Biomass-based carbon nanotube material for supercapacitor electrode and preparation method of biomass-based carbon nanotube material

The carbon nanotubes are generated in situ in supercapacitors through hydrothermal carbonization and one-step activation methods, which solves the problem of poor conductivity of activated carbon, achieves a balance between conductivity and pore structure, reduces cost and energy consumption, and is suitable for industrial production.

CN118929659AActive Publication Date: 2024-11-12SOUTH CHINA UNIV OF TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411115526.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-12
Estimated Expiration
2044-08-14

AI Technical Summary

Technical Problem

The existing activated carbon for supercapacitors has poor conductivity and requires the use of conductive additives. The traditional preparation method is complex and has high cost.

Method used

Using hydrothermal carbonization technology to synchronize carbon nanotubes in situ without adding transition metal catalysts, biomass-based carbon nanotube materials with excellent pore structure and conductivity are prepared, and cheap biomass raw materials such as fungus and corn starch are used. Hydrothermal carbonization and one-step activation are carried out to generate porous activated carbon and carbon nanotubes.

Benefits of technology

The balance between the conductivity of the material and the pore structure is achieved, the electrochemical performance is significantly improved, the production cost and energy consumption is reduced, and it is suitable for industrial production, and can replace or reduce the use of conductive additives.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929659A_ABST
    Figure CN118929659A_ABST
Patent Text Reader

Abstract

The invention discloses a biomass-based carbon nanotube material for a supercapacitor electrode and a preparation method of the biomass-based carbon nanotube material. Biomasses such as corn starch, pine wood and agaric are used as raw materials, part of light components in the raw materials are removed through a hydrothermal carbonization method, the carbon content of the raw materials is increased, and then the carbon nanotube material is generated through in-situ pyrolysis through a one-step activation method. The carbon nanotube material prepared by the method disclosed by the invention has excellent conductivity and capacitive property in a supercapacitor test. And the conductivity of the obtained carbon nanotube material can be modulated through synthesis conditions, so that the electrochemical performance of the supercapacitor is improved. Besides, the preparation method is simple in process and has an obvious cost advantage, and the obtained biomass-based carbon nanotube material is expected to be widely applied to the field of supercapacitor electrode materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of biomass resource utilization and new energy materials, and specifically relates to a biomass-based carbon nanotube material for supercapacitor electrodes and a preparation method thereof. Background Art

[0002] Supercapacitors are a new type of energy storage device between traditional capacitors and batteries. They have the characteristics of high power density, long cycle life, fast charge and discharge speed, and are suitable for a variety of environments. Therefore, they have been widely used and studied in recent years. Electrode materials are the key to the performance of supercapacitors. Among various electrode materials, activated carbon has become the mainstream due to its large specific surface area, adjustable pores, good conductivity and low price. Large specific surface area and good pore structure can provide abundant active sites to improve the specific capacitance of activated carbon materials; however, the developed pore structure will destroy the graphitized structure of the material, resulting in reduced conductivity. Excellent conductivity helps to reduce internal resistance and thus increase power density. The reduction of capacitor internal resistance can also reduce internal heating and extend the cycle life of supercapacitors. In this regard, people usually add carbon materials such as acetylene black, graphene, and carbon nanotubes in the electrode preparation step to improve its conductivity, but this undoubtedly increases the cost and preparation process of the electrode. Therefore, it is necessary to develop an electrode material that takes into account both excellent conductivity and capacitance for the application and promotion of supercapacitors.

[0003] Patent CN 109887760 A discloses "A kind of highly conductive activated carbon and its preparation and use", which uses polymer pre-oxidized silk as a template, heats to 500-1200°C in a carrier gas and keeps for a period of time, then introduces water or CO2 for activation and pore formation. The disadvantages of this method are high raw material costs and harsh process conditions. CN 109850892 A discloses "A kind of highly conductive coconut shell activated carbon for supercapacitors by double activation industrial preparation", which obtains porous activated carbon by physical activation and then reacts multiple times in a CO2 atmosphere to remove surface functional groups, then acid washes and removes functional groups again in an inert atmosphere. Although this method reduces the resistivity, the process is too complicated. In summary, it is of great significance to find a method for preparing supercapacitor electrode materials that has a simple process, low production cost and meets actual needs. Summary of the invention

[0004] The present invention aims to solve the problem that the existing activated carbon for supercapacitors has poor conductivity and needs to use conductive additives, and provides a method for preparing biomass-based carbon nanotubes for supercapacitor electrodes. The method of the present invention generates carbon nanotubes in situ in synchronization with the activation pore-forming process without the addition of an external transition metal catalyst, and finally obtains a biomass-based carbon nanotube material with excellent pore structure and conductivity. In addition, the hydrothermal carbonization technology used in the present invention also reduces energy consumption and environmental pollution.

[0005] The present invention adopts the following technical solution:

[0006] A method for preparing a biomass-based carbon nanotube material for a supercapacitor electrode comprises the following steps:

[0007] (1) grinding the biomass raw material to 10-400 mesh, placing the ground biomass and alkali solution in a hydrothermal reactor according to a set mass ratio, mixing them evenly and then performing hydrothermal carbonization treatment, after the reaction is completed, cooling to room temperature, taking out, drying, and grinding to obtain a precursor;

[0008] (2) placing the precursor obtained in step (1) and the activator in a set mass ratio in a beaker, adding deionized water, stirring thoroughly, drying, and then grinding thoroughly;

[0009] (3) placing the mixture obtained in step (2) in a tubular furnace, removing the air in the tube and heating it at a certain heating rate to perform a pyrolysis reaction, and cooling it to room temperature after the reaction is completed to obtain a crude product containing carbon nanotubes;

[0010] (4) The crude product obtained in step (3) is purified by acid washing, filtered, washed with water until neutral, and dried to obtain a pure target product.

[0011] Furthermore, in step (1), the biomass raw material is wood ear and also includes one or more of corn starch and pine wood, and the weight of wood ear in the raw material accounts for at least 5%.

[0012] Furthermore, in step (1), the alkali solution is a sodium carbonate or sodium bicarbonate solution with a pH of 7 to 11, and the mass ratio of the biomass to the alkali solution is 1:1-10.

[0013] Furthermore, in step (1), the temperature of the hydrothermal carbonization treatment is 150-300° C., and the time of the hydrothermal carbonization treatment is 2-6 hours.

[0014] Furthermore, in step (2), the activator is one or more of KOH, K2CO3, and C6H5K3O7.

[0015] Furthermore, in step (2), the mass ratio of the precursor to the activator is 1:1-4.

[0016] Furthermore, in step (2), the stirring time is 1 to 18 hours.

[0017] Furthermore, in step (2), the drying temperature is 50-150° C. and the drying time is 12-24 hours.

[0018] Furthermore, in step (3), argon gas is introduced to remove the air in the tube.

[0019] Furthermore, in step (3), the pyrolysis reaction is heated to 500-1000°C at a heating rate of 5-20°C / min and maintained for 1-3h.

[0020] The biomass-based carbon nanotube material obtained by the above preparation method has excellent conductivity and capacitance and has broad application prospects in the field of supercapacitors.

[0021] The preparation of supercapacitor electrodes using the above-mentioned biomass-based carbon nanotube material specifically includes the following steps:

[0022] The biomass-based carbon nanotube material and the binder polyvinylidene fluoride (PVDF) are mixed in a mass ratio of 90:10, and fully ground in an agate mortar to obtain a mixture. An appropriate amount of solvent N-methyl-2-pyrrolidone (NMP) is added and mixed evenly to form a slurry, which is dried in a vacuum drying oven at 100° C. to a water-free state, and cooled to room temperature to obtain an electrode material.

[0023] The principle of the present invention is as follows:

[0024] The present invention uses cheap wood ear, corn starch, pine and other biomass as raw materials. First, the light components such as hemicellulose, cellulose and lignin in the raw materials are decomposed in the hydrothermal carbonization process to generate smaller fragments, and then dehydration and decarboxylation reactions occur to increase the C / H and C / O ratios and the carbon content of the raw materials. The alkaline substances can promote the hydrothermal carbonization reaction. In the one-step activation process, KOH, K2CO3 and other K-containing +The etching action of alkaline substances activates the precursor to form pores, and porous activated carbon materials are obtained. At the same time, since wood ear itself is rich in iron, during the high-temperature pyrolysis process, free carbon species will generate porous carbon nanotubes under the synergistic catalytic action of Fe-K. The porous structure is conducive to the storage of charges, and carbon nanotubes can significantly improve the conductivity of the material. In biomass-based activated carbon / carbon nanotube materials, activated carbon is the main body, and the charge storage mainly depends on its large specific surface and pore structure. However, with the development of the pore structure, the degree of graphitization of the material decreases, and the conductivity decreases. It is usually necessary to add conductive additives such as acetylene black to improve the conductivity of the material. The in-situ generated carbon nanotubes can effectively enhance the conductivity of the material, achieve a balance between the pore structure and the conductivity, and thus replace or reduce the use of conductive additives.

[0025] Compared with the existing invention technology, the beneficial effects of the present invention are as follows:

[0026] 1. The present invention takes into account the pore structure and conductivity of carbon materials, significantly improving the electrochemical performance of the materials. The total pore volume of the materials is about 0.6-0.9cm 3 / g, and the specific surface area is about 1300~2000m 2 / g, when the current density is 1A / g, the specific capacitance reaches 270~340F / g.

[0027] 2. The present invention prepares biomass-based carbon nanotube supercapacitor electrode materials based on hydrothermal carbonization and one-step activation method. The raw materials are cheap, the process equipment is simple, the pressure on the environment is small, the energy consumption is saved, the actual requirements are met, and it is suitable for industrial production.

[0028] 3. The present invention prepares multi-walled carbon nanotubes (tube diameter of about 20 to 50 nm and length of about 20 to 40 μm) with a high aspect ratio in situ at an extremely low cost, ensuring that the material has good electrical conductivity, which can replace or reduce the addition of conductive agents such as acetylene black and graphite, thereby reducing the cost of subsequent processes; and the unique flexibility of the carbon nanotube structure helps to cope with volume changes during electrochemical reactions. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 The present invention is a process flow chart for preparing the biomass-based carbon nanotube material.

[0030] Figure 2 This is a scanning electron microscope (SEM) image of the biomass-based carbon nanotube material obtained in Example 1.

[0031] Figure 3 This is the powder X-ray diffraction (XRD) spectrum of the biomass-based carbon nanotube material obtained in Example 1.

[0032] Figure 4The constant current charge and discharge curves of the supercapacitor electrode assembled with the biomass-based carbon nanotube material obtained in Example 1 at different current densities.

[0033] Figure 5 The impedance Nyquist diagram of the supercapacitor electrode assembled based on the materials obtained in Example 1, Comparative Example 1 and Comparative Example 2. DETAILED DESCRIPTION

[0034] The present invention is described below with reference to specific examples. It will be appreciated by those skilled in the art that these examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention in any way.

[0035] The experimental methods in the following examples are conventional methods unless otherwise specified. The reagents and materials used in the following examples are commercially available products unless otherwise specified.

[0036] Figure 1 This is a process flow chart of the biomass-based carbon nanotube supercapacitor electrode material prepared in an embodiment of the present invention. Corn starch, pine wood, fungus and other biomass are used as raw materials, and a precursor is obtained after a hydrothermal carbonization process with an alkali solution; the precursor is then immersed and stirred in an activator to activate and form pores to obtain a porous activated carbon material; a porous carbon nanotube crude product is then generated in situ through high-temperature pyrolysis, and finally acid washing and purification are performed to obtain a pure target product, namely AC / CNTs.

[0037] Example 1

[0038] according to Figure 1 The process shown is to prepare a biomass-based carbon nanotube material and assemble a supercapacitor electrode. The specific steps are as follows:

[0039] The dried pine and fungus raw materials with a mass ratio of 3:1 were mixed, crushed and ground to 100 mesh, and the raw materials with a mass ratio of 1:4 and sodium bicarbonate solution (pH=11) were taken in a hydrothermal reactor for hydrothermal carbonization treatment. The hydrothermal temperature was set to 300℃ and the hydrothermal time was 4h. After the reaction was completed, the solid product was taken out after cooling to room temperature, and the precursor was obtained after drying and grinding, wherein the solid yield was 67%. The precursor and KOH were placed in a beaker at a mass ratio of 1:2, and 60mL of deionized water was added and stirred for 12h, then dried in an oven at 100℃ overnight, and then fully ground; the mixture was placed in a tubular furnace, and the air in the tube was discharged and heated to 850℃ at a rate of 5℃ / min, and the reaction was carried out for 1.5h. After the reaction was completed, it was cooled to room temperature; the crude product was acid-washed and purified, and then filtered and washed with water to neutrality, and dried to obtain pure biomass-based carbon nanotube materials.

[0040] Figure 2This is a scanning electron microscope (SEM) image of the biomass-based carbon nanotube material obtained in Example 1. It can be seen that the biomass-based carbon nanotubes prepared by the present invention have good morphology, a tube diameter of about 20 to 50 nm, and a length of about 20 to 40 μm. Figure 3 This is the powder X-ray diffraction (XRD) spectrum of the biomass-based carbon nanotube material obtained in Example 1. It can be seen that the carbon (002) peak of the material is significantly sharper than that of Comparative Example 1, indicating that the generation of carbon nanotubes significantly improves the degree of graphitization of the material, ensuring that the material has excellent electrical conductivity.

[0041] The prepared biomass-based carbon nanotube material and the binder polyvinylidene fluoride (PVDF) were mixed in a mass ratio of 90:10 and fully ground in an agate mortar to obtain a mixture. An appropriate amount of N-methyl-2-pyrrolidone (NMP) was added and mixed evenly to form a slurry, which was dried in a vacuum drying oven at 100°C to an anhydrous state and cooled to room temperature to obtain an electrode material. The obtained electrode material was evenly applied to the front end of the nickel foam as a working electrode, and metal platinum was used as a counter electrode, Hg / HgO as a reference electrode, and a 6mol / L KOH solution as an electrolyte for a three-electrode test.

[0042] Figure 4 The constant current charge and discharge curves of the electrode material at different current densities show that at a current density of 1A / g, its specific capacity is as high as 337F / g. Figure 5 The impedance Nyquist plots of supercapacitor electrodes assembled based on the materials obtained in Example 1, Comparative Example 1 and Comparative Example 2 show that the biomass-based carbon nanotube material prepared by the present invention has smaller internal resistance and higher conductivity when used as an electrode.

[0043] Example 2

[0044] according to Figure 1 The process shown is to prepare a biomass-based carbon nanotube material and assemble a supercapacitor electrode. The specific steps are as follows:

[0045] The dried corn starch and wood ear raw materials with a mass ratio of 3:1 were mixed, crushed and ground to 100 mesh, and the raw materials with a mass ratio of 1:4 and sodium bicarbonate solution (pH=11) were taken in a hydrothermal reactor for hydrothermal carbonization treatment. The hydrothermal temperature was set to 280℃ and the hydrothermal time was 3h. After the reaction was completed, the solid product was taken out after cooling to room temperature, and the precursor was obtained after drying and grinding, wherein the solid yield was 61%. The precursor and KOH were placed in a beaker at a mass ratio of 1:1.5, and 60mL of deionized water was added and stirred for 12h, then dried in an oven at 110℃ overnight, and then fully ground; the mixture was placed in a tubular furnace, and the air in the tube was discharged and heated to 900℃ at a rate of 10℃ / min, reacted for 2h, and cooled to room temperature after the reaction was completed; the crude product was acid-washed and purified, then filtered and washed with water to neutrality, and dried to obtain pure biomass-based carbon nanotube materials.

[0046] The prepared biomass-based carbon nanotube material and the binder polyvinylidene fluoride (PVDF) were mixed in a mass ratio of 90:10 and fully ground in an agate mortar to obtain a mixture. An appropriate amount of N-methyl-2-pyrrolidone (NMP) was added and mixed evenly to form a slurry, which was dried in a vacuum drying oven at 100°C to anhydrous state and cooled to room temperature to obtain the electrode material. The obtained electrode material was evenly applied to the front end of the nickel foam as the working electrode, and metal platinum was used as the counter electrode, Hg / HgO as the reference electrode, and 6mol / L KOH solution as the electrolyte for a three-electrode test. The charge and discharge test results show that at a current density of 1A / g, its specific capacity is as high as 270F / g.

[0047] Example 3

[0048] according to Figure 1 The process shown is to prepare a biomass-based carbon nanotube material and assemble a supercapacitor electrode. The specific steps are as follows:

[0049] The dried pine wood, corn starch and fungus raw materials with a mass ratio of 1.5:1.5:1 were mixed, crushed and ground to 100 mesh, and the raw materials with a mass ratio of 1:5 and sodium bicarbonate solution (pH=11) were taken in a hydrothermal reactor for hydrothermal carbonization treatment. The hydrothermal temperature was set to 280℃ and the hydrothermal time was 6h. After the reaction was completed, the solid product was taken out after cooling to room temperature, and the precursor was obtained after drying and grinding, wherein the solid yield was 58%. The precursor and KOH were placed in a beaker at a mass ratio of 1:3, 60mL of deionized water was added and stirred for 12h, and then dried in an oven at 100℃ overnight, and then fully ground; the mixture was placed in a tubular furnace, and the air in the tube was removed and heated to 900℃ at a rate of 10℃ / min, reacted for 2h, and cooled to room temperature after the reaction was completed; the crude product was acid-washed and purified, and then filtered and washed with water to neutrality, and dried to obtain pure biomass-based carbon nanotube materials.

[0050] The prepared biomass-based carbon nanotube material and the binder polyvinylidene fluoride (PVDF) were mixed in a mass ratio of 90:10 and fully ground in an agate mortar to obtain a mixture. An appropriate amount of N-methyl-2-pyrrolidone (NMP) was added and mixed evenly to form a slurry, which was dried in a vacuum drying oven at 100°C to anhydrous state and cooled to room temperature to obtain the electrode material. The obtained electrode material was evenly applied to the front end of the nickel foam as the working electrode, and metal platinum was used as the counter electrode, Hg / HgO as the reference electrode, and 6mol / L KOH solution as the electrolyte for a three-electrode test. The charge and discharge test results show that at a current density of 1A / g, its specific capacity is as high as 285F / g.

[0051] Comparative Example 1

[0052] The biomass-based activated carbon material was prepared by hydrothermal method and assembled into supercapacitor electrodes. The specific operation steps are as follows:

[0053] The dried pine wood and wood ear raw materials with a mass ratio of 4:0 were mixed, crushed and ground to 100 mesh, and the raw materials with a mass ratio of 1:4 and sodium bicarbonate solution (pH=11) were taken in a hydrothermal reactor for hydrothermal carbonization treatment. The hydrothermal temperature was set to 300°C and the hydrothermal time was 4h. After the reaction was completed, the solid product was taken out after cooling to room temperature, and the precursor was obtained after drying and grinding, wherein the solid yield was 67%. The precursor and KOH were placed in a beaker at a mass ratio of 1:2, and 60mL of deionized water was added and stirred for 12h, then dried in an oven at 100°C overnight, and then fully ground; the mixture was placed in a tubular furnace, and the air in the tube was discharged and heated to 850°C at a rate of 5°C / min, reacted for 1.5h, and cooled to room temperature after the reaction was completed; the crude product was acid-washed and purified, then filtered and washed with water to neutrality, and dried to obtain a pure biomass-based activated carbon material, which was recorded as Comparative Example 1-AC.

[0054] The prepared biomass-based activated carbon material, conductive carbon black and binder polyvinylidene fluoride (PVDF) were mixed in a mass ratio of 80:10:10, and the mixture was fully ground in an agate mortar. An appropriate amount of N-methyl-2-pyrrolidone (NMP) was added and mixed evenly to form a slurry, which was dried to anhydrous state in a vacuum drying oven at 100°C and cooled to room temperature to obtain an electrode material. The obtained electrode material was evenly applied to the front end of the nickel foam as a working electrode, and metal platinum was used as a counter electrode, Hg / HgO as a reference electrode, and a 6mol / L KOH solution as an electrolyte for a three-electrode test. The charge and discharge test results show that at a current density of 1A / g, its specific capacity is only 218F / g, which is much lower than the specific capacity of 337F / g in Example 1. This is because the introduction of wood ear in Example 1 promoted the hydrothermal in situ growth of carbon nanotubes in biomass, effectively enhanced its conductivity, and achieved an effective balance between conductivity and pore structure; at the same time, the generated carbon nanotubes can replace or reduce the addition of conductive agents such as acetylene black and graphite, reducing the cost of subsequent processes.

[0055] Comparative Example 2

[0056] The biomass-based activated carbon material was prepared according to the conventional "carbonization-activation two-step method" and the supercapacitor electrode was assembled. The specific operation steps are as follows:

[0057] The dried pine and fungus raw materials with a mass ratio of 3:1 were mixed, crushed, and ground to 100 mesh, and heated to 500°C at a rate of 5°C / min in a tube furnace, and carbonized for 1.5 hours to obtain a carbonized material. After cooling, the carbonized material with a mass ratio of 1:2 and KOH were placed in a beaker, 60mL of deionized water was added and stirred for 12 hours, and then dried in an oven at 100°C overnight, and then fully ground; the mixture was placed in a tube furnace, and the air in the tube was exhausted and heated to 850°C at a rate of 5°C / min, and reacted for 1.5 hours. After the reaction was completed, it was cooled to room temperature; the crude product was acid-washed and purified, then filtered and washed with water to neutrality, and dried to obtain a pure biomass-based activated carbon material, which was recorded as Comparative Example 2-AC.

[0058] The prepared biomass-based activated carbon material, conductive carbon black and binder polyvinylidene fluoride (PVDF) were mixed in a mass ratio of 80:10:10, and the mixture was fully ground in an agate mortar. An appropriate amount of N-methyl-2-pyrrolidone (NMP) was added and mixed evenly to form a slurry, which was dried to anhydrous state in a vacuum drying oven at 100°C and cooled to room temperature to obtain an electrode material. The obtained electrode material was evenly applied to the front end of the nickel foam as a working electrode, and metal platinum was used as a counter electrode, Hg / HgO as a reference electrode, and a 6mol / L KOH solution as an electrolyte for a three-electrode test. The charge and discharge test results show that at a current density of 1A / g, its specific capacity is only 185F / g, which is much lower than the specific capacity of 337F / g in Example 1. This is because the hydrothermal carbonization method used in Example 1 decomposes light components such as hemicellulose, cellulose and lignin in the raw material during the hydrothermal carbonization process to generate smaller fragments, which then undergo dehydration and decarboxylation reactions and increase the C / H and C / O ratios, thereby increasing the carbon content of the raw material, wherein the alkaline substance can promote the hydrothermal carbonization reaction. In the one-step activation process, the precursor is activated and pore-formed by the etching action of KOH to obtain a porous activated carbon material, which is beneficial to the subsequent high-temperature pyrolysis process, charge storage, and enhanced material conductivity.

Claims

1. A method for preparing a biomass-based carbon nanotube material for supercapacitor electrodes, characterized in that: The steps include: (1) grinding the biomass raw material, placing the ground biomass and alkali solution in a hydrothermal reactor according to a set mass ratio, mixing them evenly and then performing hydrothermal carbonization treatment, after the reaction is completed, cooling to room temperature, taking them out, drying, and grinding them to obtain a precursor; (2) placing the precursor obtained in step (1) and the activator in a set mass ratio in a beaker, adding deionized water, stirring thoroughly, drying, and then grinding thoroughly; (3) placing the mixture obtained in step (2) in a tubular furnace, exhausting the air in the tube and heating it to perform a pyrolysis reaction, and cooling it to room temperature after the reaction is completed to obtain a crude product containing carbon nanotubes; (4) The crude product obtained in step (3) is purified by acid washing, filtered, washed with water until neutral, and dried to obtain a pure target product.

2. The method for preparing a biomass-based carbon nanotube material for supercapacitor electrodes according to claim 1, characterized in that: In step (1), the biomass raw material is wood ear and also includes one or more of corn starch and pine wood, and the weight of wood ear accounts for at least 5% of the raw material.

3. The method for preparing a biomass-based carbon nanotube material for supercapacitor electrodes according to claim 1, characterized in that: In step (1), the alkali solution is a sodium carbonate or sodium bicarbonate solution with a pH of 7 to 11, and the mass ratio of the biomass raw material to the alkali solution is 1:1-10.

4. The method for preparing a biomass-based carbon nanotube material for supercapacitor electrodes according to claim 1, characterized in that: In step (1), the temperature of the hydrothermal carbonization treatment is 150-300° C., and the time of the hydrothermal carbonization treatment is 2-6 hours.

5. The method for preparing a biomass-based carbon nanotube material for supercapacitor electrodes according to claim 1, characterized in that: In step (2), the activator is one or more of KOH, K2CO3, C6H5K3O7.

6. The method for preparing a biomass-based carbon nanotube material for supercapacitor electrodes according to claim 1, characterized in that: In step (2), the mass ratio of the precursor to the activator is 1:1-4.

7. The method for preparing a biomass-based carbon nanotube material for supercapacitor electrodes according to claim 1, characterized in that: In step (2), the drying temperature is 50-150° C. and the drying time is 12-24 hours.

8. The method for preparing a biomass-based carbon nanotube material for supercapacitor electrodes according to claim 1, characterized in that: In step (3), the pyrolysis reaction is heated to 500-1000°C at a heating rate of 5-20°C / min and maintained for 1-3h.

9. A biomass-based carbon nanotube material prepared by the preparation method according to any one of claims 1 to 8.

10. A supercapacitor electrode material, characterized in that: The biomass-based carbon nanotube material according to claim 9 is uniformly mixed with a binder and a solvent to form a slurry, which is then vacuum dried and cooled to obtain the slurry.

Citation Information

Patent Citations

  • Method for preparing carbon nano-tubes by using biological product as catalyst precursor

    CN101891183A

  • Method for producing carbon nanotubes through catalytic pyrolysis of solid carbon materials