalytic activity of Fe@S-1 is stronger than that of Fe / S-1, which is also consistent with the actual experiment above.

[0122] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a novel Fe@S-1 catalytic material, characterized in that: The preparation of the Fe@S-1 catalyst is carried out by a hydrothermal method, which specifically includes the following steps: Step 1, 4.06 g of tetrapropylammonium hydroxide was mixed with 32 mL of ultrapure water; after continuous stirring on a magnetic stirrer for 10 min, 2.6 g of ethyl orthosilicate was added and stirred for 6 h to obtain a clear mixture 1; Step 2, 0.909 g of ferric nitrate nonahydrate, 0.4 mL of ethylenediamine and 4 mL of ultrapure water were mixed and stirred for 10 minutes to obtain a mixture 2; Step 3, adding mixture 2 dropwise to mixture 1, stirring for 30 min without precipitation, and then placing in an autoclave for hydrothermal synthesis at 170° C. for 4 days; Step 4: The obtained product was centrifuged and collected, washed with ethanol three times, washed with ultrapure water three times, dried at 80°C for 12 hours, and the collected product was calcined at 550°C in a hydrogen-argon mixed gas atmosphere for 8 hours for full reduction. The obtained powder was ground and named Fe@S-1.

2. The method for preparing the novel Fe@S-1 catalytic material according to claim 1, characterized in that: In step 4, the volume ratio of hydrogen to argon in the hydrogen-argon mixture is V H2 :V Ar =5:

95.

3. Application of a novel Fe@S-1 catalytic material, the Fe@S-1 catalytic material prepared by the preparation method of the novel Fe@S-1 catalytic material according to claim 2, characterized in that: Applying the Fe@S-1 catalytic material to the electrocatalytic treatment of nitrates; Among them, the electrode sheet prepared by Fe@S-1 was used as the cathode and the platinum sheet was used as the anode.

4. The use of the novel Fe@S-1 catalytic material according to claim 3, characterized in that: The preparation method of the electrode sheet based on Fe@S-1 includes the following steps: Firstly, Fe@S-1 composite material, conductive carbon black and polyvinylidene fluoride in a mass ratio of 8:1:1 were weighed, and then the mixture was dissolved in N,N-dimethylformamide, and the concentration of the mixture was controlled to be 10 g / L to prepare catalyst ink. The ink was then coated on a 1.0 cm × 2.0 cm carbon cloth to ensure that both sides were evenly coated, and then dried at 60°C for 30 minutes to obtain a working electrode sheet.

Citation Information

Patent Citations

  • Pure silicon S-1 molecular sieve catalyst for packaging metal nanoparticles and preparing method and application of catalyst

    CN109647493A

  • Preparation method of sheet FeS-1 / Fe@S-1 with different thicknesses

    CN111111743A

  • Core-shell nitrogen-doped iron metal nanoparticles as well as preparation method and electrocatalytic application thereof

    CN111992233A

  • Method for improving performance of propylene prepared by propane dehydrogenation through hydro-thermal treatment of transition metal catalyst and introduction of CO < 2 >

    CN117548136A

  • Method for preparing NANO metal / metal oxide loaded molecular sieve catalyst

    US20160074849A1

Cited By

  • Confined-range bimetallic catalyst for electrocatalytic reduction reaction as well as preparation method and application of confined-range bimetallic catalyst

    CN119926476A

  • Confined bimetallic catalysts for electrocatalytic reduction reactions, their preparation methods and applications

    CN119926476B

  • Preparation method and application of topological insulator composite catalytic material

    CN120878860A