High-rate graphene hard carbon composite material and preparation method thereof
By directly loading nanosheet-shaped graphene on the hard carbon surface of biomass, forming a high-ratio graphene hard carbon composite material, the problem of poor rate of hard carbon materials is solved, and the first Coulomb efficiency and rate performance of lithium-ion batteries are significantly improved.
Patent Information
- Application Number
- CN202411317141.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-20
- Publication Date
- 2024-11-12
AI Technical Summary
The existing hard carbon materials have poor effect on improving the rateability of lithium-ion batteries, and graphene particles are prone to accumulate in hard carbon materials, and no advantageous structural matching is formed.
Using natural basswood as carbon source, biomass hard carbon materials are prepared by calcination, and nanosheet-shaped graphene is generated by plasma-enhanced chemical vapor deposition method, which is directly loaded on the surface of biomass hard carbon to form a high-magnification graphene hard carbon composite Material.
The conductivity and rate performance of the material have been improved, and the first discharge specific capacity has been increased from 324.3mAh g-1 to 609.7mAh g-1, and the first effect has been increased to 75.2%, and the discharge specific capacity has been increased by 3.7 times at 10C maximization.
Smart Images

Figure CN118929642A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of graphite hard carbon materials, and particularly relates to a high-rate graphene hard carbon composite material and a preparation method thereof. Background Art
[0002] Lithium-ion batteries have the advantages of high voltage, high specific energy and long cycle life. In recent years, they have been applied to many fields such as electronic consumer products, electric vehicles, and smart medical care. Lithium-ion batteries are mainly composed of positive electrodes, negative electrodes and separators. Among them, positive and negative electrode materials and separators have a crucial impact on the electrochemical performance of lithium-ion batteries.
[0003] As the requirements for power density, energy density and life of lithium-ion batteries increase, the negative electrode materials used in lithium-ion batteries are required to have higher specific capacity, fast charge and discharge performance and large interlayer spacing. Among them, hard carbon material is a kind of amorphous carbon that is difficult to graphitize, with a large interlayer spacing, low expansion and high specific surface area. As the negative electrode material of lithium-ion batteries, it has a stable structure, long service life, and good rate performance, which can meet the requirements of high-power charging and discharging of lithium batteries for electric vehicles. Among them, biomass carbon, as a precursor of hard carbon, has the advantages of high specific capacity, abundant sources, low cost, and abundant active sites. However, the pores on the surface of biomass carbon easily absorb moisture and oxygen in the air, forming various CH functional groups that are easy to react with lithium ions, reducing the initial charge and discharge efficiency and specific capacity of lithium-ion batteries.
[0004] In order to meet the performance requirements of lithium-ion batteries, researchers usually modify hard carbon materials. For example, the patent with publication number CN102820455A discloses a hard carbon negative electrode material for lithium-ion batteries and its preparation method. Silicon and phosphorus are doped into the hard carbon negative electrode material to increase the specific capacity of the material. However, due to the characteristics of silicon and phosphorus materials themselves, the rate performance of lithium-ion batteries is not greatly improved. For example, the patent application with publication number CN106206047A adds graphene particles to the hard carbon material, and the prepared hard carbon composite material has good conductivity and high power density. However, this patent directly adds graphene particles to the hard carbon material. In the modified material obtained by this method, the graphene particle sheets and the hard carbon material do not form an advantageous structure, and the graphene particle sheets are easy to accumulate. Therefore, it is necessary to select a better method to prepare the hard carbon composite material. Summary of the invention
[0005] The present invention aims to provide a high-rate composite hard carbon material and a preparation method thereof, so as to solve the problem that the existing hard carbon materials have poor effect in improving the rate performance of lithium-ion batteries.
[0006] A high-rate graphene hard carbon composite material in this scheme, the graphene hard carbon material is prepared by calcining natural basswood as a carbon source to obtain a biomass hard carbon material, and then generating uniform and dense nano-sheet graphene through plasma enhanced chemical vapor deposition, and then loading the generated nano-sheet graphene onto the surface of biomass hard carbon.
[0007] The method for preparing a high-rate graphene hard carbon composite material of the present invention comprises the following steps:
[0008] S1. Basking the basswood in alkaline liquid for a certain period of time, washing it to neutrality, and then drying it;
[0009] S2, calcining the dried basswood under nitrogen protection to prepare biomass hard carbon material;
[0010] S3, generating nano-sheet graphene by plasma enhanced chemical vapor deposition, and loading the generated nano-sheet graphene onto the surface of the biomass hard carbon material in S2 to obtain the graphene-hard carbon composite material.
[0011] Further, the specific operation of S1 is as follows:
[0012] S1-1, put basswood into 2~3mol L -1 of NaOH and 0.2-0.4 mol L -1 Na 2 SO 3 The mixed solution was reacted in a water bath at 100°C for 3-5 hours, and then washed with deionized water until neutral;
[0013] S1-2, put the basswood into the H2O solution with a pH of 8-10 and a concentration of 1-3%. 2 O 2 The solution is reacted in a 100°C water bath for 1 to 6 hours. After the reaction is completed, the obtained basswood is washed with deionized water until it is neutral and dried at 100°C to 120°C for 8 to 10 hours.
[0014] Furthermore, the calcination temperature in S2 is 800-1000° C., and the calcination time is 2-4 hours.
[0015] Furthermore, the temperature rise program of S2 is 2-5℃ min -1 The heating rate was increased to 520 °C, N 2 The flow rate is 80-100 sccm, keep warm for 1-2 hours, then heat at 5-8℃ min -1 The heating rate is increased to 800-1000°C and kept at this temperature for 1-2 hours.
[0016] Further, the specific steps of S3 are as follows:
[0017] S3-1, placing the prepared biomass hard carbon material in a quartz tube, and heating it to 1000° C. in an argon atmosphere;
[0018] S3-2, pass CH 4 The reaction mixture was kept at 1000°C for 15-30 min and then naturally cooled to room temperature under an argon atmosphere.
[0019] Further, the flow rate of argon gas in S3-1 is 80-100 sccm; the CH 4 The flow rate is 20 to 50 sccm.
[0020] The beneficial technical effect of the present invention is: the present invention uses natural basswood as a carbon source, prepares biomass hard carbon material by calcination, and synthesizes biomass hard carbon with rich micro-mesoporous structure and rich specific surface area. 4 Graphene nanosheets generated by pyrolysis at high temperature are directly loaded on the surface of biomass hard carbon. There is good bonding strength between graphene and hard carbon, and the addition of graphene improves the conductivity of the material, effectively improving the first coulombic efficiency and rate performance of the composite hard carbon. The first discharge capacity of the improved hard carbon composite material increased from 324.3 mAh g -1 Increased to 609.7mAh g -1 , the first efficiency is increased to 75.2%. At a high rate of 10C, the discharge capacity of the improved hard carbon composite material is still 126mAh g -1 , an increase of 3.7 times. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is a SEM image of biomass hard carbon modified with nano-sheet graphene in Example 1 of the present invention.
[0022] Figure 2 The first charge and discharge curves at 0.1C for the batteries corresponding to Example 1, Example 2 and the comparative example.
[0023] Figure 3 It is a comparison chart of different rates of batteries corresponding to Example 1, Example 2 and the comparative example. DETAILED DESCRIPTION
[0024] The following is further described in detail through specific implementation methods:
[0025] Embodiment 1: A method for preparing a high-rate graphene hard carbon composite material, comprising the following steps:
[0026] S1. Delignification of basswood
[0027] S1-1, immerse basswood in 2 mol L -1NaOH and 0.3 mol L -1 Na 2 SO 3 The mixed solution was reacted in a water bath at 100°C for 4 h, and part of the lignin was removed by alkali boiling. After the reaction, it was washed with deionized water until neutral;
[0028] S1-2, the basswood treated by S1-1 was then placed in H2O with a pH of 9 and a concentration of 2%. 2 O 2 The solution was further used to remove lignin, and the reaction was carried out in a water bath at 100 °C for 2 h. After the reaction, the obtained basswood was washed with deionized water until it was neutral, and dried at 120 °C for 8 h.
[0029] S2. Calcination: Place the dried basswood in a tubular furnace under N 2 The temperature was raised to 800℃ and calcined for 2h under protection to obtain biomass hard carbon material. The specific heating procedure was 3℃ min -1 The heating rate was increased to 520 °C, N 2 The flow rate was 80 sccm, the temperature was kept for 2 h, and then the temperature was increased at 5 °C min -1 The heating rate was raised to 800 °C and kept at this temperature for 2 h;
[0030] S3, generating nano-sheet graphene by plasma enhanced chemical vapor deposition, and directly loading the generated nano-sheet graphene on the surface of the biomass hard carbon material, the specific steps are:
[0031] S3-1. The prepared biomass hard carbon material was placed in a quartz tube and heated to 1000°C in an argon atmosphere with an Ar flow rate of 90 sccm and a heating rate of 25°C min -1 ;
[0032] S3-2, pass CH 4 Gas, CH 4 The flow rate was 30 sccm, and after maintaining at 1000° C. for 25 min, the mixture was naturally cooled to room temperature in an Ar atmosphere to obtain a graphene-hard carbon composite material.
[0033] Embodiment 2: A method for preparing a high-rate graphene hard carbon composite material, comprising the following steps:
[0034] S1. Delignification of basswood
[0035] S1-1, immerse basswood in 2 mol L -1 NaOH and 0.4 mol L -1 Na 2 SO 3 The mixed solution was reacted in a water bath at 100°C for 5 h, and part of the lignin was removed by alkali boiling. After the reaction, it was washed with deionized water until neutral;
[0036] S1-2, the basswood treated by S1-1 was then placed in a solution with a pH of 9 and a concentration of 1% H 2 O 2 The solution was further used to remove lignin, and the reaction was carried out in a water bath at 100°C for 1 h. After the reaction, the obtained basswood was washed with deionized water until it was neutral, and dried at 100°C for 10 h;
[0037] S2. Calcination: Place the dried basswood in a tubular furnace under N 2 The temperature was raised to 900℃ and calcined for 3h under protection to obtain biomass hard carbon material. The specific heating procedure was 5℃ min -1 The heating rate was increased to 520 °C, N 2 The flow rate was 80 sccm, the temperature was kept for 2 h, and then the temperature was increased at 5 °C min -1 The heating rate was raised to 900 °C and kept at this temperature for 3 h;
[0038] S3, directly loading nano-sheet graphene on the surface of biomass hard carbon material by plasma enhanced chemical vapor deposition, the specific steps are:
[0039] S3-1. The prepared biomass hard carbon material was placed in a quartz tube and heated to 1000°C in an argon atmosphere with an Ar flow rate of 100 sccm and a heating rate of 25°C min -1 ;
[0040] S3-2, pass CH 4 Gas, CH 4 The flow rate was 30 sccm, and after maintaining at 1000° C. for 25 min, the mixture was naturally cooled to room temperature in an Ar atmosphere to obtain a graphene-hard carbon composite material.
[0041] The comparative example is different from Example 1 in that the step of directly loading the nano-sheet graphene on the surface of the biomass hard carbon material by plasma enhanced chemical vapor deposition in S3 is not performed.
[0042] Experimental testing:
[0043] 1. The high-rate graphene hard carbon composite material prepared in Example 1 is used as the active material, conductive carbon black (SP) is used as the conductive agent, and polyvinylidene fluoride (PVDF) is used as the binder. The composite hard carbon, SP and PVDF are weighed in a mass ratio of 94:3:3. N-methylpyrrolidine copper (NMP) is used as the solvent, and a uniformly mixed slurry is prepared by a planetary disperser, and then the slurry is evenly coated on the composite copper current collector to obtain a negative electrode sheet. The electrode sheet is cut into electrode discs with a diameter of 12 mm and used as the positive electrode for standby. A metal lithium sheet with a diameter of 14 mm is used as the counter electrode, a ceramic diaphragm with a diameter of 16 mm is used as the diaphragm, and 8μL 1mol / L LiPF6 / EC+DMC+DEC (volume ratio 1:1:1) was used as the electrolyte. In an argon-protected glove box, 2023 button half-cells were assembled and capacity and performance tests were carried out.
[0044] 2. The high-rate graphene hard carbon composite material prepared in Example 2 is used as the active material, SP is used as the conductive agent, and PVDF is used as the binder. The composite hard carbon, SP and PVDF are weighed in a mass ratio of 94:3:3. Using NMP as the solvent, a planetary disperser is used to prepare a uniformly mixed slurry, and then the slurry is evenly coated on the composite copper current collector to obtain a negative electrode sheet. The electrode sheet is cut into electrode discs with a diameter of 12 mm and used as the positive electrode for standby use. A metal lithium sheet with a diameter of 14 mm is used as the counter electrode, a ceramic diaphragm with a diameter of 16 mm is used as the diaphragm, and 8μL 1mol / L LiPF 6 / EC+DMC+DEC (volume ratio 1:1:1) was used as the electrolyte. In an argon-protected glove box, 2023 button half-cells were assembled and capacity and performance tests were carried out.
[0045] 3. Use the ordinary graphene hard carbon composite material prepared in the above comparative example as the active material, SP as the conductive agent, and PVDF as the binder, and weigh them according to the mass ratio of composite hard carbon, SP and PVDF of 94:3:3. Use NMP as the solvent, prepare a mixed slurry by a planetary disperser, and then evenly apply the slurry on the composite copper current collector to obtain a negative electrode sheet. Cut the electrode sheet into electrode discs with a diameter of 12 mm and use them as the positive electrode for standby use. Use a metal lithium sheet with a diameter of 14 mm as the counter electrode, a ceramic diaphragm with a diameter of 16 mm as the diaphragm, and 8μL 1mol / L LiPF 6 / EC+DMC+DEC (volume ratio 1:1:1) was used as the electrolyte. In an argon-protected glove box, 2023 button half-cells were assembled and capacity and performance tests were carried out.
[0046] The SEM image of the surface of the biomass hard carbon composite material modified with nano-sheet graphene prepared in Example 1 is as follows: Figure 1 As shown, it can be seen that the nano-sheet graphene is evenly loaded on the surface and pores of the biomass hard carbon without stacking. The addition of nano-graphene improves the conductivity of the material, greatly improving the battery's initial charge and discharge capacity and rate performance.
[0047] The 0.1C first charge and discharge curves of the batteries prepared from the high-rate graphene hard carbon composite materials obtained in Test Example 1 and Example 2 and the materials obtained in the comparative example are as follows: Figure 2As shown, the first charge specific capacity of the battery corresponding to Example 1 and Example 2 is as high as 471.65 mAh / g, and the discharge specific capacity is as high as 608.65 mAh / g, which is much higher than the corresponding data of the battery corresponding to the comparative example.
[0048] The rate performance of the battery prepared by the high-rate graphene hard carbon composite material obtained in Example 1 and Example 2 and the material obtained in the comparative example was tested. Figure 3 As shown. Figure 3 It can be seen that all discharge capacities of the batteries corresponding to Example 1 and Example 2 are much higher than those of the comparative example, indicating that the composite copper current collector prepared by this patent improves the rate performance of the battery. Taking 0.2C as a reference, the reversible specific capacities of the batteries corresponding to Example 1 and Example 2 at 10C are 27.3% of that at 0.2C, which is much higher than that of the comparative example (11.1%).
Claims
1. A high-rate graphene hard carbon composite material, characterized in that: The graphene hard carbon material is prepared by calcining natural basswood as a carbon source to obtain a biomass hard carbon material, then generating nano-sheet graphene by plasma enhanced chemical vapor deposition, and loading the generated nano-sheet graphene onto the surface of the biomass hard carbon.
2. The method for preparing a high-rate graphene hard carbon composite material according to claim 1, characterized in that: The following steps are involved: S1. Basking the basswood in alkaline liquid for a certain period of time, washing it to neutrality, and then drying it; S2, calcining the dried basswood under nitrogen protection to prepare biomass hard carbon material; S3, generating nano-sheet graphene by plasma enhanced chemical vapor deposition, and loading the generated nano-sheet graphene onto the surface of the biomass hard carbon material in S2 to obtain the graphene-hard carbon composite material.
3. The method for preparing a high-rate graphene hard carbon composite material according to claim 2, characterized in that: The specific operations of S1 are as follows: S1-1, put basswood into 2~3mol L -1 of NaOH and 0.2-0.4 mol L -1 Na2SO3 mixed solution, react in a 100℃ water bath for 3-5h, then wash with deionized water until neutral; S1-2. Place basswood in a H2O2 solution with a pH of 8 to 10 and a concentration of 1 to 3%, and react in a 100°C water bath for 1 to 6 hours. After the reaction, wash the basswood with deionized water until it is neutral, and dry it at 100°C to 120°C for 8 to 10 hours.
4. The method for preparing a high-rate graphene hard carbon composite material according to claim 2, characterized in that: The calcination temperature in S2 is 800-1000°C, and the calcination time is 2-4h.
5. The method for preparing a high-rate graphene hard carbon composite material according to claim 4, characterized in that: S2 heating program: 2~5℃ min -1 The heating rate was raised to 520°C with a N2 flow rate of 80-100 sccm, and the temperature was kept at this temperature for 1-2 h, and then the temperature was increased at 5-8°C min -1 The heating rate is increased to 800-1000°C and kept at this temperature for 1-2 hours.
6. The method for preparing a high-rate graphene hard carbon composite material according to claim 2, characterized in that: The specific steps of S3 are as follows: S3-1, placing the prepared biomass hard carbon material in a quartz tube, and heating it to 1000° C. in an argon atmosphere; S3-2, introduce CH4 gas and maintain at 1000°C for 15-30 minutes. After the reaction is completed, cool naturally to room temperature under argon atmosphere.
7. The method for preparing a high-rate graphene hard carbon composite material according to claim 6, characterized in that: The flow rate of argon gas in S3-1 is 80-100 sccm; the flow rate of CH4 in S3-2 is 20-50 sccm.
Citation Information
Patent Citations
Preparation method of hard carbon / graphene composite anode material used in lithium battery
CN107732245A
Hard carbon composite material and preparation method thereof
CN110085813A
Graphene nanosheet material, and rapid manufacturing method and application thereof
CN110697693A
Nanocarbon material composite biomass hard carbon electrode material and preparation method and application thereof
CN113044827A
High-capacity rapid charging and discharging graphene and hard carbon composite material, preparation method thereof and application of composite material in sodium-ion battery
CN114156456A
Cited By
Graphene coated hard carbon negative electrode material and preparation method thereof
CN119660717A
Graphene-Coated Hard Carbon Anode Material and Its Preparation Method
CN119660717B