Forming method of steel casting sand core
By using sand core prepared by corundum sand and water-based binder, combined with mold crumbing technology of furan resin curing agent, the problem of sand bonding and core bone bonding of small sand cores during casting is solved, and the cast steel parts are improved Quality and efficiency.
Patent Information
- Application Number
- CN202411013964.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-12
AI Technical Summary
During the casting of steel parts, small sand cores are severely bonded due to poor heat transfer, and core bone bonding problems are prominent, which increases the difficulty of cleaning and production cycle.
The sand core is prepared by mixing corundum sand with water-based binder. The mold is made of furan resin curing agent and crumbles after baking at high temperature to form a sand core without cores to ensure the anti-sanding ability and strength of the sand core. .
It effectively solves the problem of sand sticking, improves the quality and performance of cast steel parts, simplifies the subsequent cleaning process, and shortens the production cycle.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of casting and provides a method for forming a sand core of a steel casting. Background Art
[0002] Sand casting is a widely used manufacturing process in the foundry industry. Currently, chromium ore sand is the dominant material in the production of sand cores using resin sand. This type of sand has a higher refractoriness and thermal conductivity, so it is better than silica sand in terms of anti-sticking performance.
[0003] However, when casting steel parts, the performance of chrome ore sand has certain limitations for some small sand cores. This is because, due to the small size of the sand core, the chrome ore sand cannot effectively transfer heat, causing the sand to sinter and bond severely to the surface of the casting, making it difficult to clean. In addition, due to the small size of the sand core, the bonding problem of the core bone is also more prominent, which not only increases the difficulty of subsequent cleaning, but also has an adverse effect on the production cycle. In order to alleviate this problem, reduce the difficulty of subsequent cleaning, and shorten the production cycle, a more effective coreless molding method is urgently needed. Summary of the invention
[0004] In order to overcome the defects in the prior art, the present invention provides a method for forming a sand core for a steel casting. The sand core does not require a core bone when preparing the sand core, and has a strong ability to resist sintering and sand sticking. During the forming process of the sand core, the mold is made of a sand mold, and after baking, it collapses to form a sand core for the steel casting, and the sand core has a good ability to resist sand sticking. This can effectively solve the problem of sand sticking and further improve the quality and performance of steel castings.
[0005] A method for molding a sand core for a steel casting, the molding method comprising the following steps:
[0006] Make a mold by mixing molding sand with resin curing agent to prepare the mold;
[0007] Mould surface treatment and process information preparation;
[0008] Making a sand core: using corundum sand and water-based binder mixed sand to fill the mold cavity to prepare the sand core, forming a combination of the mold and the sand core;
[0009] The combination of the mold and the sand core is baked, and the sand core is formed after the mold collapses.
[0010] In one embodiment, in the step of "making sand core", the water-based binder is an inorganic water glass resin, so that it still has high strength after high-temperature baking.
[0011] In one embodiment, the liquid-to-material ratio of the inorganic water glass resin is: the proportion of water glass resin to corundum sand is 3% to 5%, and the proportion of water glass curing agent to resin is 15% to 20%; the liquid-to-material ratio control can ensure that the sand core has suitable strength after preparation and baking, and can also ensure that the strength after boxing is not too high and difficult to clean the sand.
[0012] In one embodiment, in the step of "making sand core", the aluminum content in the corundum sand is more than 90%; and preferably, the Al2O3 content in the corundum sand is more than 98%, so that the sand core has better high temperature resistance.
[0013] In one of the embodiments, in the step of "making sand cores", the corundum sand is added to the water-based adhesive until the stickiness time is maintained for 15 minutes to 25 minutes, and the hardening time is 7 hours to 9 hours; this can ensure that the sand core can be used for too short a time during use, resulting in sand core stratification, while also avoiding the sand core being difficult to harden due to too long a time of use, resulting in extended unpacking time and the risk of box collapse.
[0014] In one embodiment, in the step of "making a mold", the resin curing agent is a furan resin curing agent; using furan resin to make a mold can cause the mold to collapse after high-temperature baking.
[0015] In one embodiment, the mold is divided into an upper mold and a lower mold. When assembling the mold, a support rod is set in the lower mold, and then the lower mold is assembled to form the mold, and the cavity of the mold is filled with corundum sand and water-based binder mixed sand. After the mixed sand hardens for 7 to 9 hours, the upper mold is removed and discarded, and the sand core and the lower mold are placed in a baking furnace for baking; removing the upper mold is conducive to the escape of water vapor and gas during baking. Since the mold may collapse unevenly during the baking process, resulting in uneven stress on the sand core and fracture, it is necessary to add support rods to the mold to prevent the sand core from tipping over after the mold collapses.
[0016] In one of the embodiments, the temperature in the furnace before baking is less than 100°C. During baking, the heating rate is 30°C / h to 80°C / h, the baking temperature is between 400°C and 500°C, the insulation time is 7.5h to 8.5h, the cooling rate is 50°C / h to 100°C / h, and the mold is taken out after cooling to below 200°C and cooled in a wind-proof manner. The baking process enhances the strength of the sand core and completely collapses the mold.
[0017] The molding method of steel castings provided by the present invention aims to solve the problems of sand sticking and core bone bonding in the casting process of small and medium-sized sand cores in the prior art, thereby improving the efficiency and quality of the entire casting process. A reasonable sand mixing scheme is adopted to separately make the sand core and the mold, which ensures the strength of the sand core and is also conducive to the collapse of the mold during the baking process to achieve the purpose of molding. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] none DETAILED DESCRIPTION
[0019] In order to facilitate the understanding of the present invention, the present invention will be described more fully below, and preferred embodiments of the present invention are given. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. The purpose of providing these embodiments is to make the disclosure of the present invention more thoroughly and comprehensively understood.
[0020] This embodiment mainly provides a method for forming a sand core of a steel casting, and particularly relates to a method for forming a sand core of an annular steel casting. The steps of the forming method specifically include:
[0021] Step 1: Make the mold. Design a special sand core mold according to the complexity of the steel casting. Use molding sand and resin curing agent to mix the mold, that is, the mold is a sand mold. The resin curing agent uses furan resin curing agent. After high-temperature baking, the sand mold collapses and the sand core can be completely exposed, avoiding the problem of removing the sand core before baking and the difficulty of baking the mold.
[0022] Specifically, the mold is made by 3D printing, and furan resin curing agent is used for sand mixing. When designing the mold, the mold is divided into an upper mold and a lower mold, which is convenient for installation and shaping.
[0023] Step 2: Mould surface treatment and process information preparation: Mould surface is treated to ensure that there is no adhesion between the mould and the sand core.
[0024] Specifically, support rods need to be set in the lower half of the mold. Since the mold may collapse unevenly during the baking process, causing the sand core to be unevenly stressed and break, support rods need to be added to the mold to prevent the sand core from tipping over or breaking after the mold collapses.
[0025] Step three, making a sand core, using corundum sand and water-based binder mixed sand to fill the mold cavity to prepare the sand core, forming a combination of the mold and the sand core; in order to ensure that the sand core still has a high strength after high-temperature baking, an inorganic water glass resin is selected as the water-based coagulant.
[0026] Specifically, when designing the liquid-to-material ratio control, in order to ensure that the sand core has appropriate strength after preparation and baking, and at the same time ensure that the sand is easy to clean after boxing, the liquid-to-material ratio of the inorganic water glass resin is: the proportion of water glass resin to corundum sand is 3% to 5%, and the proportion of water glass curing agent to resin is 15% to 20%. The corundum sand is preferably corundum sand with an Al2O3 content of more than 98% and an aluminum content of more than 90%. In the sand mixing process, the corundum sand is added with a water-based binder until the stickiness time is maintained for 15 minutes to 25 minutes, and the hardening time is 7 hours to 9 hours; if the time is too short, the sand core will be delaminated, and if the time is too long, the sand core will be difficult to harden, and it will lead to a prolonged unpacking time and the risk of box collapse. Therefore, the hardening time is selected to be 7 hours to 9 hours, so that better results can be achieved.
[0027] It should be noted that, since the strength of inorganic water glass resin is limited at room temperature, the overall strength is improved after high-temperature baking, and after baking, the gas emission of the sand core is reduced, which can well meet the needs of the site. Therefore, metals such as core bones, cold irons and standard cores are not added in the process to prevent serious breakage of the sand core due to thermal expansion differences. Since the sand core of the steel casting is annular and cannot be supported internally, a core head needs to be set externally to support the sand core to form an internal cavity. After boxing, the cavity at the core head of the steel casting is welded.
[0028] When assembling the mold, a support rod is set in the lower mold, and then the lower mold is assembled to form a mold, and the cavity of the mold is filled with a mixture of corundum sand and water-based binder. After the mixed sand hardens for 7 to 9 hours, the upper mold is removed and discarded, and the sand core and the lower mold are placed in a baking furnace for baking; the upper mold is removed. Since the mold may collapse unevenly during the baking process, resulting in uneven stress on the sand core and fracture, it is necessary to add support rods to the mold to prevent the sand core from tipping over after the mold collapses.
[0029] Furthermore, in order to improve the overall strength of the sand core, it is also necessary to add process tie rods to the sand core; identify them during the sand core design process, add round or square tie rods to the large span, weak or crack-prone parts, combine them with the sand core, fill sand together to form the core, and remove them before lowering the core.
[0030] Step 4: bake the combination of the mold and the sand core, and form a sand core after the mold collapses.
[0031] Specifically, the temperature in the furnace before baking is less than 100°C. During baking, the heating rate is 30°C / h to 80°C / h, the baking temperature is between 400°C and 500°C, the insulation time is 7.5h to 8.5h, the cooling rate is 50°C / h to 100°C / h, and the mold is taken out after cooling to below 200°C and cooled in a wind-proof manner. The baking process enhances the strength of the sand core and completely collapses the mold.
[0032] It should be noted that it is best to remove the upper mold before baking, and place the sand core and the lower mold in a baking oven for baking; this is conducive to the escape of water vapor and gas during baking. The upper mold is discharged, and after the lower mold collapses, the required sand core is taken out, cleaned, and used like other normal sand cores.
[0033] Through this technical solution, a complex sand core with no core bone, high molding sand strength and strong sintering resistance can be formed.
[0034] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0035] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the invention patent. It should be pointed out that for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be based on the attached claims.
Claims
1. Forming of a sand core for steel castings, It is characterized in that The molding method comprises the following steps: Make a mold by mixing molding sand with resin curing agent to prepare the mold; Mould surface treatment and process information preparation; Making a sand core: using corundum sand and water-based binder mixed sand to fill the mold cavity to prepare the sand core, forming a combination of the mold and the sand core; The combination of the mold and the sand core is baked, and the sand core is formed after the mold collapses.
2. The method for forming a steel casting sand core according to claim 1, It is characterized in that In the step of "making sand core", the water-based binder is an inorganic water glass resin.
3. The method for forming a steel casting sand core according to claim 2, It is characterized in that The liquid-to-material ratio of the inorganic water glass resin is as follows: the proportion of the water glass resin to the corundum sand is 3% to 5%, and the proportion of the water glass curing agent to the resin is 15% to 20%.
4. The method for forming a steel casting sand core according to claim 1, It is characterized in that In the step of "making sand core", the aluminum content in the corundum sand is more than 90%.
5. The method for forming a steel casting sand core according to claim 1, It is characterized in that In the step of "making sand cores", the corundum sand is added to the water-based binder and the stickiness time is maintained for 15 minutes to 25 minutes, and the hardening time is 7 hours to 9 hours.
6. The method for forming a steel casting sand core according to claim 1, It is characterized in that In the "making mold" step, the resin curing agent is a furan resin curing agent.
7. The method for forming a steel casting sand core according to claim 1, It is characterized in that The mold is divided into an upper mold and a lower mold. When assembling the mold, a support rod is set in the lower mold, and then the lower mold is combined to form the mold, and a mixed sand of corundum sand and a water-based binder is filled in the cavity of the mold. After the mixed sand hardens, the upper mold is removed, and the sand core and the lower mold are placed in a baking oven for baking.
8. The method for forming a steel casting sand core according to claim 1 or 7, It is characterized in that The temperature in the furnace is less than 100°C before baking. During baking, the heating rate is 30°C / h to 80°C / h, the baking temperature is between 400°C and 500°C, the insulation time is 7.5h to 8.5h, the cooling rate is 50°C / h to 100°C / h, and it is taken out after cooling to below 200°C.