Production method of battery-grade lithium sulfide
By treating H2S-containing gas through a multi-stage absorption method and converting lithium sulfide using lithium hydroxide absorbent, the problems of high cost and environmental pollution in lithium sulfide production have been solved, achieving low-cost and high-efficiency production of battery-grade lithium sulfide.
Patent Information
- Application Number
- CN202411112829.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-12
AI Technical Summary
Existing technologies for lithium sulfide production involve high costs, numerous byproducts, environmental pollution, and safety risks, making industrial application difficult.
A multi-stage absorption method is adopted, using an absorbent containing lithium hydroxide to treat H2S gas in multiple stages. Through the conversion and crystallization of the first to third stage absorbents, battery-grade lithium sulfide is obtained, and the tail gas is recycled. The absorption temperature and liquid-to-gas ratio of each stage are controlled to reduce the CO2 and O2 content and increase the hydrogen sulfide content.
This technology enables low-cost, high-efficiency production of battery-grade lithium sulfide, reducing secondary pollution, improving product quality and conversion rate, and lowering production costs.
Smart Images

Figure CN118929581A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of new energy solid-state batteries, and in particular to a method for producing battery-grade lithium sulfide. Background Art
[0002] In recent years, all-solid-state lithium-ion batteries have high safety performance and excellent electrochemical performance due to the use of non-flammable solid electrolytes. Sulfide solid electrolytes have attracted widespread attention among several types of solid electrolytes because of their high ionic conductivity. Lithium sulfide (Li2S) is a key raw material for the preparation of sulfide electrolytes for solid-state batteries. A 1GWh solid-state battery based on Li6PS5Cl (LPSC) electrolyte consumes 400-450 kg of Li2S. The current kilogram-level bulk purchase price is 6000-7000 yuan / kg, accounting for 99% of the cost of LPSC electrolyte raw materials. The high price limits its widespread application in the market and hinders the rapid development of sulfide solid-state batteries. Therefore, exploring low-cost large-scale synthesis of battery-grade lithium sulfide has become one of the key factors for the industrialization of sulfide solid electrolytes.
[0003] At present, the industrial production method of Li2S is carbon thermal reduction (Li2SO4+2C→Li2S+2CO2), which has many by-products and emits CO2. Other synthesis methods include ball milling (2Li+S→Li2S), double decomposition (2LiCl+Na2S→Li2S+2NaCl), solid phase reaction (2LiOH+H2S→Li2S+H2O or Li2CO3+H2S→Li2S+H2O+CO2), etc. Double decomposition reaction and gas-solid phase reaction are not thorough, the product purity cannot meet the requirements, and double decomposition reaction requires a large amount of organic solvents, which pollutes the environment. High temperature reaction has high requirements for reaction equipment and has certain safety risks. Summary of the invention
[0004] In view of the deficiencies in the prior art, the present invention aims to provide a method for producing battery-grade lithium sulfide.
[0005] In order to achieve the above object, the present invention adopts the following technical solution:
[0006] A method for producing battery-grade lithium sulfide comprises the following steps:
[0007] S1. Perform at least three-stage multi-stage absorption of H2S-containing gas;
[0008] The absorption liquid used in the first stage is an absorption liquid containing lithium sulfide. The H2S-containing gas first passes through the absorption liquid of the first stage, and the H2S in the absorption liquid converts the lithium sulfide in the absorption liquid into lithium hydrosulfide.
[0009] The absorption liquid used in the second stage is an absorption liquid containing lithium sulfide. The H2S-containing gas enters the second stage absorption after being absorbed in the first stage, and the H2S therein converts part of the lithium sulfide in the absorption liquid of the second stage into lithium hydrosulfide. Then, the absorption liquid containing lithium hydroxide in the third stage is added to the slurry after the second stage absorption, so that the lithium hydrosulfide therein is converted into lithium sulfide. The amount of the absorption liquid containing lithium hydroxide added needs to ensure that the slurry of the second stage does not contain lithium hydroxide. Then, the lithium sulfide in the slurry and the remaining lithium hydrosulfide are crystallized by cooling.
[0010] The absorption liquid used in the third stage is an absorption liquid containing lithium hydroxide. The gas after the second stage absorption enters the third stage absorption to ensure that the remaining hydrogen sulfide is fully absorbed and no secondary pollution is generated. After the third stage absorption, the tail gas meets the emission standards.
[0011] S2, taking out the slurry after the absorption liquid containing lithium hydroxide is added in the second stage and cooled and crystallized for solid-liquid separation, and drying and pyrolyzing the separated solid to obtain battery-grade lithium sulfide, and returning the dried tail gas and the pyrolysis tail gas to step S1 for multi-stage absorption; part of the slurry after solid-liquid separation is continuously used for the absorption in the second stage, and part of it is added to the absorption liquid in the first stage.
[0012] Furthermore, in step S1, the H2S-containing gas is obtained by pretreatment of one or more of petrochemical acid gas, coal chemical low-temperature methanol washing regeneration acid gas and hydrogen and sulfur reaction process gas. The H2S-containing gas obtained after pretreatment has an oxygen volume content of <0.02%, a CO2 volume content of <0.05%, an H2S volume content of 25-99.95%, a temperature of 5-45°C, and a pressure of 15-500kPa.
[0013] Furthermore, the pretreatment includes firstly using organic amine to selectively absorb H2S, and then analyzing it under reduced pressure and heating conditions to obtain H2S-containing gas that meets the requirements.
[0014] Furthermore, in step S1, the mass concentration of lithium hydroxide in the absorption liquid containing lithium hydroxide is 10%-25%.
[0015] Furthermore, in step S2, the slurry after the cooling crystallization is cooled again to 0-10°C before solid-liquid separation, and the solid mass content of the slurry after cooling is 15%-35%.
[0016] Furthermore, in step S2, the solid-liquid separation, drying and pyrolysis are all carried out under an inert gas atmosphere; the dried tail gas returns to the gas connecting pipe between the second-stage absorption and the third-stage absorption, and the pyrolysis tail gas returns to the first-stage absorption; the temperature of the dried tail gas is 80-112°C, and the volume content of H2S is 1%-3.5%; the temperature of the pyrolysis tail gas is 170°C-290°C, and the volume content of H2S is 12%-65%.
[0017] Furthermore, in step S1, the liquid-gas ratio of the first stage absorption is 25-40 L / Nm 3 , 3-4 spray layers are set in the first-stage absorption equipment for spray absorption, the absorption temperature is 30-38°C, the absorption pressure is 100-500kPa, and the first-stage absorption liquid is cooled in the circulation pipeline with a cooler and then circulated back to the first-stage absorption equipment to remove the heat in time and ensure that the absorption temperature does not exceed 38°C;
[0018] The liquid-gas ratio of the second stage absorption is 8-15L / Nm 3 , 2-3 spray layers are set in the second-stage absorption equipment for spray absorption, the absorption temperature is 10-22°C, and the absorption pressure is 50-300kPa;
[0019] The liquid-gas ratio of the third stage absorption is 3-10L / Nm 3 In the third-level absorption equipment, 1-3 spray layers are set for spray absorption, the absorption temperature is 20-32°C, and the absorption pressure is 15-60kPa.
[0020] Furthermore, in step S1, the absorption liquid containing lithium hydroxide is obtained by adding liquid alkali to the lithium sulfate solution and then sequentially subjecting the solution to freezing separation, evaporation concentration, crystallization separation and water dissolution.
[0021] Furthermore, in step S1, 10%-50% of the H2S-containing gas is directly added to the first-stage absorption liquid according to mass percentage, and the remaining H2S-containing gas is sent to the first-stage absorption equipment for absorption; before the dry tail gas enters the gas connecting pipe between the second-stage absorption and the third-stage absorption, the dry tail gas is first cooled to 20-40°C.
[0022] The beneficial effects of the present invention are:
[0023] 1. The method of the present invention utilizes lithium hydroxide and hydrogen sulfide-containing acidic gas to produce battery-grade lithium sulfide. Compared with other processes, the raw material cost is low;
[0024] 2. The method of the present invention adopts multi-stage absorption to control the absorption temperature, liquid-gas ratio and absorption liquid composition of each stage, so as to achieve efficient output of lithium sulfide / lithium hydrosulfide slurry;
[0025] 3. In the method of the present invention, the drying tail gas and the pyrolysis tail gas are recycled to improve the conversion rate of hydrogen sulfide without secondary pollution;
[0026] 4. The method of the present invention pre-treats the hydrogen sulfide-containing gas, reduces the CO2 and O2 contents, and increases the hydrogen sulfide content, thereby ensuring the quality of the lithium sulfide product. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 Flowchart of methods according to various embodiments of the present invention. DETAILED DESCRIPTION
[0028] The present invention will be further described below in conjunction with the accompanying drawings. It should be noted that this embodiment is based on the technical solution and provides a detailed implementation method and specific operation process, but the protection scope of the present invention is not limited to this embodiment.
[0029] Example 1
[0030] This embodiment provides a method for producing battery-grade lithium sulfide, such as Figure 1 As shown, the following steps are included:
[0031] S1. Perform 3-stage multi-stage absorption of H2S-containing gas;
[0032] The absorption liquid used in the first stage is an absorption liquid containing lithium sulfide. The H2S-containing gas first passes through the absorption liquid of the first stage, and the H2S in the absorption liquid converts the lithium sulfide in the absorption liquid into lithium hydrosulfide.
[0033] The absorption liquid used in the second stage is an absorption liquid containing lithium sulfide. The H2S-containing gas enters the second stage absorption after being absorbed in the first stage, and the H2S therein converts part of the lithium sulfide in the absorption liquid of the second stage into lithium hydrosulfide. Then, the absorption liquid containing lithium hydroxide in the third stage is added to the slurry after the second stage absorption, so that the lithium hydrosulfide therein is converted into lithium sulfide. The amount of the absorption liquid containing lithium hydroxide added needs to ensure that the slurry of the second stage does not contain lithium hydroxide. Then, the lithium sulfide in the slurry and the remaining lithium hydrosulfide are crystallized by cooling.
[0034] The absorption liquid used in the third stage is an absorption liquid containing 25% (mass fraction) lithium hydroxide. The gas after the second stage absorption enters the third stage absorption to ensure that the remaining hydrogen sulfide is fully absorbed and no secondary pollution is generated. After the third stage absorption, the tail gas meets the emission standards.
[0035] In this embodiment, the H2S-containing gas is obtained by pre-treatment of the acid gas regenerated by low-temperature methanol washing in coal chemical industry. The flow rate of the acid gas regenerated by low-temperature methanol washing in coal chemical industry is 50Nm 3 / h, H2S concentration 32%. The H2S gas obtained after pretreatment has an oxygen content of 120ppm (volume), a CO2 content of 104ppm (volume), an H2S content of 93.7% (volume), and the remaining components include N2, Ar and saturated water vapor, a temperature of 25°C, and a pressure of 260kPa. The pretreatment includes organic amine absorption and analysis, using organic amine to selectively absorb H2S in the acid gas regenerated by low-temperature methanol washing in coal chemical industry, and then analyzing H2S, CO2, and oxygen-containing gas that meet the requirements under reduced pressure and heating conditions.
[0036] S2, taking out the slurry after the absorption liquid containing lithium hydroxide is added in the second stage and cooled and crystallized for solid-liquid separation, and drying and pyrolyzing the separated solid to obtain battery-grade lithium sulfide, and returning the dried tail gas and the pyrolysis tail gas to step S1 for multi-stage absorption; part of the slurry after solid-liquid separation is continuously used for the absorption in the second stage, and part of it is added to the absorption liquid in the first stage.
[0037] In this embodiment, in step S1, the liquid-gas ratio of the first stage absorption is 25L / Nm 3 The first stage absorption equipment is equipped with three spray layers, the absorption temperature is 30 / 31.5 / 33℃ from top to bottom, and the absorption pressure is 150 / 200 / 250kPa from top to bottom. The liquid-gas ratio of the second stage absorption is 12L / Nm 3 The second-stage absorption equipment is equipped with three spray layers, and the absorption temperatures are 10 / 14 / 17℃ from top to bottom, and the absorption pressures are 50 / 67 / 90kPa from top to bottom. The liquid-gas ratio of the third-stage absorption is 6L / Nm 3 The third-level absorption equipment is equipped with two spray layers, and the absorption temperature is 20 / 26℃ from top to bottom, and the absorption pressure is 15 / 40kPa from top to bottom.
[0038] In this embodiment, in step S1, in the first stage absorption, 40% (mass fraction) of H2S-containing gas is directly added to the absorption liquid of the first stage absorption in a spraying manner, and the rest of the H2S gas is added to the absorption equipment sent to the first stage.
[0039] In this embodiment, in step S1, the absorption liquid containing lithium hydroxide is obtained by adding liquid alkali to a lithium sulfate solution, freezing separation, evaporation concentration, crystallization separation, and dissolution with water.
[0040] In this embodiment, in step S1, the slurry is cooled to 5°C before solid-liquid separation, and the solid mass content of the slurry after cooling is 18%.
[0041] In this embodiment, in step S2, the solid-liquid separation, drying and pyrolysis are all carried out under nitrogen atmosphere. The temperature of the drying tail gas is 80°C, and the volume content of H2S is 1%; the temperature of the pyrolysis tail gas is 170°C, and the volume content of H2S is 12%. The drying tail gas returns to the gas connection pipe between the second stage absorption and the third stage absorption, and the pyrolysis tail gas returns to the first stage absorption.
[0042] In this embodiment, in step S2, the dry tail gas is cooled before being sent into the gas connecting pipe between the second-stage absorption and the third-stage absorption, and the cooling method includes circulating water cooling + chilled water cooling, and the temperature is reduced to 25°C.
[0043] In this embodiment, the slurry taken out in step S1 includes lithium sulfide, lithium hydrosulfide, and contains 7.5% (mass fraction) of crystals.
[0044] In this embodiment, in the third stage absorption, the amount of lithium hydroxide monohydrate replenished is equivalent to 60.4 kg / h, and the output of battery-grade lithium sulfide is 32.77 kg / h.
[0045] Example 2
[0046] This embodiment provides a method for producing battery-grade lithium sulfide, such as Figure 1 As shown, the following steps are included:
[0047] S1. Perform three-stage multi-stage absorption of H2S-containing gas, and the absorption liquid of each stage circulates independently;
[0048] The absorption liquid used in the first stage is an absorption liquid containing lithium sulfide. The H2S-containing gas first passes through the absorption liquid of the first stage, and the H2S in the absorption liquid converts the lithium sulfide in the absorption liquid into lithium hydrosulfide.
[0049] The absorption liquid used in the second stage is an absorption liquid containing lithium sulfide. The H2S-containing gas enters the second stage absorption after being absorbed in the first stage, and the H2S therein converts part of the lithium sulfide in the absorption liquid of the second stage into lithium hydrosulfide. Then, the absorption liquid containing lithium hydroxide in the third stage is added to the slurry after the second stage absorption, so that the lithium hydrosulfide therein is converted into lithium sulfide. The amount of the absorption liquid containing lithium hydroxide added needs to ensure that the slurry of the second stage does not contain lithium hydroxide. Then, the lithium sulfide in the slurry and the remaining lithium hydrosulfide are crystallized by cooling.
[0050] The absorption liquid used in the third stage is an absorption liquid containing 22% (mass fraction) lithium hydroxide. The gas after the second stage absorption enters the third stage absorption to ensure that the remaining hydrogen sulfide is fully absorbed and no secondary pollution is generated. After the third stage absorption, the tail gas meets the emission standards.
[0051] S2. The slurry after the absorption liquid containing lithium hydroxide is added to the second stage and cooled and crystallized is subjected to solid-liquid separation. The separated solid is dried and pyrolyzed. The lithium sulfide after pyrolysis is further pulverized by air flow and iron removal to obtain battery-grade lithium sulfide. Part of the slurry after solid-liquid separation is continuously used for absorption in the second stage, and part is added to the absorption liquid in the first stage.
[0052] In this embodiment, in step S1, the H2S-containing gas is obtained by pre-treatment of petrochemical acid gas, and the flow rate of the petrochemical acid gas is 120 Nm 3 / h, H2S concentration 91%. The H2S gas obtained after pretreatment has an oxygen content of 30ppm (volume), a CO2 content of 40ppm (volume), an H2S content of 99.2% (volume), and the remaining components include N2, Ar, and saturated water vapor; the temperature is 25°C, and the pressure is 420kPa;
[0053] The pretreatment includes potassium sulfide solution absorption and analysis, using potassium sulfide solution to selectively absorb H2S in petrochemical acid gas, and then analyzing H2S-containing gas with H2S, CO2 and oxygen concentrations meeting requirements under reduced pressure and heating conditions.
[0054] In this embodiment, in step S1, in the first stage absorption, 10% (mass fraction) of H2S-containing gas is directly added to the absorption liquid of the first stage absorption in a static mixing manner, and the rest of the H2S gas is added to the first stage absorption equipment.
[0055] In this embodiment, in step S1, the absorption liquid containing lithium hydroxide is obtained by adding liquid alkali to a lithium sulfate solution, freezing separation, evaporation concentration, crystallization separation, and dissolution with water.
[0056] In this embodiment, in step S2, the slurry components taken out include lithium sulfide, lithium hydrosulfide, and 10% (mass fraction) of crystals.
[0057] In this embodiment, in step S2, the slurry is first cooled to 0°C using chilled water before solid-liquid separation, and the solid content (mass fraction) of the slurry after cooling is 25%; the solid-liquid separation, drying and pyrolysis are all carried out under argon atmosphere. The temperature of the dry tail gas is 112°C, the H2S content is 3.5%, the temperature of the pyrolysis tail gas is 290°C, and the H2S content is 65%. The dry tail gas returns to the gas connecting pipe between the second-stage absorption and the third-stage absorption, and the pyrolysis tail gas returns to the first-stage absorption.
[0058] In this embodiment, in step S1, the liquid-gas ratio of the first stage absorption is 40L / Nm 3 The first-stage absorption equipment is equipped with 4 spray layers, and the absorption temperatures are 35 / 36 / 37 / 38℃ from top to bottom, and the absorption pressures are 310 / 365 / 420 / 500kPa from top to bottom; the liquid-gas ratio of the second-stage absorption is 15L / Nm 3 The second-level absorption equipment is equipped with three spray layers, with absorption temperatures of 10 / 12.5 / 16°C and pressures of 150 / 215 / 300 kPa respectively. The liquid-gas ratio of the third-level absorption is 10 L / Nm 3 The third-level absorption equipment is equipped with three spray layers, and the absorption temperatures are 27 / 28.5 / 32°C from top to bottom, and the absorption pressures are 45 / 51 / 60 kPa from top to bottom.
[0059] In this embodiment, in step S2, the dry tail gas is cooled before being sent into the gas connecting pipe between the second-stage absorption and the third-stage absorption, and the cooling method includes circulating water cooling + chilled water cooling, and the temperature is reduced to 35°C.
[0060] In this embodiment, the amount of lithium hydroxide monohydrate added in the third stage absorption is 412.2 kg / h, and the output of battery-grade lithium sulfide is 223.66 kg / h.
[0061] Example 3
[0062] This embodiment provides a method for producing battery-grade lithium sulfide, such as Figure 1 As shown, the following steps are included:
[0063] S1. Perform three-stage multi-stage absorption of H2S-containing gas, and the absorption liquid of each stage circulates independently;
[0064] The absorption liquid used in the first stage is an absorption liquid containing lithium sulfide. The H2S-containing gas passes through the absorption liquid of the first stage and converts the lithium sulfide in the absorption liquid into lithium hydrosulfide.
[0065] The absorption liquid used in the second stage is an absorption liquid containing lithium sulfide. After the H2S-containing gas is absorbed in the first stage, it enters the absorption in the second stage. The remaining H2S converts part of the lithium sulfide in the absorption liquid of the second stage into lithium hydrosulfide. Then, the absorption liquid containing lithium hydroxide in the third stage is added to the slurry after the second stage absorption, so that most of the lithium hydrosulfide therein is converted into lithium sulfide. Then, the lithium sulfide / lithium hydrosulfide in the slurry after the second stage absorption is crystallized by cooling. The amount of the absorption liquid containing lithium hydroxide added to the slurry after the second stage absorption is controlled to ensure that the slurry of the second stage does not contain lithium hydroxide.
[0066] The absorption liquid used in the third stage is an absorption liquid containing 10% (mass fraction) lithium hydroxide. The gas after the second stage absorption enters the third stage absorption to ensure that the hydrogen sulfide is fully absorbed and no secondary pollution is generated. After the third stage absorption, the exhaust gas meets the emission standards.
[0067] S2. The slurry after the absorption liquid containing lithium hydroxide is added to the second stage and cooled and crystallized is subjected to solid-liquid separation. The separated solid is dried and pyrolyzed. The lithium sulfide after pyrolysis is further pulverized by air flow and iron removal to obtain battery-grade lithium sulfide.
[0068] In this embodiment, in step S1, the H2S-containing gas is obtained by pre-treating the process gas of the reaction of hydrogen and sulfur, and the flow rate of the process gas of the reaction of hydrogen and sulfur is 45Nm 3 / h, H2S concentration 96%. The H2S gas obtained after pretreatment has an oxygen content of 5ppm (volume fraction), a CO2 content of 10ppm (volume), an H2S content of 99.9% (volume), and the remaining components include N2 and Ar; the temperature is 45°C, and the pressure is 350kPa;
[0069] The pretreatment includes sulfur removal, using sulfur to remove H2S in the process gas of hydrogen and sulfur reaction, and then analyzing H2S-containing gas with H2S, CO2 and oxygen concentrations meeting the requirements under reduced pressure and heating conditions.
[0070] In this embodiment, in step S1, the liquid-gas ratio of the first stage absorption is 36L / Nm 3 The first-stage absorption equipment is equipped with 4 spray layers, with absorption temperatures of 30 / 31 / 32 / 33°C and pressures of 260 / 280 / 303 / 330 kPa respectively; the second-stage absorption liquid-gas ratio is 13.5 L / Nm 3 The second-stage absorption equipment is equipped with three spray layers, with absorption temperatures of 15 / 17.4 / 21°C and absorption pressures of 110 / 170 / 250 kPa from top to bottom; the liquid-gas ratio of the third-stage absorption is 8 L / Nm 3 The third-level absorption equipment is equipped with two spray layers, and the absorption temperature is 20 / 25℃ from top to bottom, and the absorption pressure is 35 / 50kPa respectively.
[0071] In this embodiment, in step S1, in the first stage absorption, 30% (mass fraction) of H2S-containing gas is directly added to the absorption liquid of the first stage absorption in a static mixing manner, and the rest of the H2S gas is added to the first stage absorption equipment.
[0072] In this embodiment, in step S1, the absorption liquid containing lithium hydroxide is obtained by adding liquid alkali to a lithium sulfate solution, freezing separation, evaporation concentration, crystallization separation, and dissolution with water.
[0073] In this embodiment, in step S2, the slurry components taken out include lithium sulfide, lithium hydrosulfide, and 3% (mass fraction) of crystals.
[0074] In this embodiment, in step S2, the slurry is first cooled to 7.5°C using chilled water before solid-liquid separation, and the solid content (mass fraction) of the slurry after cooling is 15%. The solid-liquid separation, drying and pyrolysis are all carried out under the atmosphere of nitrogen + argon. The temperature of the dry tail gas is 92°C, the volume content of H2S is 1.5%, the temperature of the pyrolysis tail gas is 220°C, and the volume content of H2S is 25%. The dry tail gas returns to the gas connecting pipe between the second stage absorption and the third stage absorption, and the pyrolysis tail gas returns to the first stage absorption.
[0075] In this embodiment, in step S2, the dry tail gas is cooled before being sent into the gas connecting pipe between the second-stage absorption and the third-stage absorption, and the cooling method includes circulating water cooling + chilled water cooling, and the temperature is reduced to 23°C.
[0076] In this embodiment, in the third stage absorption, the amount of lithium hydroxide monohydrate replenished is equivalent to 163 kg / h. The output of battery-grade lithium sulfide is 88.48 kg / h.
[0077] Example 4
[0078] This embodiment provides a device for implementing the method described in embodiments 1-3, including an H2S generation unit, an H2S pretreatment unit, a primary absorption unit, a secondary absorption unit, a tertiary absorption unit, a solid-liquid separation unit, a drying unit, a pyrolysis unit, and a lithium hydroxide supply unit;
[0079] The H2S outlet, H2S pretreatment unit, primary absorption unit, secondary absorption unit, and tertiary absorption unit of the H2S generation unit are connected in sequence; the lithium sulfide / lithium hydrosulfide slurry outlet, solid-liquid separation unit, drying unit, and pyrolysis unit of the secondary absorption unit are connected in sequence; the tail gas outlet of the drying unit is connected to the gas pipe between the secondary absorption unit and the tertiary absorption unit, and the gas outlet of the pyrolysis unit is connected to the circulation pipeline and / or H2S inlet pipe of the primary absorption unit. The lithium hydroxide solution outlet of the lithium hydroxide supply unit is connected to the tertiary absorption unit.
[0080] For those skilled in the art, various corresponding changes and modifications can be made according to the above technical solutions and concepts, and all of these changes and modifications should be included in the protection scope of the claims of the present invention.
Claims
1. A method for producing battery-grade lithium sulfide, characterized in that: The following steps are involved: S1. Perform at least three-stage multi-stage absorption of H2S-containing gas; The absorption liquid used in the first stage is an absorption liquid containing lithium sulfide. The H2S-containing gas first passes through the absorption liquid of the first stage, and the H2S in the absorption liquid converts the lithium sulfide in the absorption liquid into lithium hydrosulfide. The absorption liquid used in the second stage is an absorption liquid containing lithium sulfide. The H2S-containing gas enters the second stage absorption after being absorbed in the first stage, and the H2S therein converts part of the lithium sulfide in the absorption liquid of the second stage into lithium hydrosulfide. Then, the absorption liquid containing lithium hydroxide in the third stage is added to the slurry after the second stage absorption, so that the lithium hydrosulfide therein is converted into lithium sulfide. The amount of the absorption liquid containing lithium hydroxide added needs to ensure that the slurry of the second stage does not contain lithium hydroxide. Then, the lithium sulfide in the slurry and the remaining lithium hydrosulfide are crystallized by cooling. The absorption liquid used in the third stage is an absorption liquid containing lithium hydroxide. The gas after the second stage absorption enters the third stage absorption to ensure that the remaining hydrogen sulfide is fully absorbed and no secondary pollution is generated. After the third stage absorption, the tail gas meets the emission standards. S2, taking out the slurry after the absorption liquid containing lithium hydroxide is added in the second stage and cooled and crystallized for solid-liquid separation, and drying and pyrolyzing the separated solid to obtain battery-grade lithium sulfide, and returning the dried tail gas and the pyrolysis tail gas to step S1 for multi-stage absorption; part of the slurry after solid-liquid separation is continuously used for the absorption in the second stage, and part of it is added to the absorption liquid in the first stage.
2. The production method according to claim 1, characterized in that In step S1, the H2S-containing gas is obtained by pretreatment of one or more of petrochemical acid gas, coal chemical low-temperature methanol washing regeneration acid gas and hydrogen and sulfur reaction process gas. The H2S-containing gas obtained after pretreatment has an oxygen volume content of less than 0.02%, a CO2 volume content of less than 0.05%, an H2S volume content of 25-99.95%, a temperature of 5-45°C, and a pressure of 15-500kPa.
3. The production method according to claim 2, characterized in that: The pretreatment includes firstly utilizing organic amine to selectively absorb H2S, and then analyzing it under reduced pressure and heating conditions to obtain H2S-containing gas that meets the requirements.
4. The production method according to claim 1, characterized in that In step S1, the mass concentration of lithium hydroxide in the absorption liquid containing lithium hydroxide is 10%-25%.
5. The production method according to claim 1, characterized in that: In step S2, the slurry after cooling and crystallization is cooled again to 0-10°C before solid-liquid separation, and the solid mass content of the slurry after cooling is 15%-35%.
6. The production method according to claim 1, characterized in that: In step S2, the solid-liquid separation, drying and pyrolysis are all carried out under an inert gas atmosphere; the dried tail gas returns to the gas connecting pipe between the second-stage absorption and the third-stage absorption, and the pyrolysis tail gas returns to the first-stage absorption; the temperature of the dried tail gas is 80-112°C, and the volume content of H2S is 1%-3.5%; the temperature of the pyrolysis tail gas is 170°C-290°C, and the volume content of H2S is 12%-65%.
7. The production method according to claim 1, characterized in that: In step S1, the liquid-gas ratio of the first stage absorption is 25-40L / Nm 3 , 3-4 spray layers are set in the first-stage absorption equipment for spray absorption, the absorption temperature is 30-38°C, the absorption pressure is 100-500kPa, and the first-stage absorption liquid is cooled in the circulation pipeline with a cooler and then circulated back to the first-stage absorption equipment to remove the heat in time and ensure that the absorption temperature does not exceed 38°C; The liquid-gas ratio of the second stage absorption is 8-15L / Nm 3 , 2-3 spray layers are set in the second-stage absorption equipment for spray absorption, the absorption temperature is 10-22°C, and the absorption pressure is 50-300kPa; The liquid-gas ratio of the third stage absorption is 3-10L / Nm 3 In the third-level absorption equipment, 1-3 spray layers are set for spray absorption, the absorption temperature is 20-32°C, and the absorption pressure is 15-60kPa.
8. The production method according to claim 1, characterized in that: In step S1, the absorption liquid containing lithium hydroxide is obtained by adding liquid alkali to a lithium sulfate solution and then sequentially subjecting the solution to freezing separation, evaporation concentration, crystallization separation and water dissolution.
9. The production method according to claim 7, characterized in that: In step S1, 10%-50% of the H2S-containing gas is directly added to the first-stage absorption liquid according to mass percentage, and the remaining H2S-containing gas is sent to the first-stage absorption equipment for absorption; before the dry tail gas enters the gas connecting pipe between the second-stage absorption and the third-stage absorption, the dry tail gas is first cooled to 20-40°C.
Citation Information
Patent Citations
Process for preparing lithium sulfide
CN103813980A
Preparation method and device of high-purity lithium sulfide
CN105016310A
Method of concentrating and recycling hydrogen sulfide in industrial acid gas by absorption of organic solvent
CN110052119A
Method for preparing battery-grade lithium hydroxide monohydrate from crude lithium sulfate
CN115215357A
Method for producing lithium composition and method for producing sulfide solid electrolyte material
US20160365603A1
Cited By
Lithium sulfide preparation method based on waste metal lithium resource
CN120736474A
Preparation method of lithium sulfide