Ultrahigh-barrier high-strength TPEE composite material as well as preparation method and application thereof

By optimizing the polyether content in TPEE materials and combining with high-density polyethylene fibers, combining antistatic agents and hydrophilic agents, the problem of the moisture permeability, strength and hydrostatic pressure of TPEE materials in the protective film field is difficult to increase at the same time. It achieves high strength and high barrier properties, suitable for high risk packaging fields.

CN118927744AActive Publication Date: 2024-11-12GUANGDONG KINGFA TECH CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202310516580.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-09
Publication Date
2024-11-12
Estimated Expiration
2043-05-09

AI Technical Summary

Technical Problem

It is difficult for existing polyester elastomer TPEE materials to achieve the ideal state of high moisture permeability, high strength and high hydrostatic pressure in the field of protective films, resulting in limited applications in high-risk areas such as medical and food packaging.

Method used

By preferring high polyether content on the basis of high moisture permeable TPEE material and composited with high density polyethylene fibers, a modified TPEE composite material is prepared, combining antistatic agents and hydrophilic agents, improving the strength and hygroscopicity of the material, and through heat Adhesive composite technology forms an ultra-high barrier and high strength TPEE composite film.

Benefits of technology

The high moisture permeability, strength and barrier properties of the material have been improved, allowing it to be widely used in the fields of high-risk medical packaging and food packaging, and has good economic and performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses an ultrahigh-barrier high-strength TPEE composite material as well as a preparation method and application thereof. The composite material is composed of a modified TPEE elastomer and high-density polyethylene, and the modified TPEE elastomer is prepared from the following components in parts by weight: 50 parts of TPEE resin, 2-4 parts of an antistatic agent and 1-3 parts of a hydrophilic agent; the polyether content of the TPEE elastomer is 10 to 20 weight percent; the weight-average molecular weight of the high-density polyethylene is 20,000-400,000. The TPEE material with higher polyether addition amount is preferably selected on the basis of the existing high-moisture-permeability TPEE material, and is compounded with the high-density polyethylene fiber, so that the TPEE composite film has better strength and moisture permeability, and the TPEE film prepared from the material has good barrier property and better moisture absorption, and can be used for preparing the high-moisture-permeability TPEE film. The packaging box is suitable for the fields of higher-grade medical packaging and high-grade food packaging.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of polyester elastomer TPEE materials, and in particular to an ultra-high barrier high-strength TPEE composite material and a preparation method and application thereof. Background Art

[0002] Polyether ester (TPEE) is a thermoplastic elastomer of polybutylene terephthalate-polyethylene oxide-polypropylene oxide, which is a block copolymer obtained by co-condensation of dimethyl terephthalate, butanediol, polyethylene oxide glycol and / or polypropylene oxide glycol, and has good flexibility and mechanical properties. TPEE materials have good mechanical properties and processing properties and are widely used in membrane materials. However, the moisture permeability, strength and hydrostatic pressure of protective film materials cannot reach the ideal state at the same time. Therefore, there is an urgent need for a protective film material with high moisture permeability, high strength and high hydrostatic pressure. Summary of the invention

[0003] In view of the defects in the prior art, the present invention proposes an ultra-high barrier and high-strength TPEE composite material, a preparation method and application thereof, by preferably selecting a TPEE material with a higher polyether addition amount on the basis of the existing high moisture permeability TPEE material, and compounding it with high-density polyethylene fiber, so that the TPEE composite film itself has better strength and moisture permeability. The material is made into a TPEE film, which has good barrier properties and better hygroscopicity, and can be widely used in higher-level medical packaging and high-level food packaging fields.

[0004] The present invention provides a TPEE composite material, comprising a modified TPEE elastomer and high-density polyethylene;

[0005] The modified TPEE elastomer is 53-57 parts by weight;

[0006] The high-density polyethylene is 45-55 parts by weight;

[0007] Wherein, the modified TPEE elastomer includes the following components in parts by weight:

[0008] TPEE resin 50 parts;

[0009] 2-4 parts of antistatic agent;

[0010] 1-3 parts of hydrophilic agent;

[0011] The polyether content of the TPEE elastomer is 10-20wt%; preferably 12-18%. The polyether content is determined by the mass ratio of polyester and polyether in the raw material feed. The higher the polyether content, the better the hydrophilicity of the ether-containing component, so the better the moisture permeability of the material, and the better the comfort of the fabric, but if the polyether content is too high, the mechanical properties of the material itself will be worse, affecting the hydrostatic pressure and tension of the material. The weight average molecular weight of high-density polyethylene is 200,000-400,000. The larger the molecular weight of HDPE, the higher the fiber tension and other properties, but the higher the molecular weight, the worse the spinning performance of the material. Experiments have confirmed that the molecular weight in the range of 200,000-400,000 is the preferred range of the material molecular weight.

[0012] The weight average molecular weight of the high-density polyethylene is 200,000-400,000; the use of high-density polyethylene fibers has better moisture permeability and can maintain good mechanical strength. In comparison, low-density PE and PP do not have the same mechanical strength when maintaining the same moisture permeability.

[0013] The TPEE composite material comprises a TPEE moisture permeable layer and a high-density polyethylene fiber mesh, which are composited together by thermal bonding.

[0014] Furthermore, the antistatic agent is isohexanol polyoxyethylene ether and / or polyethylene oxide. The antistatic effect of isohexanol polyoxyethylene ether and / or polyethylene oxide is more lasting than other small molecule antistatic agents. At the same time, its addition to TPEE material provides better compatibility for the subsequent composite of fabric and HDPE non-woven material.

[0015] Furthermore, the hydrophilic agent is one or more of methanesulfonic acid, octylphenol polyoxyethylene ether or acetylene glycol ethoxylate, preferably octylphenol polyoxyethylene ether. Octylphenol polyoxyethylene ether has more similar functional groups to TPEE and HDPE, and has better compatibility when the two are compounded.

[0016] Furthermore, the modified TPEE elastomer also includes an antioxidant, and the antioxidant is 0.3-1 parts by weight.

[0017] Furthermore, the surface density of the TPEE moisture permeable layer is 45±5g / m 2 ; The surface density of high-density polyethylene fiber mesh is 45±5g / m 2 .

[0018] Furthermore, the surface density of the TPEE composite material is 89-92 g / m 2 .

[0019] The present invention also provides a method for preparing the TPEE elastomer, comprising the following steps:

[0020] S1: Weigh each component by weight, and add the remaining components except high-density polyethylene into a high-speed mixer to mix and obtain a premix;

[0021] S2: The premix is ​​melt-extruded through a twin-screw extruder, small molecular substances are extracted by vacuum, and the TPEE elastomer is obtained by cooling and granulation.

[0022] Furthermore, the mixing time in S1 is 1 to 3 minutes, and the rotation speed is 1000 to 2000 rpm.

[0023] Furthermore, the temperature of each zone of the screw in S2 is 190-230° C., and the vacuum pressure is below -0.06 MPa.

[0024] The present invention also provides a method for preparing an ultra-high barrier and high-strength TPEE composite material, comprising the following steps:

[0025] (1) melt-extruding the prepared elastomer and pulling it into a film; melt-spinning the high-density polyethylene material, laying a net, and hot-rolling;

[0026] (2) melt spinning a high-density polyethylene material to obtain a fiber with a fiber diameter of 5-20 μm, and evenly laying the fiber to obtain a HDPE fiber fabric, and hot rolling to obtain a HDPE fiber fabric;

[0027] (3) TPEE and high-density polyethylene fiber fabric are hot-rolled to obtain the ultra-high barrier and high-strength TPEE composite material.

[0028] The present invention also provides the use of the ultra-high barrier high-strength TPEE composite material in the preparation of medical packaging or food packaging.

[0029] In summary, compared with the prior art, the present invention achieves the following technical effects:

[0030] (1) The present invention adopts the preferred TPEE material to modify the TPEE and compound it with the preferred HDPE material, which significantly improves the barrier property and strength of the material, making it widely used in the field of high-risk medical packaging;

[0031] (2) By selecting and compounding different high-density polyethylene and TPEE, the breaking strength and barrier capacity of the material are greatly improved, making the material have a better wrapping effect in metal medical packaging;

[0032] (3) The present invention uses common TPEE and high-density polyethylene as the substrate, and the method for obtaining the substrate has good economic efficiency and has broad application prospects in the fields of medical packaging, food packaging, etc. DETAILED DESCRIPTION

[0033] In order to enable those skilled in the art to better understand the solutions of the present invention, the technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only embodiments of a part of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0034] Example

[0035] The present invention is further described below in conjunction with specific examples and comparative examples. The following specific examples are all preferred implementations of the present invention, but the implementation of the present invention is not limited to the following examples, and is particularly not limited to the types of the various component raw materials used in the following specific examples.

[0036] 1. The raw materials used for each component are as follows:

[0037] TPEE resin: TPEE#1: polyether molar content is 15%, brand 4056, purchased from DuPont, USA;

[0038] TPEE resin: TPEE#2: polyether molar content is 20%, brand VT7812, purchased from DSM;

[0039] TPEE resin: TPEE#3: polyether molar content of 10%, brand VT3108, purchased from DSM;

[0040] TPEE resin: TPEE#4: polyether molar content is 7%, brand VT3104, purchased from DSM;

[0041] TPEE resin: TPEE#5: polyether molar content of 25%, brand VT3118, purchased from DSM;

[0042] High-density polyethylene: HDPE#1, weight average molecular weight Mw is 200,000, brand HDPE8008, purchased from Sinopec; the weight average molecular weight is tested by high temperature GPC, temperature is 150°C, flow rate is 1 mL / min, injection volume is 200 μL, the same below.

[0043] High-density polyethylene: HDPE#2, weight average molecular weight Mw is 300,000, brand BH500, purchased from Asahi Chemical;

[0044] High-density polyethylene: HDPE#3, weight average molecular weight Mw is 400,000, brand T0504F, purchased from Sinopec;

[0045] High-density polyethylene: HDPE#4, weight average molecular weight Mw is 500,000, brand T0604F, purchased from Sinopec;

[0046] High-density polyethylene: HDPE#5, weight average molecular weight Mw is 150,000, brand HDPE 5000S, purchased from Sinopec;

[0047] Low-density polyethylene: LDPE, weight average molecular weight Mw is 300,000, commercially available;

[0048] Antistatic agent #1: isohexyl alcohol polyoxyethylene ether, brand TF-481, Zhejiang Chuanhua Co., Ltd., the same substance was used in parallel experiments;

[0049] Antistatic agent #2: polyethylene oxide, brand WS308, Dow Chemical, USA;

[0050] Hydrophilic agent #1: Octylphenol polyoxyethylene ether, purchased from Shengxu Energy, the same substance was used in parallel experiments;

[0051] Hydrophilic agent #2: octadecyltrimethylammonium chloride, brand GX80, Guangzhou Diaoling Fine Chemicals;

[0052] Antioxidant: Hindered phenol antioxidant 1010, commercially available, the same substance was used in parallel experiments.

[0053] The preparation method of ultra-high barrier and high-strength TPEE composite materials is as follows: (1) Weigh each component (except HDPE) according to the weight parts in Table 1 and Table 2, add it to a high-speed mixer and mix it for 1 to 3 minutes, with a rotation speed of 1000 to 2000 rpm to obtain a premix; (2) The premix is ​​melt-extruded through a twin-screw extruder, the temperature of each zone of the screw is 190 to 230°C, and small molecules are extracted by vacuum, the vacuum pressure is below -0.06MPa, and the TPEE elastomer is obtained by vacuum granulation. (3) The prepared TPEE elastomer is added to the screw extruder for melt extrusion, and then passes through the material path and metering pump to enter the casting die. The melt meets the high-speed hot air at the outlet of the meltblowing die, and is stretched and homogenized into a film under the action of the high-speed hot air. After cooling and winding, the surface density is 45±5g / m 2 TPEE membrane structural material; (4) high-density polyethylene material is melt-spinned to obtain fibers with a fiber diameter of 5-20 μm, and the fibers are evenly laid to obtain HDPE fiber fabric, and the fabric surface density is 45±5 g / m after hot rolling. 2 (5) hot rolling TPEE and high-density polyethylene fiber fabric to obtain TPEE / HDPE composite fabric with a surface density of 89-92g / m 2 .

[0054] 2. Product performance test standards and conditions

[0055] Test the surface density, hydrostatic pressure, breaking strength and other properties of TPEE / HDPE composite fabric samples.

[0056] (1) The surface density is tested according to GB / T24218.1-2009 standard, and the testing instrument is an electronic balance;

[0057] (2) Hydrostatic pressure is tested according to ENISO811:2018 standard, with a pressure increase rate of 60 cm H 2 O / min;

[0058] (3) Breaking strength is tested according to GB / T 3923.1-1997 standard, sample size 50*150mm, pulling speed 100mm / min.

[0059] Table 1 Technical solutions and effects of the embodiments (parts by weight)

[0060]

[0061] Table 2 Comparative Examples Technical Scheme and Effects (Parts by Weight)

[0062] Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 Comparative Example 6 Comparative Example 7 TPEE#1 100 50 50 50 TPEE#4 50 TPEE#5 50 HDPE#1 100 50 50 HDPE#4 50 HDPE#5 50 LDPE 50 Antioxidants 1 1 1 1 1 1 1 Antistatic Agent #1 3 3 3 3 3 3 3 Hydrophilic Agent #1 2 2 2 2 2 2 2 <![CDATA[Areal density (g / m 2 )]]> 91 89 90 90 89 89 89 <![CDATA[Hydrostatic pressure (60 cm H 2 O / min)]]> 223 336 234 256 72 156 178 Breaking strength(N) 235 321 226 168 56 113 145

[0063] It can be seen from Examples 1 to 9 that the TPEE composite material has good strength, barrier properties and hygroscopicity through the formulation composition and preparation method of the present invention. The surface density is 89-92g / m 2 , hydrostatic pressure is 979-1234 (60cm H 2 O / min), breaking strength is 328-421N.

[0064] Comparative Examples 1 to 7 all have a single variable with Example 1, where Comparative Example 1 contains only TPEE without HDPE; Comparative Example 2 contains only HDPE without TPEE; the weight average molecular weight of the HDPE used in Comparative Example 3 is outside the range of 200,000-400,000; the polyether content of the TPEE used in Comparative Example 4 is less than 10wt%; Comparative Example 5 uses low-density polyethylene to replace high-density polyethylene, the polyether content of the TPEE used in Comparative Example 6 is greater than 20wt%, and the molecular weight of the HDPE used in Comparative Example 7 is less than 200,000. None of the above comparative examples can simultaneously meet the requirements of strength, barrier and hygroscopicity.

[0065] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A TPEE composite material, characterized in that: Including modified TPEE elastomer and high-density polyethylene; The modified TPEE elastomer is 53-57 parts by weight; The high-density polyethylene is 45-55 parts by weight; Wherein, the modified TPEE elastomer includes the following components in parts by weight: TPEE resin 50 parts; 2-4 parts of antistatic agent; 1-3 parts of hydrophilic agent; The polyether content of the TPEE elastomer is 10-20wt%; The weight average molecular weight of the high-density polyethylene is 200,000-400,000; The TPEE composite material comprises a TPEE moisture permeable layer and a high-density polyethylene fiber mesh, which are composited together by thermal bonding.

2. The TPEE composite material according to claim 1, characterized in that: The antistatic agent is isohexanol polyoxyethylene ether and / or polyethylene oxide.

3. The TPEE composite material according to claim 1, characterized in that: The hydrophilic agent is octylphenol polyoxyethylene ether.

4. The TPEE composite material according to claim 1, characterized in that: The modified TPEE elastomer also includes an antioxidant, and the antioxidant is 0.3-1 parts by weight.

5. The TPEE composite material according to claim 1, characterized in that: The surface density of TPEE moisture permeable layer is 45±5g / m 2 ; The surface density of high-density polyethylene fiber mesh is 45±5g / m 2 .

6. The TPEE composite material according to claim 1, characterized in that: The surface density of the TPEE composite material is 89-92g / m 2 .

7. The method for preparing the TPEE elastomer according to any one of claims 1 to 6, characterized in that: The steps include: S1: Weigh each component by weight, and add the remaining components except high-density polyethylene into a high-speed mixer to mix and obtain a premix; S2: The premix is ​​melt-extruded through a twin-screw extruder, small molecular substances are extracted by vacuum, and the TPEE elastomer is obtained by cooling and granulation.

8. The preparation method according to claim 7, characterized in that: The mixing time in S1 is 1 to 3 minutes, and the rotation speed is 1000 to 2000 rpm.

9. The preparation method according to claim 7, characterized in that: The temperature of each zone of the screw in S2 is 190-230°C, and the vacuum pressure is below -0.06MPa.

10. A method for preparing an ultra-high barrier and high-strength TPEE composite material, characterized in that: The steps include: (1) Melting and extruding the elastomer of claim 7, and drawing it into a film; melt spinning the high-density polyethylene material, laying a web, and hot rolling; (2) melt spinning a high-density polyethylene material to obtain a fiber with a fiber diameter of 5-20 μm, and evenly laying the fiber to obtain a HDPE fiber fabric, and hot rolling to obtain a HDPE fiber fabric; (3) TPEE and high-density polyethylene fiber fabric are hot-rolled to obtain the ultra-high barrier and high-strength TPEE composite material.

11. Use of the ultra-high barrier and high-strength TPEE composite material according to any one of claims 1 to 6 in the preparation of medical packaging or food packaging.

Citation Information

Patent Citations

  • Waterproof and moisture permeable composite membrane and preparation method thereof

    CN103963393A

  • Ultrahigh moisture-permeable matte thermoplastic polyurethane composition and preparation method thereof

    CN111171554A

  • Moisture-permeable film composite material and preparation method thereof

    CN113799465A

  • Waterproof and moisture-permeable composite material

    US20230071900A1