Cracking reaction catalyst as well as preparation method and application thereof

By preparing 13X-type molecular sieves and introducing platinum metal, combined with two calcination treatments, the pore structure and active sites were optimized, solving the problem of insufficient activity and stability of molecular sieve catalysts, achieving efficient cracking reaction at lower temperatures, and improving the performance of the catalyst.

CN118925786APending Publication Date: 2024-11-12CHINA ENERGY GRP NINGXIA COAL IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410976189.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing molecular sieve-based cracking catalysts cannot simultaneously achieve high reactivity and stability, nor can they achieve efficient cracking reactions at lower temperatures.

Method used

By preparing 13X-type molecular sieves and introducing platinum metal, combined with two calcination treatments, the pore structure and active sites are optimized to form uniformly dispersed platinum oxide or platinum metal, thereby improving the reaction activity and stability of the catalyst.

Benefits of technology

This enables efficient cracking reactions at lower temperatures, improving the economic efficiency of oil refining and enhancing the stability and activity of the catalyst.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004954579180000091
    Figure BDA0004954579180000091
  • Figure BDA0004954579180000101
    Figure BDA0004954579180000101
  • Figure BDA0004954579180000102
    Figure BDA0004954579180000102
Patent Text Reader

Abstract

The invention provides a cracking reaction catalyst as well as a preparation method and application thereof. The preparation method comprises the following steps: S1, preparing a 13X type molecular sieve; S2, mixing a platinum-containing compound with water to obtain a platinum precursor solution; s3, adding a 13X type molecular sieve into the platinum precursor solution, stirring, filtering and drying to obtain a catalyst precursor; and S4 to S5, calcining the catalyst precursor twice to obtain the cracking reaction catalyst. The method comprises the following steps: designing and controlling the whole process flow to obtain a 13X type molecular sieve with good performance; the method comprises the following steps: preparing a 13X-type molecular sieve, introducing platinum metal into the obtained 13X-type molecular sieve under specific experimental conditions to increase active sites on the 13X-type molecular sieve, and calcining twice to enable the obtained cracking catalyst to have good reaction activity and stability, so that efficient cracking reaction can be realized at a lower temperature, and the economic benefit of oil refining is finally improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of reaction catalysts, and in particular to a cracking reaction catalyst, a preparation method and application thereof. Background Art

[0002] In the oil refining and petrochemical industries, cracking is a key process used to convert heavier hydrocarbon feedstocks into more economically valuable light compounds such as petroleum fuels, olefins and aromatics. The core of the cracking reaction is the use of efficient catalysts to promote the reaction. Traditional cracking catalysts usually include acidic materials, such as zeolite molecular sieves, which can improve the selectivity and conversion rate of the reaction.

[0003] However, over time, the catalyst will become deactivated due to carbon and metal deposition, and thus needs to be replaced, resulting in production interruptions and the generation of catalyst waste, which seriously affects the efficiency of the cracking reaction. In addition, due to the limited fossil fuel resources and increasing environmental pressure, finding and developing more efficient, economical and environmentally friendly cracking catalysts has become an important issue in this field.

[0004] Based on this, how to modify the existing molecular sieve cracking reaction catalysts so that they have both high reaction activity and stability and can achieve efficient cracking reaction at a lower temperature is one of the important issues facing this field. Summary of the invention

[0005] The main purpose of the present invention is to provide a cracking reaction catalyst, a preparation method and application thereof, so as to solve the problem that the existing molecular sieve cracking reaction catalyst cannot take into account both high reaction activity and stability, and cannot achieve efficient cracking reaction at a lower temperature.

[0006] In order to achieve the above-mentioned purpose, the present invention provides a method for preparing a cracking reaction catalyst on one hand, which comprises: step S1, preparing a 13X molecular sieve: step S1-1, mixing a silicon source and an aluminum source to obtain a mixture gel; step S1-2, subjecting the mixture gel to a pH adjustment treatment, a first crystallization treatment, an aging treatment and a second crystallization treatment in sequence to obtain a 13X molecular sieve; step S2, mixing a platinum-containing compound with water to obtain a platinum precursor solution; step S3, adding the 13X molecular sieve to the platinum precursor solution, stirring, filtering and drying to obtain a catalyst precursor; step S4, subjecting the catalyst precursor to a first calcination at 450-550°C to obtain a first calcined catalyst; step S5, subjecting the first calcined catalyst to a second calcination at 700-900°C to obtain a cracking reaction catalyst.

[0007] Furthermore, in step S2, the platinum-containing compound is selected from one or more of hexachloroplatinic acid dihydrate, potassium chloroplatinate and platinum acetylacetonate, and the mass concentration of the platinum precursor solution is 1.8 to 2.2 g / L; in step S3, the amount of 13X molecular sieve added to the platinum precursor solution is 0.18 to 0.22 g / mL; preferably, the stirring time is 12 to 36 hours, the drying temperature is 90 to 130°C, and the time is 8 to 16 hours.

[0008] Furthermore, the first calcination time is 1 to 3 hours; the second calcination time is 3 to 5 hours; preferably, the first calcination is carried out in a nitrogen atmosphere, and the second calcination is carried out in an air atmosphere.

[0009] Further, in step S1-1, the silicon source is selected from one or more of silica sol, tetraethyl orthosilicate, macroporous silica gel, silicon powder and white carbon black; the aluminum source is selected from one or more of sodium aluminate, pseudo-boehmite, aluminum sulfate and aluminum nitrate; the weight ratio of the silicon source to the aluminum source is (0.01-1.25):1. Preferably, the mixing process is: mixing the silicon source and water to obtain a silicon-containing material, mixing the aluminum source and water to obtain an aluminum-containing material, and dropping the aluminum-containing material into the silicon-containing material to react to obtain a mixture gel; preferably, the reaction is carried out at 20-100°C for 0.1-24h; preferably, the dropping speed is 1-3mL / min; more preferably, the dropping and the reaction are both carried out under stirring.

[0010] Furthermore, in step S1-2, the pH adjustment process is as follows: adding sodium hydroxide solution to the mixture gel until the pH of the mixture gel is 8.5 to 12.5.

[0011] Furthermore, in step S1-2, the first crystallization treatment includes one-stage crystallization and two-stage crystallization; the temperature of the first-stage crystallization is 20-60°C, and the time is 4-24 hours; the temperature of the second-stage crystallization is 80-120°C, and the time is 6-48 hours; preferably, the temperature difference between the second-stage crystallization and the first-stage crystallization is ≥40°C.

[0012] Furthermore, in step S1-2, the aging reaction is to add the crystallized product into polyvinyl pyrrolidone and / or polyvinyl alcohol for aging; preferably, the aging reaction temperature is 20 to 100°C, and the time is 0.1 to 24 hours.

[0013] Furthermore, in step S1-2, the temperature of the second crystallization treatment is 60-105°C, and the time is 0.1-36h.

[0014] Another aspect of the present invention provides a cracking reaction catalyst, which is prepared by the above preparation method.

[0015] Another aspect of the present invention provides an application of the above-mentioned cracking reaction catalyst in cracking reactions related to the fields of petrochemical industry, coal chemical industry and waste plastic treatment.

[0016] By applying the technical solution of the present invention, the overall process flow is first designed and controlled to obtain a 13X molecular sieve with good performance, which has uniformly arranged pores, high specific surface area and pore capacity; then, platinum metal is introduced into the obtained 13X molecular sieve through specific experimental conditions to increase the active sites thereon, and after two calcinations, the obtained cracking catalyst has good reaction activity and stability, can achieve efficient cracking reaction at a lower temperature, and ultimately improve the economic benefits of oil refining. DETAILED DESCRIPTION

[0017] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below in conjunction with the embodiments.

[0018] As described in the background technology, the existing technology has the problem that molecular sieve cracking reaction catalysts cannot take into account both high reaction activity and stability, and cannot achieve efficient cracking reaction at a lower temperature. In order to solve the above technical problems, the present application provides a method for preparing a cracking reaction catalyst on the one hand, the preparation method comprising: step S1, preparing a 13X type molecular sieve: step S1-1, mixing a silicon source and an aluminum source to obtain a mixture gel; step S1-2, subjecting the mixture gel to pH adjustment treatment, a first crystallization treatment, an aging treatment and a second crystallization treatment in sequence to obtain a 13X type molecular sieve; step S2, mixing a platinum-containing compound with water to obtain a platinum precursor solution; step S3, adding a 13X type molecular sieve to the platinum precursor solution, stirring, filtering and drying to obtain a catalyst precursor; step S4, subjecting the catalyst precursor to a first calcination at 450-550°C to obtain a first calcined catalyst; step S5, subjecting the first calcined catalyst to a second calcination at 700-900°C to obtain a cracking reaction catalyst.

[0019] The present invention first designs and controls the overall process flow to obtain a 13X molecular sieve with good performance, which has uniformly arranged pores, high specific surface area and pore capacity. Specifically, the silicon source and the aluminum source are mixed, and pH adjustment treatment, first crystallization treatment, aging treatment and second crystallization treatment are carried out in sequence. Through the coordination of the above treatment processes, the pore structure of the obtained 3X molecular sieve is optimized, and its specific surface area and pore capacity are increased. Then, platinum metal is introduced into the obtained 13X molecular sieve through specific experimental conditions, the active sites thereon are increased, and after two calcinations, the platinum ions in the platinum precursor can be converted into dispersed metal platinum oxide or platinum metal, and the obtained cracking catalyst has good reactivity and stability, and can achieve efficient cracking reaction at a lower temperature; wherein the temperature of the first calcination is 450-550°C, and the temperature of the second calcination is 700-900°C, and the temperatures of the two calcinations cooperate with each other, which is more conducive to the uniform dispersion of Pt in the 13X molecular sieve, and the formation of effective active sites, and the optimization of the crystal form and pore structure, thereby showing higher catalytic activity in the cracking reaction. And, compared with other metals such as palladium (Pd), rhodium (Rh), etc., for the technical solution provided in this application, Pt is converted into metal platinum oxide or platinum metal after the above process due to its excellent catalytic activity and stability, and is compounded with the molecular sieve framework, thereby improving the catalytic activity.

[0020] In several typical embodiments, the platinum-containing compound in step S2 is selected from one or more of hexachloroplatinic acid dihydrate, potassium chloroplatinate and platinum acetylacetonate, and the mass concentration of the platinum precursor solution is 1.8 to 2.2 g / L; in principle, the type of platinum-containing compound can be selected from the types commonly used in the art, and the mass concentration of the prepared platinum precursor solution can also be conventionally adjusted, but the inventors have conducted a large number of experiments on the experimental system involved in the technical scheme of the present invention, and finally preferred the platinum-containing compounds to be the above types, and the mass concentration of the platinum precursor solution was 1.8 to 2.2 g / L. It was also found that under the above conditions, the 13X molecular sieve in the platinum precursor solution can be better dispersed, and its adsorbed Pt active sites are more, thereby showing higher reaction activity. Furthermore, in the platinum precursor solution, the addition amount of 13X molecular sieve is 0.18-0.22 g / mL. When activated and modified at this ratio, the 13X molecular sieve can be dispersed more evenly in the platinum precursor solution, which is more conducive to the attachment of Pt ions; and more preferably, the stirring time is 12-36 hours, and the drying temperature is 90-130°C, and the time is 8-16 hours. Based on the above content, the inventors have further optimized through a large number of experiments and found that when stirring and drying are carried out under the above conditions, more Pt ions can be attached to the pores of the 13X molecular sieve, and while removing moisture more effectively, more Pt sites in the pores retain high catalytic activity, so that the resulting cracking catalyst exhibits higher catalytic activity.

[0021] In order to make Pt less likely to be removed from the 13X molecular sieve framework and further optimize the crystal form of the 13X molecular sieve, in several preferred embodiments, the inventors have optimized the time of the first calcination to 1 to 3 hours after a large number of experiments; the time of the second calcination is preferably 3 to 5 hours, and found that the catalytic activity of the cracking catalyst obtained under this condition is higher and is suitable for a lower cracking reaction temperature. In a more preferred embodiment, the first calcination is carried out in a nitrogen atmosphere and the second calcination is carried out in an air atmosphere, so that the Pt ions in the platinum salt can be converted into highly dispersed metal platinum oxide or platinum metal, thereby improving the catalytic activity.

[0022] In the process of preparing 13X molecular sieve, in order to obtain a molecular sieve with a stable structure and a high silicon-aluminum ratio, in a preferred embodiment, one or more of silica sol, tetraethyl orthosilicate, coarse-pore silica gel, silicon powder and white carbon black can be selected as the silicon source; one or more of sodium aluminate, pseudo-boehmite, aluminum sulfate and aluminum nitrate can be selected as the aluminum source; and the weight ratio of the silicon source to the aluminum source is (0.01-1.25):1. Although conventional silicon sources and aluminum sources in the art can be used in principle, after a large number of experiments by the inventors, it was found that when the above-mentioned silicon sources and aluminum sources are mixed at a weight ratio of (0.01-1.25):1, the silicon-aluminum ratio of the molecular sieve finally obtained is higher and the pore structure is better, so a cracking catalyst with higher catalytic reaction activity can be better obtained in the subsequent preparation process. On the basis of the above-mentioned silicon source and aluminum source, further, the process of mixing the two includes: mixing the silicon source and water to obtain a silicon-containing material, and mixing the aluminum source and water to obtain an aluminum-containing material; wherein the mixing of the silicon source and the water is completed after stirring at 20 to 60° C. for 0.1 to 12 hours, and the stirring speed is maintained at 200 to 800 rpm, and the concentration of the obtained silicon-containing material is 2 to 99 wt%; the mixing of the aluminum source and the water is completed after stirring at 20 to 60° C. for 0.1 to 12 hours, and the stirring speed is maintained at 200 to 800 rpm, and the concentration of the obtained silicon-containing material is 40 to 60 wt%. The aluminum-containing material is added dropwise to the silicon-containing material to react to obtain a mixed gel. The aluminum-containing material prepared under the above conditions has better compatibility with the silicon-containing material, which is more convenient for the reaction of the two, and is more conducive to the formation of a 13X molecular sieve with a high aluminum-silicon ratio; in order to make the reaction more fully carried out, the reaction is preferably carried out at 20 to 100 ° C for 0.1 to 24 hours; and, in order to make the contact between the silicon source and the aluminum source more sufficient during the reaction, the inventor has preferably added a dripping speed of 1 to 3 mL / min after a large number of experiments. Slow dripping is conducive to more sufficient contact between the silicon source and the aluminum source during the reaction, thereby improving the synthesis yield and quality of the molecular sieve. In a more preferred embodiment, the dripping and reaction are both carried out under stirring conditions, so that the mixing and reaction of the silicon source and the aluminum source are more sufficient, and the synthesis yield of the 13X molecular sieve is improved.

[0023] In order to optimize the pores of the 13X molecular sieve in advance during the preparation process, in a typical embodiment, the pH adjustment treatment in step S1-2 is: adding sodium hydroxide solution to the mixture gel until the pH of the mixture gel is 8.5-12.5, that is, the alkalinity of the mixture gel formed by the aluminum source and the silicon source is optimized to a pH value of 8.5-12.5, and the pores of the 13X molecular sieve are optimized in advance by adjusting the alkalinity in its reaction system, thereby more effectively improving the structural performance of the obtained cracking catalyst.

[0024] In a typical embodiment, in step S1-2, the first crystallization treatment includes one-stage crystallization and two-stage crystallization; the temperature of the first stage crystallization is 20-60°C and the time is 4-24h; the temperature of the second stage crystallization is 80-120°C and the time is 6-48h; the first crystallization treatment is carried out in stages, which can further optimize the structure of the obtained crystallized product and improve its stability; the inventors have optimized the conditions of the above two-stage crystallization treatments through a large number of experiments, and found that crystallization under these conditions can better play the role of the two-stage crystallization, making the structure more complete and the crystal form more uniform. And, more preferably, the temperature difference between the second stage crystallization and the first stage crystallization is ≥40°C. After a large number of experiments, the inventors found that when the temperature difference between the second stage crystallization and the first stage crystallization is ≥40°C, the molar ratio of each component in the crystallized product can be further optimized, thereby effectively improving the catalytic activity. In a preferred embodiment, the molar ratio of each component in the crystallized product is: SiO2 / Al2O3=(0.01~6):1, Na2O / SiO2=(0.01~4.0):1, H2O / SiO2=(1.0~50.0):1. The crystallized product with this composition exhibits higher catalytic activity when it is obtained as a cracking reaction catalyst through a subsequent preparation process.

[0025] In the technical solution provided by the present invention, in addition to obtaining the crystallized product, it also includes aging it. In a preferred embodiment, the aging reaction in step S3 is to add the crystallized product to polyvinyl pyrrolidone and / or polyvinyl alcohol for aging, and the temperature of the aging reaction is 20 to 100 ° C, and the time is 0.1 to 24 hours. Since polyvinyl pyrrolidone and / or polyvinyl alcohol can be used as a structure directing agent and a crystal growth regulator, aging under the above conditions can further assist crystallization and optimize the crystal form, while significantly improving the structural stability of the obtained molecular sieve.

[0026] Furthermore, the temperature of the second crystallization treatment in step S1-2 is 60-105°C and the time is 0.1-36 hours. The inventors have found through a large number of experiments that crystallization under such conditions can obtain a 13X molecular sieve with a more uniform crystal structure, a more uniform size, and a better specific surface area and pore structure.

[0027] In several preferred embodiments, the pH of the mixture gel in step S1-2 is 12, the temperature of the first crystallization is 35-45°C, the time is 11-13h, the temperature of the second crystallization is 90-100°C, the time is 22-26h, and the molar ratio of each component in the obtained crystallized product is: SiO2 / Al2O3=1.5:1, Na2O / SiO2=1.6:1, H2O / SiO2=32:1. The inventor has optimized this condition through a large number of experiments and found that the cracking reaction catalyst obtained at this time has a higher pore capacity, higher activity, and better catalytic performance.

[0028] Another aspect of the present invention provides a cracking reaction catalyst, which is prepared by the above preparation method. The obtained cracking reaction catalyst has good reaction activity and stability.

[0029] Another aspect of the present invention provides an application of the above cracking reaction catalyst in cracking reactions related to petrochemicals, coal chemical industry and waste plastics treatment. The high activity, high stability and low temperature resistance of the above catalyst enable it to achieve efficient cracking reactions under various temperatures and experimental environments, especially the catalytic reaction of cracking naphtha to prepare olefins, thereby well meeting the application needs of various fields.

[0030] The present application is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in the present application.

[0031] Unless otherwise defined, all professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.

[0032] Example 1

[0033] A method for preparing a cracking reaction catalyst:

[0034] 1. Preparation of 13X molecular sieve:

[0035] 21.0g silica sol (mass fraction of 30%) was dissolved in 36.0g deionized water, and pretreated at 25°C in a closed reactor for 1 hour to obtain a silicon-containing material; 24g aluminum sulfate was dissolved in 18.0g deionized water, and stirred at 25°C for 1 hour to obtain an aluminum-containing material; the aluminum-containing material was slowly added dropwise to the silicon-containing material (the dropping speed was 1mL / min), and continued to stir at 60°C for 8 hours to obtain a mixture gel; 6.74g sodium hydroxide was dissolved in 36g deionized water dispersion and added to the mixture gel until the pH value was 12 to obtain a gel slurry solution, which was placed in a hydrothermal reactor for two-stage control. Warm crystallization, the first stage crystallization temperature is 40°C, the time is 12 hours, the second stage crystallization temperature is 95°C, the time is 24 hours, and a 13X crystallized product is obtained (the molar ratio of each component is: SiO2 / Al2O3=1.5:1, Na2O / SiO2=1.6:1, H2O / SiO2=32:1); the crystallized product is mixed with 1g of polyvinyl pyrrolidone, and then stirred and aged at 60°C for 12h, and then placed in a hydrothermal reactor at a crystallization temperature of 98°C for 24h for final crystallization, and the obtained product is filtered and washed to pH 7, and dried at 90°C to obtain a 13X molecular sieve.

[0036] 2. Preparation of cracking reaction catalyst:

[0037] Take 100g of the dried 13X molecular sieve prepared in Example 1 (drying conditions are 110°C, 4h), and dissolve 1g of H2PtCl6·2H2O in 500mL of deionized water to form a platinum precursor solution. Add the dried 13X molecular sieve to the prepared platinum precursor solution. Use a magnetic stirrer to stir thoroughly for 24 hours. Then filter, place the filtered molecular sieve in a drying oven, and further dry it at 110°C for 12 hours to obtain a catalyst precursor, which is placed in a molybdenum cloth furnace and first calcined for 2 hours in a nitrogen atmosphere at 500°C, and then calcined for 4 hours at 800°C in an air atmosphere to obtain a cracking reaction catalyst.

[0038] Example 2

[0039] A method for preparing a cracking reaction catalyst:

[0040] 1. Preparation of 13X molecular sieve:

[0041] 1g of silicon powder was dissolved in 18g of deionized water, and pretreated at 25°C in a closed reactor for 1 hour to obtain a silicon-containing material; at the same time, 12g of aluminum nitrate was dissolved in 18.0g of deionized water, and stirred at 35°C for 1 hour to prepare an aluminum-containing material. The prepared aluminum-containing material was slowly added dropwise to the silicon-containing material (the dropping speed was 2mL / min), and continued to stir at 50°C for 6 hours to obtain a mixture gel; 2g of sodium hydroxide was dissolved in 36g of deionized water to obtain a dispersion, and added to the mixture gel until the pH value was 11.8 to obtain a gel slurry solution, which was then transferred to a hydrothermal reactor to perform a two-stage temperature-controlled crystallization process: the first stage crystallization temperature was set at 50°C and lasted for 14 hours; the second stage crystallization temperature was controlled at 100°C and maintained for 14 hours. The mixture was kept for 18 hours to obtain a 13X crystallized product (wherein the molar ratio of each component is: SiO2 / Al2O3=0.6:1, Na2O / SiO2=3:1, H2O / SiO2=20:1); the crystallized product was mixed with 1 g of polyvinyl alcohol, and then stirred and aged at 60°C for 12 hours, and then placed in a hydrothermal reactor at a crystallization temperature of 95°C for 24 hours for final crystallization. The obtained product was filtered and washed to a pH of 7, and dried at 90°C to obtain a 13X molecular sieve.

[0042] 2. Preparation of cracking reaction catalyst: The 13X molecular sieve prepared in Example 1 was replaced with the 13X molecular sieve prepared in this example, and the other conditions were the same as in Example 1.

[0043] Example 3

[0044] A method for preparing a cracking reaction catalyst:

[0045] 1. Preparation of 13X molecular sieve:

[0046] 0.17g silicon powder was dissolved in 6g deionized water, and pretreated at 25°C for 1 hour in a sealed reactor to obtain a silicon-containing material; at the same time, 12g aluminum nitrate was dissolved in 18.0g deionized water, and stirred at 35°C for 1 hour to prepare an aluminum-containing material liquid. The aluminum-containing material was slowly added to the silicon-containing material (the drop rate was 1mL / min), and stirred at 100°C for 24 hours to obtain a mixture gel; 0.9g sodium hydroxide was dissolved in 6g deionized water to prepare a dispersion, and added to the mixture gel until the pH value was 12.5 to obtain a gel slurry solution, which was then transferred to a hydrothermal reactor for two-stage crystallization. First, crystallization was continued at 60°C for 24 hours, and then the temperature was increased to 120°C for crystallization reaction for 48 hours to obtain. To obtain a 13X crystallized product (wherein the molar ratio of each component is: SiO2 / Al2O3=0.1:1, Na2O / SiO2=4:1, H2O / SiO2=1:1); the crystallized product is mixed with 1g of polyvinyl alcohol, and then stirred and aged at 60°C for 12h, and then placed in a hydrothermal reactor at a crystallization temperature of 105°C and a time of 20h for final crystallization. The obtained product is filtered and washed to a pH of 7, and dried at 90°C to obtain a 13X molecular sieve.

[0047] 2. Preparation of cracking reaction catalyst: The 13X molecular sieve prepared in Example 1 was replaced with the 13X molecular sieve prepared in this example, and the other conditions were the same as in Example 1.

[0048] Example 4

[0049] A method for preparing a cracking reaction catalyst:

[0050] 1. Preparation of 13X molecular sieve:

[0051] Take 14.65g of ethyl orthosilicate and 36g of deionized water in a volume ratio of 1:1, and pretreat at 25°C in a closed reactor for 1 hour to obtain a silicon-containing material. At the same time, dissolve 12g of aluminum nitrate in 18.0g of deionized water and stir at 35°C for 1 hour to obtain an aluminum-containing material. After that, gradually add the aluminum-containing material dropwise to the silicon-containing material (the dropping speed is 3mL / min), and mix and stir at 20°C for 0.1 hour to prepare a mixture gel; dissolve 0.56g of sodium hydroxide in 6g of deionized water as a dispersion liquid, pour it into the mixture gel until the pH value is 8.5, obtain a gel slurry solution, and then transfer it to a hydrothermal reactor to perform a segmented crystallization reaction: first set the crystallization temperature to 20°C for 4 hours; then increase it to 80°C and maintain crystallization for 6 hours , and obtain a 13X crystallized product (wherein the molar ratio of each component is: SiO2 / Al2O3=2.5:1, Na2O / SiO2=0.1:1, H2O / SiO2=40:1); the crystallized product is mixed with 1g of polyvinyl alcohol, and then stirred and aged at 70°C for 15h, and then placed in a hydrothermal reactor at a crystallization temperature of 115°C and a time of 16h for final crystallization. The obtained product is filtered and washed to a pH of 7, and dried at 90°C to obtain a 13X molecular sieve.

[0052] 2. Preparation of cracking reaction catalyst: The 13X molecular sieve prepared in Example 1 was replaced with the 13X molecular sieve prepared in this example, and the other conditions were the same as in Example 1.

[0053] Example 5

[0054] A method for preparing a cracking reaction catalyst:

[0055] 1. The preparation process of 13X molecular sieve is different from that of Example 1 only in that during the process of adjusting the pH value of the mixture gel with sodium hydroxide solution, the pH value of the mixture gel is adjusted to 13.5 to obtain a gel slurry solution.

[0056] 2. Preparation of cracking reaction catalyst: The 13X molecular sieve prepared in Example 1 was replaced with the 13X molecular sieve prepared in this example, and the other conditions were the same as in Example 1.

[0057] Example 6

[0058] A method for preparing a cracking reaction catalyst:

[0059] 1. The preparation process of 13X molecular sieve is different from that of Example 1 only in that during the process of adjusting the pH value of the mixture gel by using sodium hydroxide solution, the pH value of the mixture gel is adjusted to 7.5 to obtain a gel slurry solution.

[0060] 2. Preparation of cracking reaction catalyst: The 13X molecular sieve prepared in Example 1 was replaced with the 13X molecular sieve prepared in this example, and the other conditions were the same as in Example 1.

[0061] Example 7

[0062] A method for preparing a cracking reaction catalyst:

[0063] 1. Preparation of 13X molecular sieve: same as in Example 1.

[0064] 2. The preparation process of the cracking reaction catalyst is different from that of Example 1 only in that the amount of H2PtCl6·2H2O is changed to 0.75 g, that is, the mass concentration of the platinum precursor solution is 1.5 g / L.

[0065] Example 8

[0066] A method for preparing a cracking reaction catalyst:

[0067] 1. Preparation of 13X molecular sieve: same as in Example 1.

[0068] 2. The preparation process of the cracking reaction catalyst is different from that of Example 1 only in that the amount of H2PtCl6·2H2O is changed to 1.25 g, that is, the mass concentration of the platinum precursor solution is 2.5 g / L.

[0069] Example 9

[0070] A method for preparing a cracking reaction catalyst:

[0071] 1. Preparation of 13X molecular sieve: same as in Example 1.

[0072] 2. The preparation process of the cracking reaction catalyst is different from that of Example 1 only in that the amount of 13X molecular sieve used is 75 g (ie, the amount of 13X molecular sieve added to the platinum precursor solution is 0.15 g / mL), and the stirring time is 40 h.

[0073] Example 10

[0074] A method for preparing a cracking reaction catalyst:

[0075] 1. Preparation of 13X molecular sieve: same as in Example 1.

[0076] 2. The preparation process of the cracking reaction catalyst differs from that of Example 1 only in that the amount of 13X molecular sieve used is 125 g (ie, the amount of 13X molecular sieve added to the platinum precursor solution is 0.25 g / mL), and the stirring time is 10 h.

[0077] Embodiment 11

[0078] A method for preparing a cracking reaction catalyst:

[0079] 1. Preparation of 13X molecular sieve: same as in Example 1.

[0080] 2. The preparation process of the cracking reaction catalyst is different from that of Example 1 only in that the first calcination and the second calcination are both carried out under air atmosphere.

[0081] Example 12

[0082] A method for preparing a cracking reaction catalyst:

[0083] 1. Preparation of 13X molecular sieve: same as in Example 1.

[0084] 2. The preparation process of the cracking reaction catalyst is different from that of Example 1 only in that the first calcination and the second calcination are both carried out under a nitrogen atmosphere.

[0085] Comparative Example 1

[0086] A method for preparing a cracking reaction catalyst:

[0087] The only difference between this comparative example and Example 1 is that: instead of preparing 13X molecular sieve, 100 g of 5A molecular sieve is directly used to replace 13X molecular sieve to prepare the cracking reaction catalyst.

[0088] Comparative Example 2

[0089] A method for preparing a cracking reaction catalyst:

[0090] 1. Preparation of 13X molecular sieve: same as in Example 1.

[0091] 2. The preparation process of the cracking reaction catalyst differs from that of Example 1 only in that instead of using H2PtCl6·2H2O solution, a zirconium nitrate (Zr(NO3)4) solution of the same volume and mass concentration is used.

[0092] Comparative Example 3

[0093] A method for preparing a cracking reaction catalyst:

[0094] 1. Preparation of 13X molecular sieve: same as in Example 1.

[0095] 2. The preparation process of the cracking reaction catalyst is different from that of Example 1 only in that the conditions of the two calcinations are different, wherein the first calcination is at 400° C. for 0.5 h and the second calcination is at 600° C. for 2 h.

[0096] Comparative Example 4

[0097] A method for preparing a cracking reaction catalyst:

[0098] 1. Preparation of 13X molecular sieve: same as in Example 1.

[0099] 2. The preparation process of the cracking reaction catalyst is different from that of Example 1 only in that the conditions of the two calcinations are different, wherein the first calcination is at 600° C. for 3.5 h and the second calcination is at 1000° C. for 6 h.

[0100] The various properties of the 13X molecular sieve and the cracking reaction catalyst obtained in the above embodiments and comparative examples were tested respectively, and the results are shown in Table 1.

[0101] Table 1

[0102]

[0103]

[0104] The cracking reaction catalysts obtained in the above-mentioned embodiments and comparative examples are used in the reaction of preparing trienes (trienes are ethylene, propylene, butadiene) by steam cracking of naphtha, and the specific reaction conditions are:

[0105] The reaction temperature was 550°C, the reaction pressure was 80 KPa, the reaction time was set to 2 hours, and the water-oil mass ratio was 0.6.

[0106] The total yield and total selectivity of the obtained trienes are shown in Table 2.

[0107] Table 2

[0108]

[0109]

[0110] From the above description, it can be seen that the above embodiments of the present invention achieve the synthesis of 13X molecular sieve with good performance and cracking catalyst with good reaction activity and stability.

[0111] It should be noted that the terms "first", "second", etc. in the specification and claims of the present application are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the terms used in this way can be interchangeable where appropriate, so that the embodiments of the present application described herein can be implemented in an order other than those described herein, for example.

[0112] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a cracking reaction catalyst, characterized in that: The preparation method of the cracking reaction catalyst comprises: Step S1, preparing 13X molecular sieve: Step S1-1, mixing a silicon source and an aluminum source to obtain a mixture gel; Step S1-2, subjecting the mixture gel to a pH adjustment treatment, a first crystallization treatment, an aging treatment and a second crystallization treatment in sequence to obtain the 13X molecular sieve; Step S2, mixing a platinum-containing compound with water to obtain a platinum precursor solution; Step S3, adding the 13X molecular sieve to the platinum precursor solution, stirring, filtering and drying to obtain a catalyst precursor; Step S4, calcining the catalyst precursor at 450-550° C. to obtain a first calcined catalyst; Step S5, performing a second calcination on the first calcined catalyst at 700-900° C. to obtain the cracking reaction catalyst.

2. The method for preparing a cracking reaction catalyst according to claim 1, characterized in that: In step S2, the platinum-containing compound is selected from one or more of hexachloroplatinic acid dihydrate, potassium chloroplatinate and platinum acetylacetonate, and the mass concentration of the platinum precursor solution is 1.8 to 2.2 g / L; In step S3, the amount of the 13X molecular sieve added to the platinum precursor solution is 0.18-0.22 g / mL; Preferably, the stirring time is 12 to 36 hours, and the drying temperature is 90 to 130° C. for 8 to 16 hours.

3. The method for preparing a cracking reaction catalyst according to claim 1 or 2, characterized in that: The first calcination time is 1 to 3 hours; the second calcination time is 3 to 5 hours; Preferably, the first calcination is performed under a nitrogen atmosphere, and the second calcination is performed under an air atmosphere.

4. The method for preparing a cracking reaction catalyst according to claim 1 or 2, characterized in that: In step S1-1, The silicon source is selected from one or more of silica sol, tetraethyl orthosilicate, macroporous silica gel, silicon powder and white carbon black; the aluminum source is selected from one or more of sodium aluminate, pseudo-boehmite, aluminum sulfate and aluminum nitrate; the weight ratio of the silicon source to the aluminum source is (0.01-1.25):1; Preferably, the mixing process is: mixing the silicon source and water to obtain a silicon-containing material, mixing the aluminum source and water to obtain an aluminum-containing material, and dropping the aluminum-containing material into the silicon-containing material to react to obtain the mixture gel; Preferably, the reaction is carried out at 20 to 100° C. for 0.1 to 24 h; Preferably, the dripping speed is 1 to 3 mL / min; More preferably, the dropping and the reacting are both performed under stirring.

5. The method for preparing a cracking reaction catalyst according to any one of claims 1 to 4, characterized in that: In step S1-2, the pH adjustment process is: adding sodium hydroxide solution to the mixture gel until the pH of the mixture gel is 8.5-12.

5.

6. The method for preparing a cracking reaction catalyst according to any one of claims 1 to 5, characterized in that: In step S1-2, the first crystallization process includes a first stage crystallization and a second stage crystallization; The temperature of the first stage of crystallization is 20 to 60° C. and the time is 4 to 24 hours; The temperature of the second stage crystallization is 80-120°C and the time is 6-48h; Preferably, the temperature difference between the second-stage crystallization and the first-stage crystallization is ≥40°C.

7. The method for preparing a cracking reaction catalyst according to any one of claims 1 to 6, characterized in that: In step S1-2, the aging reaction is to add the crystallized product into polyvinyl pyrrolidone and / or polyvinyl alcohol for aging; Preferably, the aging reaction temperature is 20-100° C. and the time is 0.1-24 h.

8. The method for preparing a cracking reaction catalyst according to any one of claims 1 to 7, characterized in that: In step S1-2, the temperature of the second crystallization treatment is 60-105°C, and the time is 0.1-36 hours.

9. A cracking reaction catalyst, characterized in that: The cracking reaction catalyst is prepared by the preparation method according to any one of claims 1 to 8.

10. Use of the cracking reaction catalyst according to claim 9 in cracking reactions related to petrochemical industry, coal chemical industry and waste plastic treatment.