Preparation method of high-compaction power type lithium iron phosphate

Nano-scale lithium iron phosphate particles were prepared by ferrous oxalate method, and ball milling treatment with methanol and organic dispersant was combined to solve the problem of uneven dispersion of lithium iron phosphate particles, and achieved high compaction density and good dynamic performance lithium iron phosphate Materials meet the needs of high energy density while reducing production costs.

CN118929610APending Publication Date: 2024-11-12湖南鹏博新材料有限公司

Patent Information

Application Number
CN202411113541.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing solution to improve the particle size of lithium iron phosphate mixing is difficult to achieve uniform dispersion of nano-scale particles, resulting in insufficient compaction density and unable to meet the needs of high energy density.

Method used

Using ferrous oxalate as the precursor, nanoscale lithium iron phosphate particles are prepared by ball milling, drying and calcining treatment, and methanol is used as a medium and organic dispersant during the ball milling process, combined with carbon source and grinding aid to form a slurry for spraying. Sintering to achieve uniform mixing and particle grading at the submicron level.

Benefits of technology

The high compaction density and good power performance of lithium iron phosphate are achieved, with compaction density greater than 2.72g/cm3 and the 0.5C discharge capacity greater than 146mAh/g, while reducing production costs.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides a preparation method of high-compaction power type lithium iron phosphate. The preparation method of the high-compaction power type lithium iron phosphate comprises the following steps: preparing lithium iron phosphate powder on the basis of ferrous oxalate, preparing lithium iron phosphate slurry, preparing lithium iron phosphate slurry on the basis of iron phosphate, and mixing. The preparation method of the high-compaction power type lithium iron phosphate provided by the invention solves the problem that uniform dispersion is difficult to realize in the existing scheme of mixing the lithium iron phosphate to improve the particle size.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of batteries, and in particular to a method for preparing high-density power lithium iron phosphate. Background Art

[0002] Currently, lithium iron phosphate is the main application material for new energy vehicles, with a market share of more than 60%. However, the energy density of lithium iron phosphate is naturally lower than that of ternary lithium. In order to improve the energy density of lithium iron phosphate batteries, improving the compaction of the pole pieces is the key, that is, to increase the compaction density of lithium iron phosphate materials. At present, the focus is on optimizing the carbon source coating to improve the compaction density, and achieving a reasonable gradation through particle size distribution is the underlying logic for improving the compaction of lithium iron phosphate. There are existing solutions to increase the particle size by mixing lithium iron phosphate of different particle sizes, but all of them are to mix the finished lithium iron phosphate, without considering the problem that nano-scale particles are difficult to disperse evenly during mixing. Summary of the invention

[0003] In order to solve the problem that the existing solution of mixing lithium iron phosphate to increase particle size is difficult to achieve uniform dispersion, the present invention provides a method for preparing high-density dynamic lithium iron phosphate that solves the above problem.

[0004] A method for preparing high-pressure compaction power type lithium iron phosphate comprises the following steps:

[0005] Step 1: Based on ferrous oxalate, a phosphorus source and a lithium source are added, and the first powder is obtained by ball milling, drying and calcining;

[0006] This step is to prepare nano-scale lithium iron phosphate particles. Since nanoparticles are highly active and the electron conductivity inside the particles is much higher than that between particles, the nanoparticles have better rate performance, making the positive electrode material meet the needs of power batteries.

[0007] The usual preparation of nanoparticles requires the preparation of nanoscale precursors by coprecipitation or long-term high-energy ball milling to crush the materials to nanoscale, which increases costs. This step can save costs to a large extent by spontaneously generating nanoparticles through the high-temperature decomposition characteristics of ferrous oxalate. By controlling the sintering temperature and time, excessive growth of particles can be avoided.

[0008] Step 2: ball-milling the first powder, the first carbon source and the dispersant with methanol as the medium to obtain a first slurry;

[0009] The key to this step is to disperse the nano-sized lithium iron phosphate particles prepared in the previous step. The key is to use an organic dispersant to attach to the particles to form a "film" to prevent the particles from agglomerating and achieve a dispersion effect. Carbon source PP, as a hard spherical carbon source, can also play a grinding aid role.

[0010] Step 3: Based on iron phosphate, a lithium source and a second carbon source are added, and methanol is used as a medium to obtain a second slurry through ball milling;

[0011] In this step, lithium iron phosphate is prepared using the iron phosphate process. By controlling the ball milling parameters and adjusting the particle size of the iron phosphate, a particle grading is achieved to achieve a higher compaction.

[0012] Step 4: The first slurry and the second slurry are mixed, and after drying, calcination and crushing, a finished high-density power-type lithium iron phosphate positive electrode material is obtained.

[0013] In a preferred embodiment of the method for preparing high-pressure power lithium iron phosphate provided by the present invention, in the step 1, ferrous oxalate and lithium dihydrogen phosphate are added at a molar ratio of Li:Fe of 1:(0.97-0.99).

[0014] The mixture is ball-milled for 30 to 60 minutes until the particle size is 2 to 4 μm, spray-dried, and calcined at 400 to 500° C. for 3 to 6 hours to obtain the first powder.

[0015] In a preferred embodiment of the high-pressure compaction power lithium iron phosphate preparation method provided by the present invention, in the step 2, the first carbon source is added at a ratio of 2 to 6% of the mass of the first powder, the dispersant is added at a ratio of 1 to 5% of the mass of the first powder, and methanol is added at a ratio of 1 kg / 5 L of the mass of the first powder.

[0016] The first slurry is obtained by ball milling for 1 to 3 hours.

[0017] The first carbon source is PP, which is spherical in shape and has a particle size of less than 10 μm; the dispersant is one or more of ethylene glycol, stearic acid, oleic acid, sodium fatty alcohol sulfate, and carboxy betaine.

[0018] In a preferred embodiment of the method for preparing high-pressure power lithium iron phosphate provided by the present invention, in the step 3, iron phosphate and lithium bicarbonate are added at a molar ratio of Li:Fe of 1:(0.95-0.98), and the total mass of iron phosphate and lithium bicarbonate is 4-7 times that of the first powder; the second carbon source is added at a ratio of 2-6% of the total mass of iron phosphate and lithium bicarbonate, and methanol is added at a ratio of 1 kg / 5 L of the total mass of iron phosphate and lithium bicarbonate.

[0019] The ball milling treatment is performed for 2 to 4 hours until the particle size is 1 to 2 μm, thereby obtaining the second slurry.

[0020] The second carbon source is one or more of glucose, sucrose, citric acid, ascorbic acid, and polyethylene glycol 400-800.

[0021] In a preferred embodiment of the method for preparing high-pressure compaction power lithium iron phosphate provided by the present invention, in the step 4, the solid matter ratio of the first slurry to the second slurry is (0.5-1.5):1.

[0022] The mixture is ground and mixed for 30 minutes to 2 hours, spray-dried, calcined in an inert atmosphere at 750 to 800° C. for 20 to 25 hours, and air flow crushed and sieved to obtain a finished high-density power-type lithium iron phosphate positive electrode material.

[0023] Compared with the prior art, the high-pressure dynamic lithium iron phosphate preparation method provided by the present invention has the following beneficial effects:

[0024] 1. The present invention is based on two commonly used process routes for synthesizing lithium iron phosphate, namely, the ferrous phosphate method and the ferrous oxalate method. The two slurries are combined in the ball milling stage and spray sintered in one step to achieve uniform mixing at the submicron level. The lithium iron phosphate particles generated by ferrous oxalate can be evenly distributed between the particles generated by iron phosphate to achieve particle grading, thereby improving compaction.

[0025] 2. In the present invention, the powder is pre-sintered in step 1, and a dispersant and a grinding aid are added in step 2, which also has the effect of improving compaction.

[0026] 3. The lithium iron phosphate prepared by the present invention has an obvious bimodal particle size distribution, with one peak at 500-800nm ​​and one peak at about 2μm. Its compacted density is greater than 2.72g / cm3, and it has good power performance, and its 0.5C discharge capacity is greater than 146mAh / g.

[0027] 4. Low cost, no need for new equipment. DETAILED DESCRIPTION

[0028] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.

[0029] Embodiment 1:

[0030] Step 1: Add ferrous oxalate and lithium dihydrogen phosphate into a ball mill at a molar ratio of Li:Fe=1:0.98, ball mill for 30 minutes until the particle size is 2-4 μm, spray dry to obtain a spray material, and calcine the spray material at 500°C for 5 hours to obtain a first powder.

[0031] Step 2: Add the first powder and methanol into a ball mill at a ratio of 1 kg / 5 L, add oleic acid as a dispersant and spherical PP as a first carbon source at 2% and 5% of the mass of the first powder, respectively, and ball mill for 1 hour to obtain a first slurry.

[0032] Step 3: Add iron phosphate and lithium bicarbonate into a ball mill at a molar ratio of Li:Fe=1:0.96, and the total mass of iron phosphate and lithium bicarbonate is 5 times the mass of the first powder. Then, glucose is added as a second carbon source at 5% of the total mass of iron phosphate and lithium bicarbonate. Ball mill for 3 hours in a methanol medium to make the slurry particle size reach 1-2 μm to obtain a second slurry.

[0033] Step 4: While the second slurry is being stirred continuously, the first slurry is introduced into the second slurry. The mixture is stirred for 1 hour, and spray-dried to obtain a spray material. The spray material is calcined at 800° C. in a nitrogen atmosphere for 24 hours to obtain a lithium iron phosphate positive electrode material.

[0034] Embodiment 2:

[0035] Step 1: Add ferrous oxalate and lithium dihydrogen phosphate into a ball mill at a molar ratio of Li:Fe=1:0.98, and ball mill for 30 minutes until the particle size is 2-4 μm; add methanol at a ratio of 1 kg / 5 L of the total mass of ferrous oxalate and lithium dihydrogen phosphate, add oleic acid and spherical PP carbon source at 2% and 5% of the total mass respectively, and ball mill for 1 hour to obtain the first slurry.

[0036] Step 2: Add iron phosphate and lithium bicarbonate into a ball mill at a molar ratio of Li:Fe=1:0.96, the total mass of iron phosphate and lithium bicarbonate is 5 times the total mass of ferrous oxalate and lithium dihydrogen phosphate, and then add glucose at 5% of the total mass of iron phosphate and lithium bicarbonate, and ball mill for 3 hours in a methanol medium to make the slurry particle size reach 1-2 μm to obtain a second slurry.

[0037] Step 3: While the second slurry is being stirred continuously, the first slurry is introduced into the second slurry. The mixture is stirred for 1 hour, and spray dried to obtain a spray material. The spray material is calcined at 800° C. in a nitrogen atmosphere for 24 hours to obtain a lithium iron phosphate positive electrode material.

[0038] Embodiment 3:

[0039] Step 1: Add ferrous oxalate and lithium dihydrogen phosphate into a ball mill at a molar ratio of Li:Fe=1:0.98, ball mill for 30 minutes until the particle size is 2-4 μm, spray dry to obtain a spray material, and calcine the spray material at 500°C for 5 hours to obtain a first powder.

[0040] Step 2: Add the first powder and methanol into a ball mill at a ratio of 1 kg / 5 L, and ball mill for 1 h to obtain a first slurry.

[0041] Step 3: Add iron phosphate and lithium bicarbonate into a ball mill at a molar ratio of Li:Fe=1:0.96, and the total mass of iron phosphate and lithium bicarbonate is 5 times the mass of the first powder. Then add glucose at 5% of the total mass of iron phosphate and lithium bicarbonate, and ball mill for 3 hours in a methanol medium to make the slurry particle size reach 1-2 μm to obtain a second slurry.

[0042] Step 4: While the second slurry is being stirred continuously, the first slurry is introduced into the second slurry. The mixture is stirred for 1 hour, and spray-dried to obtain a spray material. The spray material is calcined at 800° C. in a nitrogen atmosphere for 24 hours to obtain a lithium iron phosphate positive electrode material.

[0043] It should be noted that in the above three embodiments:

[0044] Example 1 is a lithium iron phosphate prepared according to the method of the present invention, with a compaction of 2.73 and an obvious bimodal distribution, one peak at 500-800nm ​​and one peak at about 2μm;

[0045] In Example 2, the first slurry and the second slurry are directly mixed and calcined to prepare lithium iron phosphate with a compaction of 2.65 and a weak bimodal distribution;

[0046] In Example 3, no dispersant and grinding aid PP were added in step 2, and the compaction of the prepared lithium iron phosphate was 2.62, without a bimodal distribution, and the particle grading effect was not achieved.

[0047] The comparison of the above three embodiments illustrates the effect of pre-sintering the first powder and the dispersant and grinding aid on the preparation of high-density lithium iron phosphate, but does not represent the optimal solution.

[0048] The above descriptions are merely embodiments of the present invention and are not intended to limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made using the contents of the present invention specification, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.

Claims

1. A method for preparing high-density power lithium iron phosphate, characterized in that: The following steps are involved: Step 1: Based on ferrous oxalate, a phosphorus source and a lithium source are added, and the first powder is obtained by ball milling, drying and calcining; Step 2: ball-milling the first powder, the first carbon source and the dispersant with methanol as the medium to obtain a first slurry; Step 3: Based on iron phosphate, a lithium source and a second carbon source are added, and methanol is used as a medium to obtain a second slurry through ball milling; Step 4: The first slurry and the second slurry are mixed, and after drying, calcination and crushing, a finished high-density power-type lithium iron phosphate positive electrode material is obtained.

2. The method for preparing high-density power type lithium iron phosphate according to claim 1, characterized in that: In the step 1, ferrous oxalate and lithium dihydrogen phosphate are added at a molar ratio of Li:Fe of 1:(0.97-0.99).

3. The method for preparing high-density power type lithium iron phosphate according to claim 2, characterized in that: In the step 1, ball milling is performed for 30 to 60 minutes to a particle size of 2 to 4 μm, and after spray drying, calcination is performed at 400 to 500° C. for 3 to 6 hours to obtain the first powder.

4. The method for preparing high-density power type lithium iron phosphate according to claim 1, characterized in that: In the step 2, the first carbon source is added at a ratio of 2 to 6% of the mass of the first powder, the dispersant is added at a ratio of 1 to 5% of the mass of the first powder, and methanol is added at a ratio of 1 kg / 5 L of the mass of the first powder; The first slurry is obtained by ball milling for 1 to 3 hours.

5. The method for preparing high-density power type lithium iron phosphate according to claim 4, characterized in that: In step 2, the first carbon source is PP, which is spherical in shape and has a particle size of less than 10 μm; the dispersant is one or more of ethylene glycol, stearic acid, oleic acid, sodium fatty alcohol sulfate, and carboxy betaine.

6. The method for preparing high-density power type lithium iron phosphate according to claim 1, characterized in that: In the step 3, iron phosphate and lithium bicarbonate are added at a molar ratio of Li:Fe of 1:(0.95-0.98), and the total mass of iron phosphate and lithium bicarbonate is 4-7 times that of the first powder; the second carbon source is added at a ratio of 2-6% of the total mass of iron phosphate and lithium bicarbonate, and methanol is added at a ratio of 1 kg / 5 L of the total mass of iron phosphate and lithium bicarbonate.

7. The method for preparing high-density power type lithium iron phosphate according to claim 6, characterized in that: In the step 3, the ball milling treatment is performed for 2 to 4 hours until the particle size is 1 to 2 μm, thereby obtaining the second slurry.

8. The method for preparing high-density power type lithium iron phosphate according to claim 7, characterized in that: In step 3, the second carbon source is one or more of glucose, sucrose, citric acid, ascorbic acid, and polyethylene glycol 400-800.

9. The method for preparing high-density power type lithium iron phosphate according to claim 1, characterized in that: In the step 4, the solid matter ratio of the first slurry to the second slurry is (0.5-1.5):

1.

10. The method for preparing high-density power type lithium iron phosphate according to claim 9, characterized in that: In the step 4, the mixture is ground and mixed for 30 minutes to 2 hours, spray-dried, calcined in an inert atmosphere at 750 to 800° C. for 20 to 25 hours, and air flow crushed and sieved to obtain a finished high-density power-type lithium iron phosphate positive electrode material.

Citation Information

Patent Citations

  • Method for preparing high-compaction lithium iron phosphate material

    CN109336079A

  • High-compaction lithium iron phosphate material and preparation method thereof

    CN111217347A

  • Method for preparing high-compaction lithium iron phosphate positive electrode material based on airflow regulation

    CN117756079A

Cited By

  • High-energy density type lithium iron phosphate positive electrode material and preparation method thereof

    CN120637450A