Molecular sieve catalyst and preparation method and application thereof

CN118925787APending Publication Date: 2024-11-12SUZHOU UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410989061.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-12

Smart Images

  • Figure CN118925787A_ABST
    Figure CN118925787A_ABST
Patent Text Reader

Abstract

The invention discloses a molecular sieve catalyst and a preparation method and application thereof.The preparation method comprises the steps that a molecular sieve serves as a carrier, different metal salts are selected as metal sources, and the molecular sieve loaded transition metal hydroxide catalyst is obtained through a sodium hydroxide sedimentation method; and then carrying out phosphating treatment to obtain the molecular sieve loaded small-size transition metal phosphide catalyst. On the basis, synthesis of transition metal and phosphide nanoparticles with the size smaller than 3 nanometers is achieved, the crystalline phase of transition metal phosphide is changed through high-temperature hydrogen reduction, and in a non-alkaline system and inert gas atmosphere, ultraviolet-visible light is introduced, so that the induction period of a transition metal phosphide catalyst is successfully eliminated. The amino molecular sieve loaded transition metal and phosphide catalyst provided by the invention has excellent catalytic activity in hydrogen production by hydrolysis of ammonia borane, and the conversion frequency at room temperature is up to 240.0 min <-1 >.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of molecular sieve catalysts, and in particular to a molecular sieve catalyst and a preparation method and application thereof. Background Art

[0002] Hydrogen energy is a high-energy-density, renewable and environmentally friendly energy carrier, and is widely considered to be one of the favorable candidates to replace fossil energy. However, the bottleneck of hydrogen energy development is how to store and transport it safely, efficiently and at low cost. At present, common physical hydrogen storage methods have problems such as high hydrogen storage cost, poor safety, inconvenient logistics and transportation, low physical adsorption capacity and serious self-volatilization problems. Chemical hydrogen storage materials have attracted widespread attention from academia and industry due to their safety, high efficiency and mild hydrogen release conditions.

[0003] Among the many hydrogen storage materials, chemical hydrogen storage materials with high mass and volumetric hydrogen storage densities, such as ammonia borane, hydrazine hydrate, formic acid and sodium borohydride, are considered to be the most promising hydrogen storage materials. Ammonia borane (NH3BH3, AB) has been studied in depth due to its extremely high hydrogen content (19.6wt%) and its non-toxic, stable and environmentally friendly properties, and is considered to be a highly promising vehicle-mounted hydrogen storage medium. In the presence of a suitable catalyst, H2 can be produced from the hydrolysis reaction of ammonia borane (NH3BH3+2H2O=NH4 + +BO2 - +3H2) is released controllably.

[0004] In the ammonia borane hydrolysis hydrogen production reaction, the development of high-performance transition metal phosphide catalysts faces three key problems. First, the transition metal phosphide nanoparticles are large in size, resulting in fewer active sites exposed per unit volume; second, the catalytic activity is much lower than that of precious metal catalysts; third, when the transition metal phosphide catalyst is used in the ammonia borane hydrolysis hydrogen production reaction, there is a long induction period, which is not conducive to the production of hydrogen. In recent years, researchers have developed transition metal phosphide catalysts supported by materials such as activated carbon, titanium dioxide and silicon dioxide, anchoring transition metal phosphide species on the surface of the carrier. Usually, in the ammonia borane hydrolysis hydrogen production catalytic system, additional alkali (such as sodium hydroxide, potassium hydroxide and cesium hydroxide, etc.) needs to be added to eliminate the induction period of the transition metal phosphide catalyst, but it will reduce the overall hydrogen content of the system. In addition, compared with the transition metal phosphide crystals synthesized by solvothermal synthesis, although smaller phosphide nanoparticles can be obtained, their size is still generally greater than 5 nanometers, and the turnover frequency (TOF) value in the ammonia borane hydrolysis hydrogen production at room temperature is generally less than 100min. -1 , current technology cannot achieve the controllable synthesis of small-sized, highly active transition metal phosphide catalysts using simple methods. Summary of the invention

[0005] In order to solve the above technical problems, the purpose of the present invention is to provide a molecular sieve catalyst and a preparation method and application thereof, wherein the molecular sieve catalyst includes a molecular sieve-loaded transition metal phosphide catalyst, a molecular sieve-loaded transition metal and its phosphide catalyst, an amino molecular sieve-loaded transition metal phosphide catalyst and an amino molecular sieve-loaded transition metal and its phosphide catalyst. The amino molecular sieve-loaded transition metal and its phosphide catalyst provided by the present invention realizes the synthesis of transition metal and its phosphide nanoparticles with a size less than 3 nanometers, changes the crystal phase of the transition metal phosphide by high-temperature hydrogen reduction, and successfully eliminates the induction period of the transition metal phosphide catalyst by introducing ultraviolet-visible light in a non-alkaline system and an inert gas atmosphere.

[0006] The above object of the present invention is achieved through the following technical solutions:

[0007] The first aspect of the present invention provides a method for preparing a molecular sieve-supported transition metal phosphide catalyst, comprising the following steps:

[0008] (1) Dissolving the molecular sieve and the transition metal salt in an alkaline solution to react to obtain a molecular sieve-supported transition metal hydroxide catalyst (M(OH) x / Zeolite, M represents a transition metal, Zeolite represents a molecular sieve, and x is 1 to 6); the molecular sieve is a Y-type molecular sieve, a Beta molecular sieve or a ZSM-5 molecular sieve;

[0009] (2) subjecting the molecular sieve-supported transition metal hydroxide catalyst obtained in step (1) to phosphating treatment at 250-400° C. in a phosphine gas atmosphere to obtain the molecular sieve-supported transition metal phosphide catalyst (M y P / Zeolite, y is 1~2).

[0010] The invention uses molecular sieve as a carrier, selects different metal salts as metal sources, adopts a sodium hydroxide precipitation method to obtain a molecular sieve-loaded transition metal hydroxide catalyst, and then performs a phosphating treatment to obtain the molecular sieve-loaded small-size transition metal phosphide catalyst.

[0011] On this basis, the second aspect of the present invention provides a method for preparing a molecular sieve-supported transition metal and its phosphide catalyst, comprising the following steps:

[0012] (1) Dissolving the molecular sieve and the transition metal salt in an alkaline solution to react to obtain a molecular sieve-supported transition metal hydroxide catalyst (M(OH) x / Zeolite, M represents a transition metal, Zeolite represents a molecular sieve, and x is 1 to 6); the molecular sieve is a Y-type molecular sieve, a Beta molecular sieve or a ZSM-5 molecular sieve;

[0013] (2) subjecting the molecular sieve-supported transition metal hydroxide catalyst obtained in step (1) to phosphating treatment at 250-400° C. in a phosphine gas atmosphere to obtain the molecular sieve-supported transition metal phosphide catalyst (M y P / Zeolite, y is 1 to 2);

[0014] (3) reducing the molecular sieve-supported transition metal phosphide catalyst obtained in step (2) at 200-600° C. in a hydrogen atmosphere to obtain a molecular sieve-supported transition metal and its phosphide catalyst (M z P / Zeolite, z is 1 to 3, z is greater than y).

[0015] Furthermore, in step (1), the transition metal salt is a nitrate or chloride of a transition metal, and the transition metal is selected from one or more of cobalt, nickel, copper, iron, manganese, chromium, molybdenum, tungsten, platinum, palladium, ruthenium, rhodium, osmium, gold, iridium and silver.

[0016] Furthermore, in step (1), the alkaline solution is an aqueous solution of sodium hydroxide or an aqueous solution of sodium borohydride.

[0017] Furthermore, the concentration of sodium hydroxide in the sodium hydroxide aqueous solution is 0.5 to 5 mol / L.

[0018] Furthermore, the concentration of sodium borohydride in the sodium borohydride aqueous solution is 0.5 to 5 mol / L.

[0019] Furthermore, in step (1), the reaction temperature is 25 to 60° C. and the reaction time is 2 to 4 hours.

[0020] Furthermore, in step (1), the mass ratio of the molecular sieve to the transition metal salt is 1:(0.01-2), preferably 1:(0.05-1.5), and more preferably 1:(0.03-0.3).

[0021] Furthermore, in step (1), the concentration of the transition metal salt in the mixed solution obtained by dissolving the molecular sieve and the transition metal salt in an alkaline solution is 0.001 to 0.2 mol / L.

[0022] Furthermore, in step (2), the phosphating treatment is carried out in a tubular furnace, and under an inert atmosphere, the molecular sieve-loaded transition metal hydroxide catalyst is placed downstream of the tubular furnace, and sodium hypophosphite is placed upstream of the tubular furnace, and sodium hypophosphite (NaH2PO2) is thermally decomposed to produce phosphine (PH3) gas.

[0023] Furthermore, in step (2), the phosphating treatment time is 1 to 4 hours.

[0024] Furthermore, in step (2), the mass ratio of the molecular sieve-supported transition metal hydroxide catalyst to sodium hypophosphite is 1:(0.1-20), preferably 1:(0.5-15).

[0025] Furthermore, in step (3), the reduction treatment time is 2 to 4 hours.

[0026] The third aspect of the present invention provides a method for preparing an amino molecular sieve loaded with a transition metal phosphide catalyst, wherein step (1) of the method described in the first aspect further comprises a step of functionalizing the surface of the molecular sieve with amino groups using an amino-containing silane coupling agent.

[0027] Furthermore, the amino-containing silane coupling agent is selected from one or more of 3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropyltriethoxysilane and diethylenetriaminopropyltrimethoxysilane.

[0028] The fourth aspect of the present invention provides a method for preparing an amino molecular sieve loaded with a transition metal and a phosphide thereof catalyst, comprising the following steps:

[0029] (1) using an amino-containing silane coupling agent to functionalize the surface of the molecular sieve with amino groups to obtain an amino molecular sieve (NH2-Zeolite), dissolving the amino molecular sieve and a transition metal salt in an aqueous sodium hydroxide solution, and reacting to obtain an amino molecular sieve-supported transition metal hydroxide catalyst (M(OH) x / NH2-Zeolite); the molecular sieve is a Y-type molecular sieve, a Beta molecular sieve or a ZSM-5 molecular sieve;

[0030] (2) subjecting the amino molecular sieve-supported transition metal hydroxide catalyst obtained in step (1) to phosphating treatment at 250-400° C. in a phosphine gas atmosphere to obtain an amino molecular sieve-supported transition metal phosphide catalyst (M y P / NH2-Zeolite, y is 1 to 2);

[0031] (3) reducing the amino molecular sieve-supported transition metal phosphide catalyst obtained in step (2) at 200-600° C. in a hydrogen atmosphere to obtain the amino molecular sieve-supported transition metal and its phosphide catalyst (MM z P / NH2-Zeolite, z is 1 to 3, z is greater than y).

[0032] The present invention uses amino molecular sieve as a carrier. After the molecular sieve is amino-functionalized, a silane coupling agent with an amino group at the end is grafted inside and on the surface of the pores. Different transition metal salts are selected as transition metal sources. After the amino molecular sieve is loaded with a transition metal hydroxide catalyst by a sodium hydroxide precipitation method, the amino molecular sieve is then subjected to a phosphating treatment to load the amino molecular sieve with a transition metal phosphide catalyst. The amino functionalization can enhance the carrier-metal interaction. The amino groups carried by the molecular sieve form an interaction force with the transition metal species to form a transition metal-N bond, thereby facilitating the dispersion of the transition metal phosphide. Finally, after a reduction treatment, the transition metal phosphide undergoes a crystal transformation in a high-temperature hydrogen atmosphere to obtain an amino molecular sieve loaded with a transition metal and its phosphide catalyst.

[0033] Furthermore, in step (1), the amino-containing silane coupling agent is selected from one or more of 3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropyltriethoxysilane and diethylenetriaminopropyltrimethoxysilane.

[0034] Furthermore, in step (1), the transition metal salt is a nitrate of a transition metal, and the transition metal is selected from one or more of cobalt, nickel, copper, iron, manganese, chromium, molybdenum, tungsten, platinum, palladium, ruthenium, rhodium, osmium, gold, iridium and silver.

[0035] Furthermore, in step (1), the amino functionalization is carried out at 50-100° C. for 2-8 hours.

[0036] Furthermore, in step (1), the specific method of amino functionalization is: dissolving an amino-containing silane coupling agent and a molecular sieve in an organic solvent aqueous solution.

[0037] Furthermore, the organic solvent is ethanol, methanol or ethyl acetate.

[0038] Furthermore, in step (1), the mass ratio of the amino molecular sieve to the transition metal salt is 1:(0.01-2), preferably 1:(0.05-1.5).

[0039] Furthermore, in step (1), the reaction temperature of the amino molecular sieve and the transition metal salt in the sodium hydroxide aqueous solution is 25 to 60° C., and the reaction time is 2 to 4 hours.

[0040] Furthermore, in step (2), the phosphating treatment is carried out in a tubular furnace, and under an inert atmosphere, the molecular sieve-loaded transition metal hydroxide catalyst is placed downstream of the tubular furnace, and sodium hypophosphite is placed upstream of the tubular furnace, and sodium hypophosphite (NaH2PO2) is thermally decomposed to produce phosphine (PH3) gas.

[0041] Furthermore, the mass ratio of the molecular sieve-supported transition metal hydroxide catalyst to sodium hypophosphite is 1:(0.1-20), preferably 1:(0.5-15), and more preferably 1:(0.03-0.3).

[0042] Furthermore, in step (2), the phosphating treatment time is 1 to 4 hours.

[0043] Furthermore, in step (3), the reduction treatment time is 2 to 4 hours.

[0044] The present invention protects the molecular sieve catalyst prepared by the above method, including molecular sieve-loaded transition metal phosphide catalysts, molecular sieve-loaded transition metal and its phosphide catalysts, amino molecular sieve-loaded transition metal phosphide catalysts and amino molecular sieve-loaded transition metal and its phosphide catalysts.

[0045] Furthermore, the mass percentage of transition metal in the molecular sieve catalyst is 1% to 30%.

[0046] The invention also protects the application of four molecular sieve catalysts in the production of hydrogen by hydrolysis of ammonia borane.

[0047] The molecular sieve catalyst provided by the present invention can also eliminate the induction period of the cobalt phosphide catalyst in ammonia borane hydrolysis hydrogen production under non-alkaline conditions by using a gas atmosphere, wherein the gas is hydrogen, nitrogen or an inert gas.

[0048] Furthermore, the inert gas is selected from one of argon, helium, krypton and xenon.

[0049] On this basis, the induction period of the cobalt phosphide catalyst can be eliminated by using a gas atmosphere and light conditions, wherein the gas is hydrogen, nitrogen or an inert gas.

[0050] Furthermore, the illumination condition is ultraviolet visible light irradiation, and the wavelength of the light source is 320-780nm. The amino molecular sieve loaded with transition metal and its phosphide catalyst provided by the present invention has excellent catalytic activity in the hydrolysis of ammonia borane to produce hydrogen. At room temperature, the highest conversion frequency (TOF) reaches 240.0min -1 , surpassing the reported non-precious metal phosphide catalysts and even comparable to some precious metal catalysts.

[0051] Beneficial effects of the present invention:

[0052] 1. The present invention uses molecular sieve as a carrier, selects different metal salts as metal sources, adopts a sodium hydroxide precipitation method to obtain a molecular sieve-loaded transition metal hydroxide catalyst, and then performs a phosphating treatment to obtain the molecular sieve-loaded small-size transition metal phosphide catalyst.

[0053] 2. The present invention uses amino molecular sieve as a carrier. After the molecular sieve is amino-functionalized, a silane coupling agent with an amino group at the end is grafted inside and on the surface of the pores. Different transition metal salts are selected as transition metal sources. After the amino molecular sieve is loaded with a transition metal hydroxide catalyst by a sodium hydroxide precipitation method, the amino molecular sieve is then subjected to a phosphating treatment to load the amino molecular sieve with a transition metal phosphide catalyst. The amino functionalization can enhance the carrier-metal interaction. The amino groups carried by the molecular sieve form an interaction force with the transition metal species to form a transition metal-N bond, which is conducive to the dispersion of the transition metal phosphide. Finally, after a reduction treatment, the transition metal phosphide undergoes a crystal transformation in a high-temperature hydrogen atmosphere to obtain an amino molecular sieve loaded with a transition metal and its phosphide catalyst.

[0054] 3. The molecular sieve-supported transition metal phosphide catalyst provided by the present invention can also eliminate the induction period of the cobalt phosphide catalyst in the hydrolysis of ammonia borane under non-alkaline conditions by using an inert gas atmosphere and / or light conditions.

[0055] 4. The amino molecular sieve loaded with transition metal and its phosphide catalyst provided by the present invention has excellent catalytic activity in hydrogen production by hydrolysis of ammonia borane. At room temperature, the maximum conversion frequency (TOF) reaches 240.0min -1 , surpassing the reported non-precious metal phosphide catalysts and even comparable to some precious metal catalysts. BRIEF DESCRIPTION OF THE DRAWINGS

[0056] Figure 1 The CoP prepared in Example 1 1% / Y catalyst, CoP prepared in Example 2 3% / Y catalyst, CoP prepared in Example 3 5% / XRD patterns of Y catalyst and Y-type molecular sieve.

[0057] Figure 2 These are the XRD patterns of the Beta molecular sieve, NH2-Beta molecular sieve, CoP / NH2-Beta catalyst, Co-Co2P / NH2-Beta catalyst in Example 15 and the CoP / Beta catalyst prepared in Example 4.

[0058] Figure 3 The XRD diagrams of the CoP / SiO2 catalyst and the Co-Co2P / SiO2 catalyst in Comparative Example 2 are shown.

[0059] Figure 4 The CoP prepared in Example 2 3% TEM images and particle size distribution diagram of / Y catalyst; among them, (a), (b), and (c) are TEM images, and (d) is the particle size distribution diagram.

[0060] Figure 5 The CoP prepared in Example 4 5% TEM images and particle size distribution diagram of / Beta catalyst; among them, (a), (b), and (c) are TEM images, and (d) is the particle size distribution diagram.

[0061] Figure 6 The CoP prepared in Example 5 10% TEM images and particle size distribution diagram of / Beta catalyst; among them, (a) and (b) are TEM images, and (c) is the particle size distribution diagram.

[0062] Figure 7 The CoP prepared in Example 6 20% TEM images and particle size distribution diagram of / Beta catalyst; among them, (a) and (b) are TEM images, and (c) is the particle size distribution diagram.

[0063] Figure 8 The CoP prepared in Example 7 30% TEM images and particle size distribution diagram of / Beta catalyst; among them, (a) and (b) are TEM images, and (c) is the particle size distribution diagram.

[0064] Fig. 9 The CoP prepared in Example 8 5% TEM images and particle size distribution diagram of / ZSM-5 catalyst; among them, (a) and (b) are TEM images, and (c) is the particle size distribution diagram.

[0065] Fig.10 The CoP prepared in Comparative Example 1 5% TEM images and particle size distribution diagram of / MCM-41 catalyst; among them, (a) and (b) are TEM images, and (c) is the particle size distribution diagram.

[0066] Fig.11 is the CoP in Comparative Example 2 3% TEM images and particle size distribution diagram of / SiO2 catalyst; among them, (a), (b), and (c) are TEM images, and (d) is the particle size distribution diagram.

[0067] Fig.12 TEM images and particle size distribution diagrams of the CoP / NH2-Beta catalyst in Example 15; wherein (a), (b), and (c) are TEM images, and (d) is a particle size distribution diagram.

[0068] Fig.13 TEM images and particle size distribution diagram of the Co-Co2P / NH2-Beta catalyst prepared in Example 15; wherein (a), (b), and (c) are TEM images, and (d) is a particle size distribution diagram.

[0069] Fig.14 The CoP prepared in Example 2 3% / Y catalyst and CoP in Comparative Example 2 3% / SiO2 catalyst for hydrogen production rate diagram of ammonia borane hydrolysis.

[0070] Fig.15 The CoP prepared in Example 3 5% / Y catalyst is used to catalyze the hydrolysis of ammonia borane under the conditions of gas atmosphere and light, inert gas atmosphere and no light, and no light. The hydrogen production rate diagram of the hydrolysis of ammonia borane is shown in Figure 2; (a) is a hydrogen production rate diagram for the hydrolysis of ammonia borane under inert gas atmosphere and light, inert gas atmosphere and no light, and no light; (b) is a hydrogen production rate diagram for the hydrolysis of ammonia borane under different gas atmospheres and light conditions, and no light.

[0071] Fig.16 The CoP prepared in Example 3 5% / Y catalyst, CoP prepared in Example 4 5% / Beta catalyst, CoP prepared in Example 8 5% / ZSM-5 catalyst and CoP prepared in Comparative Example 1 5% / Hydrogen production rate diagram of MCM-41 catalyst used for catalytic hydrolysis of ammonia borane.

[0072] Fig.17 This is a performance comparison chart of the Beta molecular sieves prepared in Examples 4 and 9 to 14 loaded with different metal phosphide catalysts for catalyzing the hydrolysis of ammonia borane to produce hydrogen.

[0073] Fig.18 This is a graph of the hydrogen production rate when the Beta molecular sieve, CoP / NH2-Beta catalyst, Co-Co2P / NH2-Beta catalyst in Example 15 and the CoP / Beta catalyst prepared in Example 4 are used to catalyze the hydrolysis of ammonia borane.

[0074] Fig.19 This is a graph of the hydrogen production rate of the CoP / NH2-Beta catalyst and the Co-Co2P / NH2-Beta catalyst in Example 15 used to catalyze the hydrolysis of ammonia borane at different hydrogen reduction temperatures.

[0075] Fig. 20 This is a graph of the hydrogen production rate of the Co-Co2P / NH2-Beta catalyst prepared in Example 15 for catalyzing the hydrolysis of ammonia borane under different alkaline environments; wherein (a) represents different alkali concentrations, and (b) represents different alkali solutions.

[0076] Fig.21This is a comparison chart of the activities of the Co-Co2P / NH2-Beta catalyst prepared in Example 15 and the non-precious metal phosphide catalyst reported in the prior art. DETAILED DESCRIPTION

[0077] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.

[0078] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.

[0079] Unless otherwise specified, the experimental methods used in the following examples are all conventional methods, and the materials, reagents, etc. used are all available from commercial sources unless otherwise specified.

[0080] Example 1

[0081] A Y-type molecular sieve supported CoP catalyst (CoP 1% / Y, 1% means that the mass percentage of Co in the Y-type molecular sieve-supported CoP catalyst is 1%), comprising the following steps:

[0082] (1) Add 0.5 g of Y-type molecular sieve (Si / Al=12) to a 100 mL beaker, add 50 mL of ultrapure water, stir at 25°C for 5 min and ultrasonically treat for 30 min to obtain a Y-type molecular sieve solution; add 0.025 g of cobalt nitrate hexahydrate to the Y-type molecular sieve solution, continue to stir at 25°C for 1 h to obtain a mixed solution; add 0.172 mL of sodium hydroxide aqueous solution (concentration of 1 mol / L) to the mixed solution, continue to stir at 25°C for 30 min, centrifuge the contents of the beaker to separate the solid product, repeatedly wash the solid product with ultrapure water, and then freeze-dry to obtain a Co(OH)2 / Y catalyst.

[0083] (2) 0.3 g of the Co(OH)2 / Y catalyst obtained in step (1) was placed downstream of the quartz boat, and 0.15 g of sodium hypophosphite was placed upstream of the quartz boat. The phosphating treatment was performed in a tube furnace in an argon atmosphere. The temperature was raised to 300° C. for 2 h, and then kept at 300° C. for 2 h to obtain CoP 1% / Y catalyst.

[0084] Example 2

[0085] A Y-type molecular sieve supported CoP catalyst (CoP 3% / Y, 3% means that the mass percentage of Co in the Y-type molecular sieve-supported CoP catalyst is 3%), comprising the following steps:

[0086] (1) Add 0.5 g of Y-type molecular sieve (Si / Al=12) to a 100 mL beaker, add 50 mL of ultrapure water, stir at 25°C for 5 min and ultrasonically treat for 30 min to obtain a Y-type molecular sieve solution; add 0.075 g of cobalt nitrate hexahydrate to the Y-type molecular sieve solution, continue to stir at 25°C for 1 h to obtain a mixed solution; add 0.516 mL of sodium hydroxide aqueous solution (concentration of 1 mol / L) to the mixed solution, continue to stir at 25°C for 30 min, centrifuge the contents of the beaker to separate the solid product, repeatedly wash the solid product with ultrapure water, and then freeze-dry to obtain a Co(OH)2 / Y catalyst.

[0087] (2) 0.3 g of the Co(OH)2 / Y catalyst obtained in step (1) was placed downstream of the quartz boat, and 0.45 g of sodium hypophosphite was placed upstream of the quartz boat. The phosphating treatment was performed in a tube furnace in an argon atmosphere. The temperature was raised to 300° C. for 2 h, and then kept at 300° C. for 2 h to obtain CoP 3% / Y catalyst.

[0088] Example 3

[0089] A Y-type molecular sieve supported CoP catalyst (CoP 5% / Y, 5% means that the mass percentage of Co in the Y-type molecular sieve-supported CoP catalyst is 5%), comprising the following steps:

[0090] (1) 0.5 g of Y-type molecular sieve (Si / Al=12) was added to a 100 mL beaker, and 50 mL of ultrapure water was added, and the mixture was stirred at 25°C for 5 min and ultrasonically treated for 30 min to obtain a Y-type molecular sieve solution; 0.125 g of cobalt nitrate hexahydrate was added to the Y-type molecular sieve solution, and the mixture was stirred at 25°C for 1 h to obtain a mixed solution; 0.860 mL of sodium hydroxide aqueous solution (concentration of 1 mol / L) was added to the mixed solution, and the mixture was stirred at 25°C for 30 min, the solid product was separated by centrifugation, the solid product was repeatedly washed with ultrapure water, and then freeze-dried to obtain a Co(OH)2 / Y catalyst.

[0091] (2) 0.3 g of the Co(OH)2 / Y catalyst obtained in step (1) was placed downstream of the quartz boat, and 0.75 g of sodium hypophosphite was placed upstream of the quartz boat. The phosphating treatment was performed in a tube furnace in an argon atmosphere. The temperature was raised to 300° C. for 2 h, and then kept at 300° C. for 2 h to obtain CoP 5% / Y catalyst.

[0092] Example 4

[0093] A Beta molecular sieve supported CoP catalyst (CoP 5% / Beta, 5% means that the mass percentage of Co in the Beta molecular sieve-supported CoP catalyst is 5%), comprising the following steps:

[0094] (1) Add 0.5 g of Beta molecular sieve (Si / Al=12) to a 100 mL beaker, add 50 mL of ultrapure water, stir at 25°C for 5 min and ultrasonically treat for 30 min to obtain a Beta molecular sieve solution; add 0.125 g of cobalt nitrate hexahydrate to the Beta molecular sieve solution, continue to stir at 25°C for 1 h to obtain a mixed solution; add 0.860 mL of sodium hydroxide aqueous solution (concentration of 1 mol / L) to the mixed solution, continue to stir at 25°C for 30 min, centrifuge the contents of the beaker to separate the solid product, repeatedly wash the solid product with ultrapure water, and then freeze-dry to obtain a Co(OH)2 / Beta catalyst.

[0095] (2) 0.3 g of the Co(OH)2 / Beta catalyst obtained in step (1) was placed downstream of the quartz boat, and 0.75 g of sodium hypophosphite was placed upstream of the quartz boat. The phosphating treatment was performed in a tube furnace in an argon atmosphere. The temperature was raised to 300° C. for 2 h, and then kept at 300° C. for 2 h to obtain CoP 5% / Beta catalyst.

[0096] Example 5

[0097] A Beta molecular sieve supported CoP catalyst (CoP 10% / Beta, 10% means the mass percentage of Co in the Beta molecular sieve-supported CoP catalyst is 10%), comprising the following steps:

[0098] (1) Add 0.5 g of Beta molecular sieve (Si / Al=12) to a 100 mL beaker, add 50 mL of ultrapure water, stir at 25°C for 5 min and ultrasonically treat for 30 min to obtain a Beta molecular sieve solution; add 0.250 g of cobalt nitrate hexahydrate to the Beta molecular sieve solution, continue to stir at 25°C for 1 h to obtain a mixed solution; add 1.720 mL of sodium hydroxide aqueous solution (concentration of 1 mol / L) to the mixed solution, continue to stir at 25°C for 30 min, centrifuge the contents of the beaker to separate the solid product, repeatedly wash the solid product with ultrapure water, and then freeze-dry to obtain a Co(OH)2 / Beta catalyst.

[0099] (2) 0.3 g of the Co(OH)2 / Beta catalyst obtained in step (1) was placed downstream of the quartz boat, and 1.50 g of sodium hypophosphite was placed upstream of the quartz boat. The phosphating treatment was performed in a tube furnace in an argon atmosphere. The temperature was raised to 300° C. for 2 h, and then kept at 300° C. for 2 h to obtain CoP 10% / Beta catalyst.

[0100] Example 6

[0101] A Beta molecular sieve supported CoP catalyst (CoP 20% / Beta, 20% means that the mass percentage of Co in the Beta molecular sieve-supported CoP catalyst is 20%), comprising the following steps:

[0102] (1) Add 0.5 g of Beta molecular sieve (Si / Al=12) to a 100 mL beaker, add 50 mL of ultrapure water, stir at 25°C for 5 min and ultrasonically treat for 30 min to obtain a Beta molecular sieve solution; add 0.500 g of cobalt nitrate hexahydrate to the Beta molecular sieve solution, continue to stir at 25°C for 1 h to obtain a mixed solution; add 3.440 mL of sodium hydroxide aqueous solution (concentration of 1 mol / L) to the mixed solution, continue to stir at 25°C for 30 min, centrifuge the contents of the beaker to separate the solid product, repeatedly wash the solid product with ultrapure water, and then freeze-dry to obtain a Co(OH)2 / Beta catalyst.

[0103] (2) 0.3 g of the Co(OH)2 / Beta catalyst obtained in step (1) was placed downstream of the quartz boat, and 3.00 g of sodium hypophosphite was placed upstream of the quartz boat. The phosphating treatment was performed in a tube furnace in an argon atmosphere. The temperature was raised to 300° C. for 2 h, and then kept at 300° C. for 2 h to obtain CoP 20% / Beta catalyst.

[0104] Example 7

[0105] A Beta molecular sieve supported CoP catalyst (CoP 30% / Beta, 30% means that the mass percentage of Co in the Beta molecular sieve-supported CoP catalyst is 30%), comprising the following steps:

[0106] (1) Add 0.5 g of Beta molecular sieve (Si / Al=12) to a 100 mL beaker, add 50 mL of ultrapure water, stir at 25°C for 5 min and ultrasonically treat for 30 min to obtain a Beta molecular sieve solution; add 0.750 g of cobalt nitrate hexahydrate to the Beta molecular sieve solution, continue to stir at 25°C for 1 h to obtain a mixed solution; add 5.160 mL of sodium hydroxide aqueous solution (concentration of 1 mol / L) to the mixed solution, continue to stir at 25°C for 30 min, centrifuge the contents of the beaker to separate the solid product, repeatedly wash the solid product with ultrapure water, and then freeze-dry to obtain a Co(OH)2 / Beta catalyst.

[0107] (2) 0.3 g of the Co(OH)2 / Beta catalyst obtained in step (1) was placed downstream of the quartz boat, and 4.50 g of sodium hypophosphite was placed upstream of the quartz boat. The phosphating treatment was performed in a tube furnace in an argon atmosphere. The temperature was raised to 300° C. for 2 h, and then kept at 300° C. for 2 h to obtain CoP 30% / Beta catalyst.

[0108] Example 8

[0109] A ZSM-5 molecular sieve supported CoP catalyst (CoP 5% / ZSM-5, 5% refers to the mass percentage of Co in the ZSM-5 molecular sieve supported CoP catalyst is 5%), comprising the following steps:

[0110] (1) 0.5 g of ZSM-5 molecular sieve (Si / Al=12) was added to a 100 mL beaker, and 50 mL of ultrapure water was added, and the mixture was stirred at 25° C. for 5 min and ultrasonically treated for 30 min to obtain a ZSM-5 molecular sieve solution; 0.125 g of cobalt nitrate hexahydrate was added to the ZSM-5 molecular sieve solution, and the mixture was stirred at 25° C. for 1 h to obtain a mixed solution; 0.860 mL of sodium hydroxide aqueous solution (concentration of 1 mol / L) was added to the mixed solution, and the mixture was stirred at 25° C. for 30 min, the solid product was separated by centrifugation, the solid product was repeatedly washed with ultrapure water, and then freeze-dried to obtain a Co(OH)2 / ZSM-5 catalyst.

[0111] (2) 0.3 g of the Co(OH)2 / ZSM-5 catalyst obtained in step (1) was placed downstream of the quartz boat, and 0.75 g of sodium hypophosphite was placed upstream of the quartz boat. The catalyst was subjected to phosphating treatment in a tube furnace in an argon atmosphere. The temperature was raised to 300° C. for 2 h, and then kept at 300° C. for 2 h to obtain CoP 5% / ZSM-5 catalyst.

[0112] Example 9

[0113] A Beta molecular sieve supported NiP catalyst (NiP 5% / Beta, 5% means that the mass percentage of Ni in the Beta molecular sieve supported NiP catalyst is 5%), which is basically the same as that in Example 4, except that: in step (1), 0.125g of cobalt nitrate hexahydrate is replaced by 0.125g of nickel nitrate hexahydrate.

[0114] Example 10

[0115] A Beta molecular sieve supported CuP catalyst (CuP 5% / Beta, 5% means that the mass percentage of Cu in the Beta molecular sieve-supported CuP catalyst is 5%) is basically the same as that in Example 4, except that in step (1), 0.125 g of cobalt nitrate hexahydrate is replaced by 0.095 g of copper nitrate trihydrate.

[0116] Embodiment 11

[0117] A Beta molecular sieve supported FeP catalyst (FeP 5% / Beta, 5% means that the mass percentage of Fe in the Beta molecular sieve supported FeP catalyst is 5%), which is basically the same as that in Example 4, except that: in step (1), 0.125g of cobalt nitrate hexahydrate is replaced by 0.181g of ferric nitrate nonahydrate.

[0118] Example 12

[0119] A Beta molecular sieve supported CrP catalyst (CrP 5% / Beta, 5% means that the mass percentage of Cr in the Beta molecular sieve supported CrP catalyst is 5%), which is basically the same as that in Example 4, except that: in step (1), 0.125g of cobalt nitrate hexahydrate is replaced by 0.192g of chromium nitrate nonahydrate.

[0120] Embodiment 13

[0121] A Beta molecular sieve supported MnP catalyst (MnP 5% / Beta, 5% means that the mass percentage of Mn in the Beta molecular sieve supported MnP catalyst is 5%), which is basically the same as that in Example 4, except that in step (1), 0.125g of cobalt nitrate hexahydrate is replaced by 0.114g of manganese nitrate tetrahydrate.

[0122] Embodiment 14

[0123] A Beta molecular sieve supported MoP catalyst (MoP 5% / Beta, 5% means that the mass percentage of Mo in the Beta molecular sieve supported MoP catalyst is 5%), which is basically the same as that in Example 4, except that: in step (1), 0.125g of cobalt nitrate hexahydrate is replaced by 0.071g of molybdenum pentachloride.

[0124] Comparative Example 1

[0125] A MCM-41 molecular sieve supported CoP catalyst (CoP 5% / MCM-41, 5% refers to the mass percentage of Co in the MCM-41 molecular sieve supported CoP catalyst is 5%), comprising the following steps:

[0126] (1) Add 0.5 g of MCM-41 molecular sieve (Si / Al=12) to a 100 mL beaker, add 50 mL of ultrapure water, stir at 25°C for 5 min and ultrasonically treat for 30 min to obtain an MCM-41 molecular sieve solution; add 0.125 g of cobalt nitrate hexahydrate to the MCM-41 molecular sieve solution, continue to stir at 25°C for 1 h to obtain a mixed solution; add 0.860 mL of sodium hydroxide aqueous solution (concentration of 1 mol / L) to the mixed solution, continue to stir at 25°C for 30 min, centrifuge the contents of the beaker to separate the solid product, repeatedly wash the solid product with ultrapure water, and then freeze-dry to obtain a Co(OH)2 / MCM-41 catalyst.

[0127] (2) 0.3 g of the Co(OH)2 / MCM-41 catalyst obtained in step (1) was placed downstream of the quartz boat, and 0.75 g of sodium hypophosphite was placed upstream of the quartz boat. The catalyst was subjected to phosphating treatment in a tube furnace in an argon atmosphere. The temperature was raised to 300°C for 2 h, and then kept at 300°C for 2 h to obtain CoP 5% / MCM-41 catalyst.

[0128] Embodiment 15

[0129] A method for preparing an amino Beta molecular sieve loaded with Co and Co2P catalyst (Co-Co2P / NH2-Beta), comprising the following steps:

[0130] (1) 1.0 g of Beta molecular sieve (Si / Al=25) was added to a 100 mL two-necked flask, and 45 mL of ethanol and 5 mL of ultrapure water were added, and the mixture was stirred at 25°C for 5 min and ultrasonically treated for 30 min to obtain a Beta molecular sieve solution; 1 mL of 3-aminopropyltriethoxysilane was added to the Beta molecular sieve solution, and the mixture was stirred at 25°C for 30 min, and stirred and refluxed at 60°C for 4 h for amino functionalization treatment, and then naturally cooled to room temperature; the contents of the flask were centrifuged to separate the solid product, and the solid product was repeatedly washed with ultrapure water, and then dried in an oven at 80°C to obtain NH2-Beta molecular sieve.

[0131] (2) Add 0.5 g NH2-Beta to a 100 mL beaker, add 50 mL ultrapure water, stir at 25 ° C for 5 min and ultrasonically treat for 30 min to obtain an NH2-Beta molecular sieve solution; add 0.125 g cobalt nitrate hexahydrate to the NH2-Beta molecular sieve solution, continue to stir at 25 ° C for 1 hour to obtain a mixed solution; add 0.860 mL of sodium hydroxide aqueous solution (concentration of 1 mol / L) to the mixed solution, and continue to stir at 25 ° C for 30 min; centrifuge the contents of the beaker to separate the solid product, repeatedly wash the solid product with ultrapure water, and then freeze-dry to obtain Co(OH)2 / NH2-Beta catalyst.

[0132] (3) 0.3 g of the Co(OH)2 / NH2-Beta catalyst obtained in step (2) is placed downstream of the quartz boat, and 0.75 g of sodium hypophosphite is placed upstream of the quartz boat. The mixture is subjected to phosphating treatment in a tubular furnace in an argon atmosphere. The temperature is raised to 300° C. for 2 h, and then maintained at 300° C. for 2 h to obtain a CoP / NH2-Beta catalyst.

[0133] (4) The CoP / NH2-Beta catalyst obtained in step (3) is placed in a tubular furnace for H2 reduction treatment, the temperature is raised to 300°C for 2 hours, and then kept at 300°C for 2 hours to obtain a Co-Co2P / NH2-Beta catalyst.

[0134] Comparative Example 2

[0135] A method for preparing a SiO2-loaded Co and Co2P catalyst (Co-Co2P / SiO2) comprises the following steps:

[0136] (1) Add 0.5 g of SiO2 to a 100 mL beaker, add 50 mL of ultrapure water, stir at 25°C for 5 min and ultrasonically treat for 30 min to obtain a SiO2 solution; add 0.075 g of cobalt nitrate hexahydrate to the SiO2 solution, continue to stir at 25°C for 1 h to obtain a mixed solution; add 0.520 mL of sodium hydroxide aqueous solution (concentration of 1 mol / L) to the mixed solution, continue to stir at 25°C for 30 min, centrifuge the contents of the beaker to separate the solid product, repeatedly wash the solid product with ultrapure water, and then freeze-dry to obtain a Co(OH)2 / SiO2 catalyst.

[0137] (2) 0.3 g of the Co(OH)2 / SiO2 catalyst obtained in step (1) was placed downstream of the quartz boat, and 0.45 g of sodium hypophosphite was placed upstream of the quartz boat, and phosphating treatment was performed in a tube furnace in an argon atmosphere. The temperature was raised to 300° C. for 2 h, and then kept at 300° C. for 2 h to obtain a CoP / SiO2 catalyst (CoP 3% / SiO2, 3% means that the mass percentage of Co in the CoP / SiO2 catalyst is 3%).

[0138] (3) The CoP / SiO2 catalyst obtained in step (2) is placed in a tubular furnace for H2 reduction treatment, the temperature is raised to 300°C for 2 hours, and then kept at 300°C for 2 hours to obtain a Co-Co2P / SiO2 catalyst.

[0139] Test Example 1

[0140] The crystal structures of the catalysts in Examples 1 to 3, Example 15 and Comparative Example 2 were characterized by X-ray diffraction (XRD).

[0141] Figure 1 The CoP prepared in Example 1 1% / Y catalyst, CoP prepared in Example 2 3% / Y catalyst, CoP prepared in Example 3 5% XRD patterns of / Y catalyst and Y-type molecular sieve, from Figure 1 It can be seen that the catalysts prepared in Examples 1 to 3 maintain a complete FAU topological structure.

[0142] Figure 2 The Beta molecular sieve in Example 15 (i.e., H-Beta in the figure), NH2-Beta molecular sieve, CoP / NH2-Beta catalyst, Co-Co2P / NH2-Beta catalyst and CoP prepared in Example 4 5% / Beta catalyst (i.e. CoP / Beta in the figure), from Figure 2It can be seen that the catalysts prepared in Example 15 and Example 4 both retain complete * BEA topology.

[0143] Figure 3 The XRD patterns of the CoP / SiO2 catalyst and the Co-Co2P / SiO2 catalyst in Comparative Example 2 are shown in FIG. Figure 3 It can be seen that high-temperature hydrogen reduction transforms CoP into Co2P.

[0144] Test Example 2

[0145] Transmission electron microscopy (TEM) was used to characterize the microscopic morphology of Example 2, Examples 4 to 8, Example 15 and Comparative Examples 1 to 2 and to test their particle size distribution.

[0146] Figure 4 The CoP prepared in Example 2 3% TEM image and particle size distribution of / Y catalyst, the average particle size of CoP nanoparticles is 1.9 nm.

[0147] Figure 5 The CoP prepared in Example 4 5% TEM image and particle size distribution of / Beta catalyst. The average particle size of CoP nanoparticles is 3.4 nm.

[0148] Figure 6 The CoP prepared in Example 5 10% TEM image and particle size distribution of / Beta catalyst. The average particle size of CoP nanoparticles is 4.0 nm.

[0149] Figure 7 The CoP prepared in Example 6 20% TEM image and particle size distribution of / Beta catalyst. The average particle size of CoP nanoparticles is 4.7 nm.

[0150] Figure 8 The CoP prepared in Example 7 30% TEM image and particle size distribution diagram of / Beta catalyst. The average particle size of CoP nanoparticles is 4.9 nanometers. After the Co content increases to 30%, the size of CoP particles is still less than 5nm, which reflects the advantages of acidic molecular sieve carrier.

[0151] Fig. 9 The CoP prepared in Example 8 5% TEM image and particle size distribution of ZSM-5 catalyst. The average particle size of CoP nanoparticles is 4.5 nm, slightly larger than that of CoP with the same Co content. 5% / Beta catalyst, but still smaller than 5nm.

[0152] Fig.10 The CoP prepared in Comparative Example 1 5% TEM image and particle size distribution of MCM-41 catalyst. The average particle size of CoP nanoparticles is 15.9 nm, which is the highest among CoP nanoparticles with the same Co content. 5% / Beta catalyst is about 4.6 times the average particle size of CoP nanoparticles.

[0153] Fig.11 is the CoP in Comparative Example 2 3% TEM image and particle size distribution diagram of / SiO2 catalyst, the average particle size of CoP nanoparticles is 7.7 nanometers, and no one is less than 5nm.

[0154] Fig.12 The TEM image and particle size distribution diagram of the CoP / NH2-Beta catalyst in Example 15 show that the average particle size of the CoP nanoparticles is 3.1 nanometers, which is similar to that of the CoP prepared in Example 4. 5% Compared with the Beta catalyst, the size of CoP nanoparticles was reduced after amino functionalization.

[0155] Fig.13 TEM image and particle size distribution diagram of the Co-Co2P / NH2-Beta catalyst prepared in Example 15. The average particle size of the Co2P nanoparticles is 2.9 nanometers. Compared with the CoP / NH2-Beta catalyst, CoP is converted into Co2P after hydrogen reduction, and the size of the Co2P nanoparticles is reduced again.

[0156] Test Example 3

[0157] The CoP prepared in Example 2 3% / Y catalyst and CoP in Comparative Example 2 3% / SiO2 catalyst was used for hydrogen production by hydrolysis of ammonia borane and its catalytic activity was tested.

[0158] The test method is as follows: the hydrolysis reaction of ammonia borane (AB) is carried out in a double-necked flask at normal pressure, and an appropriate amount of catalyst (n Co / n AB =0.03) and 0.5mL ultrapure water are added to the flask, and ultrasonic treatment for 2min forms a uniform solution. The reaction system is purged with nitrogen to completely remove oxygen. The temperature is controlled (298K) by a circulating water bath, and the magnetic stirring speed is set to 600rpm. Subsequently, 0.5mL ammonia borane aqueous solution (2.0M, ammonia borane consumption is 1mmol) is rapidly injected into the flask to start the reaction immediately. The rate of gas generation is measured by the drainage method, the flask is tailed with a drainage device, and the quality of the discharged water is recorded in real time using an analytical balance.

[0159] The test results are as follows Fig.14 As shown, Fig.14 The CoP prepared in Example 2 3% / Y catalyst and CoP in Comparative Example 2 3% / SiO2 catalyst for the hydrogen production rate diagram of ammonia borane hydrolysis, compared with CoP 3% / Y catalyst, CoP 3% / SiO2 catalyst still has an induction period of about 5 minutes.

[0160] Test Example 4

[0161] The CoP prepared in Example 3 5% / Y catalyst is used to catalyze the hydrolysis of ammonia borane to produce hydrogen, and its catalytic performance is tested.

[0162] The test method is: add 40mg CoP into the photocatalytic reactor 5% / Y catalyst and 0.5mL ultrapure water were ultrasonically treated for 2min to form a uniform solution, and then the reaction was carried out in a double-jacketed flask. The reaction temperature was controlled by an external circulating water bath, and the magnetic stirring speed was set to 600rpm. The reaction system was purged with gas to completely remove oxygen. Then, ammonia borane solution (0.5mL, 2.0M) was injected into the reactor under UV-visible light irradiation, and the amount of H2 precipitation was monitored by the drainage method. UV-visible light conditions: A 300W xenon lamp (PLS-SXE300UV, Beijing Bofeilai Technology Co., Ltd.) was used as the light source, with a wavelength range of 320-780nm, a total output light power of 50W, and a light power density of 2000mW / cm -2 .

[0163] Test results such as Fig.15 As shown, Fig.15 The CoP prepared in Example 3 5% / Y catalyst is used to catalyze the hydrolysis of ammonia borane under the conditions of gas atmosphere and light; (a) is the hydrogen production rate diagram for the hydrolysis of ammonia borane under the conditions of inert gas atmosphere and light, inert gas atmosphere, no light and no light, (b) is the hydrogen production rate diagram for the hydrolysis of ammonia borane under different gas atmospheres and light conditions, and no light. Fig.15 It can be seen that under non-alkaline conditions, the introduction of inert atmosphere and UV-visible light successfully eliminates the induction period of cobalt phosphide.

[0164] Test Example 5

[0165] The catalysts prepared in Example 3, Example 4, Example 8 and Comparative Example 1 were used to catalyze the hydrolysis of ammonia borane to produce hydrogen, and their catalytic performance was tested.

[0166] The test method is as follows: the hydrolysis reaction of ammonia borane (AB) is carried out in a double-necked flask at normal pressure, and an appropriate amount of catalyst (n Co / n AB =0.03) and 1.5mL sodium hydroxide solution (2.0M) were added to the flask, and ultrasonic treatment was performed for 2min to form a uniform solution. The temperature was controlled at 298K by a circulating water bath, and the magnetic stirring speed was set to 600rpm. Subsequently, 0.5mL ammonia borane aqueous solution (2.0M, ammonia borane consumption was 1mmol) was rapidly injected into the flask to start the reaction immediately. The rate of gas generation was measured by the water displacement method, and the flask was connected to a water displacement device, and the quality of the discharged water was recorded in real time using an analytical balance.

[0167] The test results are as follows Fig.16 As shown, Fig.16 The CoP prepared in Example 3 5% / Y catalyst, CoP prepared in Example 4 5% / Beta catalyst, CoP prepared in Example 8 5% / ZSM-5 catalyst and CoP prepared in Comparative Example 1 5% / The hydrogen production rate diagram of MCM-41 catalyst for the hydrolysis of ammonia borane, from Fig.16 It can be seen that CoP 5% / Y catalyst, CoP 5% / Beta Catalyst and CoP 5% The catalytic performance of ZSM-5 catalyst is better than that of CoP 5% / MCM-41 catalyst.

[0168] Test Example 6

[0169] The catalysts prepared in Example 4 and Examples 9 to 14 were used to catalyze the hydrolysis of ammonia borane to produce hydrogen, and their catalytic performance was tested.

[0170] The test method is as follows: the hydrolysis reaction of ammonia borane is carried out in a double-necked flask at normal pressure. First, an appropriate amount of catalyst (n Co / n AB =0.09) and 1.5mL sodium hydroxide solution (2.0M) were added to the flask, and ultrasonic treatment was performed for 2min to form a uniform solution. The temperature was controlled at 298K by a circulating water bath, and the magnetic stirring speed was set to 600rpm. Subsequently, 0.5mL ammonia borane aqueous solution (2.0M, ammonia borane consumption was 1mmol) was rapidly injected into the flask to start the reaction immediately. The rate of gas generation was measured by the water displacement method, and the flask was connected to a water displacement device, and the quality of the discharged water was recorded in real time using an analytical balance.

[0171] The test results are as follows Fig.17 As shown, Fig.17The performance comparison of Beta molecular sieves loaded with different metal phosphide catalysts to catalyze the hydrolysis of ammonia borane to produce hydrogen is shown in Figure 4 and Figure 9-14. Fig.17 It can be seen that only Ni and Co metal phosphide catalysts are active in catalyzing the hydrolysis of ammonia borane to produce hydrogen, while metal phosphide catalysts of other elements are inactive.

[0172] Test Example 7

[0173] The catalyst in Example 15 was used to catalyze the hydrolysis of ammonia borane to produce hydrogen, and its catalytic performance was tested.

[0174] The test method is as follows: the hydrolysis reaction of ammonia borane is carried out in a double-necked flask at normal pressure, and an appropriate amount of catalyst (n Co / n AB =0.03) and 1.5mL sodium hydroxide solution (2.0M) were added to the flask, and ultrasonic treatment was performed for 2min to form a uniform solution. The temperature was controlled at 298K by a circulating water bath, and the magnetic stirring speed was set to 600rpm. Subsequently, 0.5mL ammonia borane aqueous solution (2.0M, ammonia borane consumption was 1mmol) was rapidly injected into the flask to start the reaction immediately. The rate of gas generation was measured by the water displacement method, and the flask was connected to a water displacement device, and the quality of the discharged water was recorded in real time using an analytical balance.

[0175] Test results such as Fig.18 , Fig.19 , Fig. 20 and Fig.21 As shown, Fig.18 The Beta molecular sieve, CoP / NH2-Beta catalyst, Co-Co2P / NH2-Beta catalyst and CoP prepared in Example 4 are 5% / Beta catalyst (i.e. CoP / Beta in the figure) is used to catalyze the hydrogen production rate of ammonia borane hydrolysis. Fig.18 It can be seen that the transformation of CoP to Co2P and the formation of elemental Co are beneficial to accelerate the hydrolysis of ammonia borane to produce hydrogen.

[0176] Fig.19 The graph shows the hydrogen production rate of the CoP / NH2-Beta catalyst and the Co-Co2P / NH2-Beta catalyst in Example 15 for catalyzing the hydrolysis of ammonia borane at different hydrogen reduction temperatures (the reduction temperature of step (4) in Example 15).

[0177] Fig. 20 The figure is a graph of the hydrogen production rate of the Co-Co2P / NH2-Beta catalyst prepared in Example 15 for catalyzing the hydrolysis of ammonia borane under different alkaline environments; wherein (a) is different alkali concentrations, and (b) is different alkali solutions. Fig. 20It can be seen that alkalinity helps to improve the activity of transition metal phosphides. The stronger the base, the higher the activity of the transition metal phosphides.

[0178] Fig.21 The activity comparison chart of the Co-Co2P / NH2-Beta catalyst prepared in Example 15 and the non-precious metal phosphide catalyst reported in the prior art. At room temperature, the TOF value of the Co-Co2P / NH2-Beta catalyst reached a maximum of 240.0 min -1 , surpassing the reported non-precious metal phosphide catalysts and even comparable to some precious metal catalysts.

[0179] Obviously, the above embodiments of the present invention are only examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. Those skilled in the art should understand that other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.

Claims

1. A method for preparing a molecular sieve catalyst, It is characterized in that The following steps are involved: (1) dissolving a molecular sieve and a transition metal salt in an alkaline solution, and reacting to obtain a molecular sieve-supported transition metal hydroxide catalyst; the molecular sieve is a Y-type molecular sieve, a Beta molecular sieve or a ZSM-5 molecular sieve; (2) subjecting the molecular sieve-supported transition metal hydroxide catalyst obtained in step (1) to phosphating treatment at 250-400° C. in a phosphine gas atmosphere to obtain a molecular sieve-supported transition metal phosphide catalyst; or (1) dissolving a molecular sieve and a transition metal salt in an alkaline solution, and reacting to obtain a molecular sieve-supported transition metal hydroxide catalyst; the molecular sieve is a Y-type molecular sieve, a Beta molecular sieve or a ZSM-5 molecular sieve; (2) subjecting the molecular sieve-supported transition metal hydroxide catalyst obtained in step (1) to phosphating treatment at 250-400° C. in a phosphine gas atmosphere to obtain a molecular sieve-supported transition metal phosphide catalyst; (3) The molecular sieve-supported transition metal phosphide catalyst obtained in step (2) is subjected to reduction treatment at 200-600° C. in a hydrogen atmosphere to obtain a molecular sieve-supported transition metal and its phosphide catalyst.

2. The preparation method according to claim 1, It is characterized in that Step (1) also includes a step of using an amino-containing silane coupling agent to functionalize the surface of the molecular sieve with amino groups.

3. The preparation method according to claim 2, It is characterized in that The amino-containing silane coupling agent is selected from one or more of 3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropyltriethoxysilane and diethylenetriaminopropyltrimethoxysilane.

4. The preparation method according to claim 1, It is characterized in that In step (1), the transition metal salt is a nitrate or chloride of a transition metal, and the transition metal is selected from one or more of cobalt, nickel, copper, iron, manganese, chromium, molybdenum, tungsten, platinum, palladium, ruthenium, rhodium, osmium, gold, iridium and silver.

5. The preparation method according to claim 1, It is characterized in that In step (2), the phosphating treatment is carried out in a tubular furnace. Under an inert atmosphere, a molecular sieve-loaded transition metal hydroxide catalyst is placed downstream of the tubular furnace, and sodium hypophosphite is placed upstream of the tubular furnace. The sodium hypophosphite is thermally decomposed to produce phosphine gas.

6. A molecular sieve catalyst prepared by the method according to any one of claims 1 to 5.

7. The molecular sieve catalyst according to claim 6, It is characterized in that The mass percentage of transition metal in the molecular sieve catalyst is 1% to 30%.

8. Use of the molecular sieve catalyst according to claim 6 or 7 in hydrogen production by hydrolysis of ammonia borane.

9. The use according to claim 8, It is characterized in that Ammonia borane is hydrolyzed to produce hydrogen in a gas atmosphere, wherein the gas is hydrogen, nitrogen or an inert gas.

10. The use according to claim 8, It is characterized in that Ammonia borane is hydrolyzed to produce hydrogen under gas atmosphere and light conditions, and the gas is hydrogen, nitrogen or inert gas.