Titanium / steel composite plate and preparation method thereof

By using nickel-chromium-vana composite intermediate layer and forging process in titanium/steel composite panels, the problems of joint brittleness and intermetallic compounds are solved, and the effect of high interface bonding strength and simplified process is achieved, which is suitable for industrial production.

CN118926342APending Publication Date: 2024-11-12INST OF METAL RESEARCH - CHINESE ACAD OF SCI
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411227584.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-11-12

Smart Images

  • Figure CN118926342A_ABST
    Figure CN118926342A_ABST
Patent Text Reader

Abstract

The invention provides a titanium / steel composite plate and a preparation method thereof, and the preparation method is characterized by comprising the following steps: assembling: stacking and assembling a steel substrate, a nickel foil, a chromium foil, a vanadium foil and a titanium substrate in sequence to obtain a combined blank; heat preservation is conducted, specifically, the combined blank is placed in an alloy steel sheath for vacuum packaging, and then heat preservation treatment is conducted; forging is conducted, specifically, the combined blank subjected to heat preservation treatment is forged; and post-treatment is conducted, specifically, post-treatment is conducted on the forged combined blank, and the titanium / steel composite plate is obtained. The nickel-chromium-vanadium composite intermediate layer is added between the steel substrate and the titanium substrate (at the interface bonding position), and the steel substrate, the nickel foil, the chromium foil, the vanadium foil and the titanium substrate are assembled in sequence, so that on one hand, mutual diffusion of elements such as iron and titanium is inhibited, on the other hand, intermetallic compounds are prevented from being generated between the intermediate layer and steel and titanium, and the service life of the steel substrate is prolonged. Therefore, the interface bonding strength of the titanium / steel composite plate is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of titanium / steel composite plate preparation, and in particular relates to a titanium / steel composite plate using a nickel-chromium-vanadium composite intermediate layer and a preparation method thereof. Background Art

[0002] Steel has good mechanical properties and is inexpensive, but due to its poor corrosion resistance, most marine steel and steel in special environments have short maintenance cycles, high costs, and very limited service life. Titanium has excellent corrosion resistance and is widely used in marine, aerospace, chemical and other fields, but due to its high price, using a large amount of titanium as a substrate will greatly increase costs. The combination of the two in the form of plates can achieve a combination of their advantages, with both the excellent mechanical properties of steel and the corrosion resistance of titanium. While improving product performance, the cost is also greatly reduced, meeting the needs of the automotive industry, aerospace, and chemical industry.

[0003] Existing titanium / steel composite plates are usually directly composited with titanium steel plates by explosive welding or hot rolling. The titanium / steel composite plates obtained by explosive welding have a unique wavy interface at the joint, which greatly improves the interface bonding strength and is basically close to the matrix strength. However, this method has a low yield rate on the one hand, and on the other hand, it has great environmental pollution, huge energy consumption and is difficult to mass produce. The heterogeneous metal joints obtained by hot rolling often contain a large amount of TiC, FeTi and Fe2Ti, which makes the joint brittle and has poor performance, making it difficult to achieve the performance of the matrix.

[0004] In order to avoid joint brittleness, it is necessary to eliminate various intermetallic compounds that cause stress concentration at the joint. By adding an intermediate layer, direct contact between titanium and steel can be avoided, and the mutual diffusion of iron and titanium atoms at the joint can be suppressed, thereby effectively eliminating various intermetallic compounds. At present, the intermediate layers that have been tried more are pure iron, nickel, silver, copper, niobium, vanadium, aluminum and other pure metals and some alloy intermediate layers. However, most of the intermediate layers will still form new intermetallic compounds with titanium, and the newly generated intermetallic compounds will also affect the interface bonding strength to a certain extent. For example, the prior art discloses a high-temperature rolling method for a titanium / steel composite plate with nickel as an intermediate layer, and hot rolling is performed on the combined billet assembled in the order of steel plate / titanium plate / nickel foil / steel plate to obtain a larger size plate, which suppresses the mutual diffusion of iron and titanium atoms; however, the process of this technology is cumbersome, the rolling cycle is long, the plate cools quickly during the process, and the intermetallic compounds such as Ni3Ti that are inevitably generated at the nickel and titanium joints, the final interface bonding strength is only 210MPa, which is expected to be further improved. There is also a technology that discloses a method for preparing a titanium / steel composite plate with vanadium as an intermediate layer. The combined billet assembled in the order of steel plate / titanium plate / vanadium foil / steel plate is hot rolled to obtain a titanium / steel composite plate. After the vanadium intermediate layer is added, the interface bonding strength is improved to a certain extent compared with the nickel intermediate layer. When the heating temperature is 950°C, the interface bonding strength is between 280 and 300 MPa. However, the process flow of this technology is cumbersome, the rolling cycle is long, the plate cools down quickly during the process, and two mixed metal intermetallic compounds of FeV and VC are easily formed at the joint of the steel and vanadium intermediate layers, which deteriorates the joint performance. Therefore, the interface bonding strength of this invention still has room for improvement.

[0005] In view of this, it is necessary to provide a method for preparing a titanium / steel composite plate with high interface bonding strength. Summary of the invention

[0006] Therefore, the present invention provides a titanium / steel composite plate and a preparation method thereof, the main purpose of which is to provide a titanium / steel composite plate with high interface bonding strength and a preparation method thereof.

[0007] In order to solve the above problems, the present invention provides a method for preparing a titanium / steel composite plate, comprising the following steps:

[0008] Assembly: stacking and assembling the steel substrate, nickel foil, chromium foil, vanadium foil and titanium substrate in the order of stacking and assembling to obtain a combined blank;

[0009] Insulation: placing the combined blank in an alloy steel ladle for vacuum packaging, and then performing insulation treatment;

[0010] Forging: Forging the combined billet after heat preservation treatment;

[0011] Post-processing: The forged composite billet is post-processed to obtain a titanium / steel composite plate.

[0012] Furthermore, in the assembling step: the steel substrate and the titanium substrate are respectively a steel plate and a titanium plate;

[0013] Preferably, the steel plate, nickel foil, chromium foil, vanadium foil and titanium plate have the same length and width.

[0014] Furthermore, in the assembly step: the thickness of the nickel foil is 50-100 μm; and / or

[0015] The thickness of the chromium foil is 50-100 μm; and / or

[0016] The thickness of the vanadium foil is 50-100 μm.

[0017] Furthermore, in the assembling step: a release agent is applied to the non-bonding surfaces of the steel plate and the titanium plate respectively;

[0018] Preferably, the thickness of the isolation agent is not less than 100 μm.

[0019] Furthermore, before the assembling step, the method further comprises:

[0020] Surface treatment steps: grinding and polishing the surfaces to be bonded between the titanium plate and the steel plate; polishing the surfaces to be contacted between the nickel foil, the chromium foil and the vanadium foil respectively.

[0021] Furthermore, in the heat preservation step: vacuum electron beam welding is used for vacuum packaging.

[0022] Furthermore, in the heat preservation step: the temperature of the heat preservation treatment is 850° C. to 900° C.; and / or

[0023] The insulation treatment time is 2h to 3h.

[0024] Furthermore, in the forging step: the forging is performed by multi-pass forging; the total deformation of the multi-pass forging is 50% to 60%;

[0025] Preferably, the deformation amount of the first forging during multi-pass forging does not exceed 10%.

[0026] Furthermore, the post-processing steps include fine forging, fine rolling and machining.

[0027] In another aspect, the present invention provides a titanium / steel composite plate, wherein the interface shear strength of the titanium / steel composite plate is ≥370 MPa;

[0028] Preferably, the titanium / steel composite plate is obtained by any of the preparation methods described above.

[0029] The titanium / steel composite plate and the preparation method thereof provided by the present invention have the following beneficial effects:

[0030] 1. The present invention adds a composite intermediate layer of nickel, chromium and vanadium between the steel substrate and the titanium substrate (interface bonding), and assembles the steel substrate, nickel foil, chromium foil, vanadium foil and titanium substrate in order, thereby suppressing the mutual diffusion of elements such as iron and titanium on the one hand, and preventing the intermediate layer from generating intermetallic compounds with steel and titanium on the other hand, thereby improving the interface bonding strength of the titanium / steel composite plate; wherein nickel and steel, vanadium and titanium have a very high solid solubility, and adding a chromium intermediate layer to the nickel intermediate layer and the vanadium intermediate layer can not only well prevent nickel and vanadium from generating intermetallic compounds, but also ensure that the composite intermediate layers are mutually solid-dissolved, thereby, no intermetallic compounds will be formed at the overall joint (interface bonding) of the titanium / steel composite plate, and a very high interface bonding strength can be obtained through solid solution strengthening.

[0031] 2. The present invention achieves strong metallurgical bonding at the titanium-steel metal interface through a forging process. The hot working time of forging is short, so the atomic diffusion during the composite process will not be too intense, thereby avoiding the formation of metal compounds after diffusion, which helps to ensure the interface bonding strength of the composite plate. At the same time, compared with the hot rolling process, there is no need for multiple heating and rolling, the process is environmentally friendly and simple, the bonding time is short, and it can be applied to industrial production and titanium-steel composite needs of various structures and sizes. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] In order to more clearly illustrate the implementation methods of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for the implementation methods or the description of the prior art. The drawings described below are only exemplary, and for ordinary technicians in this field, other implementation drawings can be derived from the provided drawings without creative work.

[0033] Figure 1 1 is a schematic diagram of the sequence of stacking and assembling blanks in an embodiment of the present invention;

[0034] Figure 2 Schematic diagram of the process of placing the stacked blanks into the outer alloy steel ladle in an embodiment of the present invention;

[0035] in: Figure 2 a is a schematic diagram of stacking assembly, Figure 2 b and 2c are schematic diagrams of placing the combined billet in the alloy steel jacket; Figure 2 d is a schematic diagram of the alloy steel ladle after sealing welding;

[0036] Figure 3 is a process flow chart of the preparation of a titanium / steel composite plate in an embodiment of the present invention;

[0037] in: Figure 3 a is a schematic diagram of the surface treatment steps, Figure 3 b is a schematic diagram of the combined billet placed in the alloy steel jacket. Figure 3 c is a schematic diagram of the alloy steel ladle after sealing welding. Figure 3 d is a schematic diagram of the heat preservation treatment steps. Figure 3 e is a schematic diagram of the forging steps. Figure 3 f is a schematic diagram of the heat preservation step for the titanium / steel composite plate forging billet, Figure 3 g is a schematic diagram of the finishing step, Figure 3 h is a schematic diagram of the titanium / steel composite plate obtained after stripping the alloy steel sheath;

[0038] Figure 4 is the interface microstructure of the titanium / steel composite plate prepared in Example 1 of the present invention;

[0039] Figure 5 is the test result of the interfacial compressive shear strength of the titanium / steel composite plate prepared in Example 1 of the present invention;

[0040] Figure 6 is the interfacial compressive shear strength test result of the titanium / steel composite plate prepared in Example 2 of the present invention;

[0041] Figure 7 is the test result of the interfacial compressive shear strength of the titanium / steel composite plate prepared in Example 3 of the present invention;

[0042] Figure 8 is the test result of the interfacial compressive shear strength of the titanium / steel composite plate prepared in Example 4 of the present invention;

[0043] Fig. 9 The interface microstructure of the titanium / steel composite plate prepared in Comparative Example 1 of the present invention;

[0044] Fig.10 This is the interface microstructure of the titanium / steel composite plate prepared in Comparative Example 2 of the present invention;

[0045] Fig.11 This is the interface microstructure of the titanium / steel composite plate prepared in Comparative Example 3 of the present invention;

[0046] Fig.12 is the interface microstructure of the titanium / steel composite plate prepared in Comparative Example 4 of the present invention;

[0047] Markings in the figure: 1 is a steel plate, 2 is a nickel foil, 3 is a chromium foil, 4 is a vanadium foil, and 5 is a titanium plate. DETAILED DESCRIPTION

[0048] In order to more clearly illustrate the implementation methods of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for the implementation methods or the description of the prior art. The drawings described below are only exemplary, and for ordinary technicians in this field, other implementation drawings can be derived from the provided drawings without creative work.

[0049] The present invention provides a method for preparing a titanium / steel composite plate with a nickel-chromium-vanadium composite intermediate layer. By designing the intermediate layer, the generation or introduction of new intermetallic compounds at the joint (interface bonding) of the titanium / steel composite plate is avoided, so as to further improve the interface bonding performance of the titanium / steel composite plate. The specific scheme is as follows:

[0050] A method for preparing a titanium / steel composite plate comprises the following steps:

[0051] Assembly: stacking and assembling the steel substrate, nickel foil, chromium foil, vanadium foil and titanium substrate in the order of stacking and assembling to obtain a combined blank;

[0052] Insulation: Place the combined blanks in an alloy steel ladle for vacuum packaging, and then perform insulation treatment;

[0053] Forging: Forging the combined billet after heat preservation treatment;

[0054] Post-processing: The forged composite billet is post-processed to obtain a titanium / steel composite plate.

[0055] Based on the above method, by adding a composite intermediate layer of nickel, chromium and vanadium between the steel substrate and the titanium substrate, and assembling the blanks in the order of steel substrate, nickel foil, chromium foil, vanadium foil and titanium substrate, on the one hand, the mutual diffusion of elements such as iron and titanium is suppressed, and on the other hand, the intermediate layer is prevented from producing intermetallic compounds with steel and titanium, thereby improving the interface bonding strength of the titanium / steel composite plate.

[0056] In the above method, the nickel foil, chromium foil and vanadium foil are respectively made of three pure metal foils of nickel, chromium and vanadium.

[0057] In some embodiments, in the assembling step: the steel substrate and the titanium substrate are respectively a steel plate and a titanium plate;

[0058] Preferably, the length and width of the steel plate, nickel foil, chromium foil, vanadium foil and titanium plate are the same to facilitate subsequent forging.

[0059] In some embodiments, in the assembly step: the thickness of the nickel foil is 50-100 μm; and / or

[0060] The thickness of the chrome foil is 50-100 μm; and / or

[0061] The thickness of the vanadium foil is 50-100 μm. If the thickness of the middle layer foil is too low, the interdiffusion of Fe and Ti atoms cannot be effectively avoided, and Fe-Ti intermetallic compounds are formed at the interface, thereby deteriorating the interface performance; when the thickness of the middle layer foil is too high, the failure crack is easy to extend along the foil, resulting in low performance at the interface.

[0062] In some embodiments, in the assembling step: a release agent is applied to the non-bonding surfaces of the steel plate and the titanium plate respectively;

[0063] Preferably, the thickness of the release agent is not less than 100 μm.

[0064] In some embodiments, before the assembling step, the method further comprises:

[0065] Surface treatment steps: Use an angle grinder to grind and polish the surfaces to be bonded between the titanium plate and the steel plate to remove dirt and oxide layers, then use the organic solvent acetone to clean the surfaces to be bonded, blow dry and set aside; use a sponge with a small amount of polishing paste to wipe the surfaces to be contacted of the nickel foil, chromium foil and vanadium foil respectively to polish the surfaces to be contacted of the nickel foil, chromium foil and vanadium foil, then use ethanol to clean the surface to be contacted of the middle layer, blow dry and set aside.

[0066] In some embodiments, vacuum electron beam welding is used for vacuum packaging. Vacuum packaging ensures that the connection is in a vacuum state during the forging process, prevents oxidation of the titanium and steel surfaces at high temperatures during the connection process, and thus ensures the quality of the titanium-steel bonding. The welding depth during packaging depends on the wall thickness of the alloy steel jacket.

[0067] In some embodiments, in the heat preservation step: the temperature of the heat preservation treatment is 850° C. to 900° C.; and / or

[0068] The insulation treatment time is 2h to 3h.

[0069] In some embodiments, in the forging step: the forging is performed by multi-pass forging; the total deformation of the multi-pass forging is 50% to 60%;

[0070] Preferably, the deformation amount of the first forging during multi-pass forging does not exceed 10%.

[0071] In some embodiments, the post-processing step includes sequentially performing fine forging, fine rolling and machining. The dimensional accuracy of the titanium / steel composite plate is improved by fine forging and fine rolling to obtain a titanium / steel composite plate with dimensions that meet specific requirements; and the outer alloy steel sheath is peeled off by machining.

[0072] In another aspect, the present invention provides a titanium / steel composite plate, wherein the interface shear strength of the titanium / steel composite plate is ≥370 MPa;

[0073] Preferably, the titanium / steel composite plate is obtained by any of the above-mentioned preparation methods.

[0074] The steel substrate and titanium substrate of the embodiment and the comparative example of the present invention are respectively made of steel plate and titanium plate.

[0075] The present invention is further described below in conjunction with specific examples and comparative examples. Figure 3 shown.

[0076] Example 1

[0077] This embodiment provides a method for preparing a titanium / steel composite plate, wherein the steel plate is 10CrNiCu microalloy steel with a size of 100×75×30 mm, the titanium plate is TA3 commercial pure titanium with a size of 100×75×20 mm, and the middle layer is three pure metal foils of nickel foil, chromium foil and vanadium foil, and the sizes of the three pure metal foils are all 100×75×0.05 mm;

[0078] The specific steps include:

[0079] Assembly: Use an angle grinder to grind the surfaces of the steel plate and titanium plate to remove dirt and oxide layer, then use organic solvent acetone to clean and dry the surfaces, then use a sponge with a small amount of polishing paste to scrub the upper and lower surfaces of the nickel foil, chromium foil, and vanadium foil, then rinse the surfaces of the three foils with ethanol and blow dry (such as Figure 3 a);

[0080] Then, the steel plate, nickel foil, chromium foil, vanadium foil and titanium plate are stacked in the order of Figure 1 As shown), a combined blank is obtained, and a release agent is applied to the non-bonding surfaces of the steel plate and the titanium plate (i.e., the top surface of the steel plate and the bottom surface of the titanium plate);

[0081] Insulation: After spraying the isolation agent on the inner side of the alloy steel ladle with a size of 120×95×70mm and a wall thickness of 10mm, put the combined billet into the alloy steel ladle (such as Figure 2 Then, a vacuum electron beam welder is used to seal the interface of the alloy steel jacket in a vacuum chamber. After sealing, the combined blank is placed in a heating furnace for heat preservation treatment (as shown in FIG. Figure 3 b);

[0082] When the vacuum degree in the vacuum chamber reaches 1×10 -2 Pa, welding (sealing) was started, the welding depth was 10 mm, the insulation temperature was 900 ° C, and the insulation time was 2 h (such as Figure 3 c and 3d);

[0083] Forging: Place the combined billet after heat preservation treatment on the operating platform of the forging press, and perform multiple forging deformation along the height direction of the combined billet, with a total deformation of 50% to 60%; among them, the deformation of the first forging does not exceed 10%. After five forgings, a titanium / steel composite plate forging billet with a total downward pressure (total deformation) of 50% is obtained, and air-cooled to room temperature (such as Figure 3 e);

[0084] Post-treatment: After the titanium / steel composite plate forging billet is kept warm, it is successively subjected to fine forging and fine rolling (such as Figure 3 g); the alloy steel sleeve is peeled off by machining to obtain a titanium / steel composite plate (as shown in Figure 3 h).

[0085] The interface microstructure of the titanium / steel composite plate prepared in this embodiment is as follows: Figure 4 As shown in the figure, it can be seen that no obvious intermetallic compounds and holes were found at the joints of the steel plate and the titanium plate, achieving excellent interface metallurgical bonding. Samples were taken for bonding strength testing, and the shear test curve is shown in Figure 5 As shown, it can be seen that the interface bonding strength of the titanium / steel composite plate of this embodiment is 456 MPa.

[0086] Example 2

[0087] This embodiment provides a method for preparing a titanium / steel composite plate, wherein the steel plate is 10CrNiCu microalloy steel with a size of 100×75×30 mm, the titanium plate is TA3 commercial pure titanium with a size of 100×75×20 mm, and the middle layer is three pure metal foils of nickel foil, chromium foil and vanadium foil, and the sizes of the three pure metal foils are all 100×75×0.05 mm;

[0088] The specific steps include:

[0089] Assembly: Use an angle grinder to grind the surfaces of the steel plate and titanium plate to remove dirt and oxide layer, then use organic solvent acetone to clean and dry the surfaces, then use a sponge with a small amount of polishing paste to scrub the upper and lower surfaces of the nickel foil, chromium foil, and vanadium foil, then rinse the surfaces of the three foils with ethanol and blow dry (such as Figure 3 a);

[0090] Then, the steel plate, nickel foil, chromium foil, vanadium foil and titanium plate are stacked in the order of Figure 1 As shown), a combined blank is obtained, and a release agent is applied to the non-bonding surfaces of the steel plate and the titanium plate (i.e., the top surface of the steel plate and the bottom surface of the titanium plate);

[0091] Insulation: After spraying the isolation agent on the inner side of the alloy steel ladle with a size of 120×95×70mm and a wall thickness of 10mm, put the combined billet into the alloy steel ladle (such as Figure 2 Then, a vacuum electron beam welder is used to seal the interface of the alloy steel jacket in a vacuum chamber. After sealing, the combined blank is placed in a heating furnace for heat preservation treatment (as shown in FIG. Figure 3 b);

[0092] When the vacuum degree in the vacuum chamber reaches 1×10 -2 Pa, welding (sealing) was started, the welding depth was 10 mm, the insulation temperature was 900 ° C, and the insulation time was 3 h (such as Figure 3c and 3d);

[0093] Forging: Place the combined billet after heat preservation treatment on the operating platform of the forging press, and perform multiple forging deformation along the height direction of the combined billet, with a total deformation of 50% to 60%; among them, the deformation of the first forging does not exceed 10%. After five forgings, a titanium / steel composite plate forging billet with a total downward pressure (total deformation) of 50% is obtained, and air-cooled to room temperature (such as Figure 3 e);

[0094] Post-treatment: After the titanium / steel composite plate forging billet is kept warm, it is successively subjected to fine forging and fine rolling (such as Figure 3 g); the alloy steel sleeve is peeled off by machining to obtain a titanium / steel composite plate (as shown in Figure 3 h).

[0095] Samples were taken for bonding strength test, and the shear test curve was as follows: Figure 6 As shown, it can be seen that the interface bonding strength of the titanium / steel composite plate of this embodiment is 407 MPa.

[0096] Example 3

[0097] This embodiment provides a method for preparing a titanium / steel composite plate, wherein the steel plate is 10CrNiCu microalloy steel with a size of 100×75×30 mm, the titanium plate is TA3 commercial pure titanium with a size of 100×75×20 mm, and the middle layer is three pure metal foils of nickel foil, chromium foil and vanadium foil, and the sizes of the three pure metal foils are all 100×75×0.05 mm;

[0098] The specific steps include:

[0099] Assembly: Use an angle grinder to grind the surfaces of the steel plate and titanium plate to remove dirt and oxide layer, then use organic solvent acetone to clean and dry the surfaces, then use a sponge with a small amount of polishing paste to scrub the upper and lower surfaces of the nickel foil, chromium foil, and vanadium foil, then rinse the surfaces of the three foils with ethanol and blow dry (such as Figure 3 a);

[0100] Then, the steel plate, nickel foil, chromium foil, vanadium foil and titanium plate are stacked in the order of Figure 1 As shown), a combined blank is obtained, and a release agent is applied to the non-bonding surfaces of the steel plate and the titanium plate (i.e., the top surface of the steel plate and the bottom surface of the titanium plate);

[0101] Insulation: After spraying the isolation agent on the inner side of the alloy steel ladle with a size of 120×95×70mm and a wall thickness of 10mm, put the combined billet into the alloy steel ladle (such as Figure 2Then, a vacuum electron beam welder is used to seal the interface of the alloy steel jacket in a vacuum chamber. After sealing, the combined blank is placed in a heating furnace for heat preservation treatment (as shown in FIG. Figure 3 b);

[0102] When the vacuum degree in the vacuum chamber reaches 1×10 -2 Pa, welding (sealing) was started, the welding depth was 10mm, the insulation temperature was 850℃, and the insulation time was 2h (such as Figure 3 c and 3d);

[0103] Forging: Place the combined billet after heat preservation treatment on the operating platform of the forging press, and perform multiple forging deformation along the height direction of the combined billet, with a total deformation of 50% to 60%; among them, the deformation of the first forging does not exceed 10%. After five forgings, a titanium / steel composite plate forging billet with a total downward pressure (total deformation) of 50% is obtained, and air-cooled to room temperature (such as Figure 3 e);

[0104] Post-treatment: After the titanium / steel composite plate forging billet is kept warm, it is successively subjected to fine forging and fine rolling (such as Figure 3 g); the alloy steel sleeve is peeled off by machining to obtain a titanium / steel composite plate (as shown in Figure 3 h).

[0105] Samples were taken for bonding strength test, and the shear test curve was as follows: Figure 7 As shown, it can be seen that the interface bonding strength of the titanium / steel composite plate of this embodiment is 390 MPa.

[0106] Combining Examples 1 to 3, it can be seen that after adding the nickel-chromium-vanadium composite intermediate layer, the forging process parameters can obtain titanium-steel composite plates with good performance within a certain range. The difference lies in the insulation temperature and insulation time before forging. The microstructure of the connection interface obtained is not significantly different, and only the results obtained in the shear test are slightly different. When the insulation temperature is in the range of 850℃ to 900℃, the insulation time is 2h, and other parameters remain unchanged, the strength of the titanium-steel composite plate obtained is 390MPa to 407MPa; when the insulation time is 2h to 3h, the insulation temperature is 900℃, and other parameters remain unchanged, the strength of the titanium-steel composite plate obtained is 456MPa to 407MPa. The results obtained beyond this parameter range will be reduced to a certain extent.

[0107] Example 4

[0108] This embodiment provides a method for preparing a titanium / steel composite plate, wherein the steel plate is 10CrNiCu microalloy steel with a size of 100×75×30 mm, the titanium plate is TA3 commercial pure titanium with a size of 100×75×20 mm, and the middle layer is three pure metal foils of nickel foil, chromium foil and vanadium foil, and the sizes of the three pure metal foils are all 100×75×0.1 mm;

[0109] The specific steps include:

[0110] Assembly: Use an angle grinder to grind the surfaces of the steel plate and titanium plate to remove dirt and oxide layer, then use organic solvent acetone to clean and dry the surfaces, then use a sponge with a small amount of polishing paste to scrub the upper and lower surfaces of the nickel foil, chromium foil, and vanadium foil, then rinse the surfaces of the three foils with ethanol and blow dry (such as Figure 3 a);

[0111] Then, the steel plate, nickel foil, chromium foil, vanadium foil and titanium plate are stacked in the order of Figure 1 As shown), a combined blank is obtained, and a release agent is applied to the non-bonding surfaces of the steel plate and the titanium plate (i.e., the top surface of the steel plate and the bottom surface of the titanium plate);

[0112] Insulation: After spraying the isolation agent on the inner side of the alloy steel ladle with a size of 120×95×70mm and a wall thickness of 10mm, put the combined billet into the alloy steel ladle (such as Figure 2 Then, a vacuum electron beam welder is used to seal the interface of the alloy steel jacket in a vacuum chamber. After sealing, the combined blank is placed in a heating furnace for heat preservation treatment (as shown in FIG. Figure 3 b);

[0113] When the vacuum degree in the vacuum chamber reaches 1×10 -2 Pa, welding (sealing) was started, the welding depth was 10 mm, the insulation temperature was 900 ° C, and the insulation time was 2 h (such as Figure 3 c and 3d);

[0114] Forging: Place the combined billet after heat preservation treatment on the operating platform of the forging press, and perform multiple forging deformation along the height direction of the combined billet, with a total deformation of 50% to 60%; among which, the deformation of the first forging does not exceed 10%. After five forgings, a titanium / steel composite plate forging billet with a total downward pressure (total deformation) of 55% is obtained, and air-cooled to room temperature (such as Figure 3 e);

[0115] Post-treatment: After the titanium / steel composite plate forging billet is kept warm, it is successively subjected to fine forging and fine rolling (such as Figure 3 g); the alloy steel sleeve is peeled off by machining to obtain a titanium / steel composite plate (as shown in Figure 3 h).

[0116] The interface bonding strength of the titanium / steel composite plate of this embodiment was measured to be 371 MPa.

[0117] Comparative Example 1

[0118] This comparative example provides a method for preparing a titanium / steel composite plate, wherein the steel plate is made of 10CrNiCu microalloy steel with a size of 100×75×30 mm, the titanium plate is made of TA3 commercial pure titanium with a size of 100×75×20 mm, and the middle layer is made of nickel foil with a size of 100×75×0.05 mm;

[0119] The specific steps include:

[0120] Assembly: Use an angle grinder to grind the surfaces of the steel plate and titanium plate to remove dirt and oxide layers, then use an organic solvent, acetone, to clean and dry the surfaces, then use a sponge with a small amount of polishing paste to scrub the upper and lower surfaces of the nickel foil, chromium foil, and vanadium foil, then rinse the surfaces of the three foils with ethanol and blow dry;

[0121] Then, the steel plate, the nickel foil, and the titanium plate are stacked and assembled in the order to obtain a combined blank, and a release agent is applied on the non-bonding surfaces of the steel plate and the titanium plate (i.e., the top surface of the steel plate and the bottom surface of the titanium plate);

[0122] Insulation: After spraying an isolation agent on the inner side of an alloy steel ladle with a size of 120×95×70mm and a wall thickness of 10mm, the combined blank is placed in the alloy steel ladle; then a vacuum electron beam welder is used to seal the interface of the alloy steel ladle in a vacuum chamber, and after sealing, the combined blank is placed in a heating furnace for insulation treatment;

[0123] When the vacuum degree in the vacuum chamber reaches 1×10 -2 Welding started at 1000 Pa, welding depth was 10 mm, insulation temperature was 900 °C, insulation time was 2 h;

[0124] Forging: placing the combined billet after heat preservation treatment on the operating platform of the forging press, and performing multiple forging deformations along the height direction of the combined billet, with a total deformation of 50% to 60%; wherein, the deformation of the first forging does not exceed 10%, and after five forgings, a titanium / steel composite plate forging billet with a total reduction of 50% is obtained, and air-cooled to room temperature;

[0125] Post-processing: After the titanium / steel composite plate forging billet is kept warm, fine forging and fine rolling are performed in sequence; the alloy steel sheath is stripped off through fine forging and fine rolling to obtain the titanium / steel composite plate.

[0126] The interface microstructure of the titanium / steel composite plate prepared in this comparative example is as follows: Figure 8As shown, it can be seen that an obvious intermetallic compound region appears at the joint of the steel plate and the titanium plate. The interface bonding strength of the titanium / steel composite plate prepared in this comparative example is 253 MPa.

[0127] Comparative Example 2

[0128] This comparative example provides a method for preparing a titanium / steel composite plate, wherein the steel plate is made of 10CrNiCu microalloy steel with a size of 100×75×30 mm, the titanium plate is made of TA3 commercial pure titanium with a size of 100×75×20 mm, and the middle layer is made of nickel foil and vanadium foil with a size of 100×75×0.075 mm;

[0129] The specific steps include:

[0130] Assembly: Use an angle grinder to grind the surfaces of the steel plate and titanium plate to remove dirt and oxide layers, then use an organic solvent, acetone, to clean and dry the surfaces, then use a sponge with a small amount of polishing paste to scrub the upper and lower surfaces of the nickel foil, chromium foil, and vanadium foil, then rinse the surfaces of the three foils with ethanol and blow dry;

[0131] Then, the steel plate, nickel foil, vanadium foil and titanium plate are stacked and assembled in the order to obtain a combined blank, and a release agent is applied on the non-bonding surfaces of the steel plate and the titanium plate (i.e., the top surface of the steel plate and the bottom surface of the titanium plate);

[0132] Insulation: After spraying an isolation agent on the inner side of an alloy steel ladle with a size of 120×95×70mm and a wall thickness of 10mm, the combined blank is placed in the alloy steel ladle; then a vacuum electron beam welder is used to seal the interface of the alloy steel ladle in a vacuum chamber, and after sealing, the combined blank is placed in a heating furnace for insulation treatment;

[0133] When the vacuum degree in the vacuum chamber reaches 1×10 -2 Welding started at 1000 Pa, welding depth was 10 mm, insulation temperature was 900 °C, insulation time was 2 h;

[0134] Forging: placing the combined billet after heat preservation treatment on the operating platform of the forging press, and performing multiple forging deformations along the height direction of the combined billet, with a total deformation of 50% to 60%; wherein, the deformation of the first forging does not exceed 10%, and after five forgings, a titanium / steel composite plate forging billet with a total reduction of 50% is obtained, and air-cooled to room temperature;

[0135] Post-processing: After the titanium / steel composite plate forging billet is kept warm, fine forging and fine rolling are performed in sequence; the alloy steel sheath is stripped off through fine forging and fine rolling to obtain the titanium / steel composite plate.

[0136] The interface microstructure of the titanium / steel composite plate prepared in this comparative example is as follows: Fig. 9As shown, it can be seen that an obvious intermetallic compound region appears at the joint of the steel plate and the titanium plate. The interface bonding strength of the titanium / steel composite plate prepared in this comparative example is 299 MPa.

[0137] Comparative Example 3

[0138] This comparative example provides a method for preparing a titanium / steel composite plate, wherein the steel plate is made of 10CrNiCu microalloy steel with a size of 100×75×30 mm, the titanium plate is made of TA3 commercial pure titanium with a size of 100×75×20 mm, and the middle layer is made of chromium foil and vanadium foil with a size of 100×75×0.075 mm;

[0139] The specific steps include:

[0140] Assembly: Use an angle grinder to grind the surfaces of the steel plate and titanium plate to remove dirt and oxide layers, then use an organic solvent, acetone, to clean and dry the surfaces, then use a sponge with a small amount of polishing paste to scrub the upper and lower surfaces of the nickel foil, chromium foil, and vanadium foil, then rinse the surfaces of the three foils with ethanol and blow dry;

[0141] Then, the steel plate, chromium foil, vanadium foil and titanium plate are stacked and assembled in the order to obtain a combined blank, and a release agent is applied on the non-bonding surfaces of the steel plate and the titanium plate (i.e., the top surface of the steel plate and the bottom surface of the titanium plate);

[0142] Insulation: After spraying an isolation agent on the inner side of an alloy steel ladle with a size of 120×95×70mm and a wall thickness of 10mm, the combined blank is placed in the alloy steel ladle; then a vacuum electron beam welder is used to seal the interface of the alloy steel ladle in a vacuum chamber, and after sealing, the combined blank is placed in a heating furnace for insulation treatment;

[0143] When the vacuum degree in the vacuum chamber reaches 1×10 -2 Welding started at 1000 Pa, welding depth was 10 mm, insulation temperature was 900 °C, insulation time was 2 h;

[0144] Forging: placing the combined billet after heat preservation treatment on the operating platform of the forging press, and performing multiple forging deformations along the height direction of the combined billet, with a total deformation of 50% to 60%; wherein, the deformation of the first forging does not exceed 10%, and after five forgings, a titanium / steel composite plate forging billet with a total reduction of 50% is obtained, and air-cooled to room temperature;

[0145] Post-processing: After the titanium / steel composite plate forging billet is kept warm, fine forging and fine rolling are performed in sequence; the alloy steel sheath is stripped off through fine forging and fine rolling to obtain the titanium / steel composite plate.

[0146] The interface microstructure of the titanium / steel composite plate prepared in this comparative example is as follows: Fig.10As shown, it can be seen that an obvious intermetallic compound region appears at the joint of the steel plate and the titanium plate. The interface bonding strength of the titanium / steel composite plate prepared in this comparative example is 327 MPa.

[0147] Combining Example 1 and Comparative Examples 1 to 3, it can be seen that the performance of the titanium / steel composite plate prepared with a nickel-chromium-vanadium composite intermediate layer is better than that of the titanium / steel composite plate obtained by combining any one or two intermediate layers. This is because only a single intermediate layer or a combination of two intermediate layers cannot guarantee that no intermetallic compounds will be generated at the connection joint, and such intermetallic compounds will deteriorate the joint performance to a certain extent. When the billet is assembled in the order of steel plate / nickel foil / chromium foil / vanadium foil / titanium plate and then forged, it can be ensured that no intermetallic compounds are generated at the joint, and the effect of strengthening the joint can be achieved in the form of elemental solid solution between the several materials.

[0148] Comparative Example 4

[0149] This comparative example provides a method for preparing a titanium / steel composite plate, wherein the steel plate is made of 10CrNiCu microalloy steel with a size of 100×75×30 mm, the titanium plate is made of TA3 commercial pure titanium with a size of 100×75×20 mm, and the middle layer is made of nickel foil with a size of 100×75×0.05 mm;

[0150] The specific steps include:

[0151] Assembly: Use an angle grinder to grind the surfaces of the steel plate and titanium plate to remove dirt and oxide layers, then use an organic solvent, acetone, to clean and dry the surfaces, then use a sponge with a small amount of polishing paste to scrub the upper and lower surfaces of the nickel foil, chromium foil, and vanadium foil, then rinse the surfaces of the three foils with ethanol and blow dry;

[0152] Then, the steel plate, nickel foil, chromium foil, vanadium foil and titanium plate are stacked and assembled in the order to obtain a combined blank, and a release agent is applied on the non-bonding surfaces of the steel plate and the titanium plate (i.e., the top surface of the steel plate and the bottom surface of the titanium plate);

[0153] Insulation: After spraying an isolation agent on the inner side of an alloy steel ladle with a size of 120×95×70mm and a wall thickness of 10mm, the combined blank is placed in the alloy steel ladle; then a vacuum electron beam welder is used to seal the interface of the alloy steel ladle in a vacuum chamber, and after sealing, the combined blank is placed in a heating furnace for insulation treatment;

[0154] When the vacuum degree in the vacuum chamber reaches 1×10 -2 Welding started at 1000 Pa, welding depth was 10 mm, insulation temperature was 900 °C, insulation time was 2 h;

[0155] Forging: placing the combined billet after heat preservation treatment on the operating platform of the forging press, and performing multiple forging deformation along the height direction of the combined billet, with a total deformation of 30%; wherein, the deformation of the first forging does not exceed 10%, and after three forgings, a titanium / steel composite plate forging billet with a total reduction of 30% is obtained, and air-cooled to room temperature;

[0156] Post-processing: After the titanium / steel composite plate forging billet is kept warm, fine forging and fine rolling are performed in sequence; the alloy steel sheath is stripped off through fine forging and fine rolling to obtain the titanium / steel composite plate.

[0157] The interface microstructure of the titanium / steel composite plate prepared in this comparative example is as follows: Fig.11 As shown, it can be seen that a large number of interface holes appear at the joint of the steel plate and the titanium plate. The interface bonding strength of the titanium / steel composite plate prepared in this comparative example is 292 MPa.

[0158] Combining Example 1 and Comparative Example 4, it can be seen that the performance of the titanium / steel composite plate prepared with a deformation of 50% is better than that of the titanium / steel composite plate obtained with a deformation of 30%. This is because a larger deformation can ensure that after forging is completed, the holes on the various interfaces at the joints are completely healed, and the performance is higher. If there are a large number of holes, the titanium / steel composite plate will crack at the locations of these holes during service, causing failure. It can be found that when the deformation reaches 50%, there are no obvious holes on each interface. However, at the same time, since the forging temperature is 850-900°C, the material deformation resistance is low in this temperature range. If the deformation is too large, the slab itself will crack, and the resulting composite plate will be unqualified. Considering all factors, the total deformation during forging is 50% to 60%, which is the best.

[0159] It is easy for those skilled in the art to understand that, without conflict, the advantageous technical features of the above-mentioned methods can be freely combined and superimposed.

[0160] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principle of the present invention shall be included in the protection scope of the present invention. The above description is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and variations can be made without departing from the technical principles of the present invention. These improvements and variations should also be regarded as the protection scope of the present invention.

Claims

1. A method for preparing a titanium / steel composite plate, characterized in that: The following steps are involved: Assembly: stacking and assembling the steel substrate, nickel foil, chromium foil, vanadium foil and titanium substrate in the order of stacking and assembling to obtain a combined blank; Insulation: placing the combined blank in an alloy steel ladle for vacuum packaging, and then performing insulation treatment; Forging: Forging the combined billet after heat preservation treatment; Post-processing: The forged composite billet is post-processed to obtain a titanium / steel composite plate.

2. The method for preparing a titanium / steel composite plate according to claim 1, characterized in that: In the assembling step: the steel substrate and the titanium substrate are respectively a steel plate and a titanium plate; Preferably, the steel plate, nickel foil, chromium foil, vanadium foil and titanium plate have the same length and width.

3. The method for preparing a titanium / steel composite plate according to claim 1 or 2, characterized in that: In the assembly step: the thickness of the nickel foil is 50-100 μm; and / or The thickness of the chromium foil is 50-100 μm; and / or The thickness of the vanadium foil is 50-100 μm.

4. The method for preparing a titanium / steel composite plate according to claim 2, characterized in that: In the assembling step: coating the non-bonding surfaces of the steel plate and the titanium plate with a release agent respectively; Preferably, the thickness of the isolation agent is not less than 100 μm.

5. The method for preparing a titanium / steel composite plate according to claim 2, characterized in that: Before the assembling step, the method further comprises: Surface treatment steps: grinding and polishing the surfaces to be bonded between the titanium plate and the steel plate; polishing the surfaces to be contacted between the nickel foil, the chromium foil and the vanadium foil respectively.

6. The method for preparing a titanium / steel composite plate according to claim 1, characterized in that: In the heat preservation step: vacuum packaging is performed by vacuum electron beam welding.

7. The method for preparing a titanium / steel composite plate according to claim 1, characterized in that: In the heat preservation step: the temperature of the heat preservation treatment is 850° C. to 900° C.; and / or The insulation treatment time is 2h to 3h.

8. The method for preparing a titanium / steel composite plate according to claim 7, characterized in that: In the forging step: the forging is performed by multi-pass forging; the total deformation of the multi-pass forging is 50% to 60%; Preferably, the deformation amount of the first forging during multi-pass forging does not exceed 10%.

9. The method for preparing a titanium / steel composite plate according to claim 1, characterized in that: The post-processing steps include finish forging, finish rolling and machining.

10. A titanium / steel composite plate, characterized in that: The interface shear strength of the titanium / steel composite plate is ≥390MPa; Preferably, the titanium / steel composite plate is obtained by the preparation method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Method for high-temperature rolling of titanium steel composite board with nickel as interlayer

    CN104826866A

  • Preparation method of titanium-steel composite board with vanadium as interlayer

    CN106040741A

  • Preparation method of titanium-steel composite plate with IF steel as interlayer

    CN108393653A

  • Titanium steel composite board manufacturing method

    CN109127729A

  • Heterogeneous metal laminated composite armor and preparation method thereof

    CN116336870A