Heat treatment method and application of continuously controllable Prussian blue material

Through a continuous controllable heat treatment method using rotary equipment for dynamic heating in a protective atmosphere, the problems of inaccurate temperature control and excessive dehydration rate in traditional heat treatment methods are solved, and the crystallinity and electrochemical properties of Prussian blue materials are improved. Suitable for sodium ion batteries, it achieves the improvement of material stability and production efficiency.

CN118929694APending Publication Date: 2024-11-12湖州超钠新能源科技有限公司

Patent Information

Application Number
CN202410985803.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Traditional heat treatment methods do not accurately control the temperature of Prussian blue materials, and the rapid dehydration rate leads to crystal rupture, which limits its application in sodium ion batteries and has problems of high energy consumption and low production efficiency.

Method used

Using a continuous controllable heat treatment method performed in a protective atmosphere, dynamic heating is performed through a rotating device, which is divided into first heat treatment and second heat treatment. The second heat treatment temperature is higher than the first heat treatment, and the dehydration rate is controlled to avoid crystal rupture, and Suitable for continuous production.

Benefits of technology

It improves the crystallinity and purity of Prussian blue cathode material, enhances electrochemical performance, maintains the morphological consistency and stability of the material, is suitable for the application of sodium ion batteries, and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929694A_ABST
    Figure CN118929694A_ABST
Patent Text Reader

Abstract

The invention discloses a heat treatment method and application of a continuously controllable Prussian blue material. The heat treatment method comprises the following steps: providing a wet Prussian blue material matrix, and carrying out heat treatment on the wet Prussian blue material matrix by using rotary equipment in a protective atmosphere to obtain the heat-treated Prussian blue material, the heat treatment comprises first heat treatment and second heat treatment which are sequentially carried out, and the temperature of the second heat treatment is higher than that of the first heat treatment. The heat treatment method provided by the invention is better in drying uniformity, the dehydration rate in the material can be controlled, crystal breakage caused by too high dehydration rate is avoided, the material structure is protected from being damaged, continuous production can be realized, and industrial amplification is more facilitated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of sodium ion battery materials, and in particular relates to a continuously controllable heat treatment method for Prussian blue materials and an application thereof. Background Art

[0002] With the development of economy and society, the excessive use of fossil energy has led to a sharp decrease in the reserves of non-renewable energy, causing a series of serious problems such as resource depletion and environmental degradation. Therefore, the development and utilization of renewable energy storage technology has become one of the important ways to achieve sustainable development.

[0003] Prussian blue (PB) and its analogs are considered to be promising cathode materials for sodium-ion batteries due to their high theoretical capacity and low cost. However, the practical application of Prussian blue materials is limited by the problem of inevitable introduction of crystal water during their synthesis in aqueous solution. In order to improve these properties, researchers have tried a variety of synthesis and post-treatment techniques, including heat treatment. Traditional heat treatment methods, such as vacuum oven heat treatment, have problems such as high energy consumption, long treatment time, imprecise temperature control, and easy damage to the vacuum pump. In addition, the dehydration rate is too fast, resulting in crystal breakage and material structure damage. These problems limit the industrial development of Prussian blue materials. Therefore, it is necessary to propose a new dehydration method to overcome the above problems. Summary of the invention

[0004] The main purpose of the present invention is to provide a continuous and controllable heat treatment method for Prussian blue materials to overcome the shortcomings of the prior art.

[0005] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention includes:

[0006] One aspect of the present invention provides a continuous and controllable heat treatment method for Prussian blue-based materials, comprising:

[0007] Provide a wet material matrix of Prussian blue type materials;

[0008] In a protective atmosphere, heat-treating the wet Prussian blue material matrix with a rotary device to obtain a heat-treated Prussian blue material;

[0009] The heat treatment includes a first heat treatment and a second heat treatment performed sequentially, and the temperature of the second heat treatment is higher than the temperature of the first heat treatment.

[0010] Another aspect of the present invention provides a Prussian blue material obtained by the aforementioned heat treatment method, wherein the moisture content of the material is less than 1500 ppm.

[0011] Another aspect of the present invention also provides the use of the aforementioned Prussian blue material in a sodium ion battery.

[0012] Another aspect of the present invention also provides a sodium ion battery positive electrode material, which includes the aforementioned Prussian blue material.

[0013] Compared with the prior art, the technical solution of the present invention has at least the following advantages:

[0014] 1) The present invention can significantly improve the crystallinity and purity of the Prussian blue positive electrode material by precisely controlling the heat treatment parameters, thereby improving its electrochemical performance;

[0015] 2) The present invention controls the heat treatment time and furnace pressure of the rotary device, and adopts the rotary device for dynamic heating so that the material is heated more evenly, and the dehydration rate in the material can be controlled to avoid crystal breakage caused by too fast dehydration rate, protect the material structure from damage, and help maintain the consistency and stability of the material morphology;

[0016] 3) The present invention can continuously perform heat treatment, is suitable for continuous production, is beneficial to improve production efficiency and reduce production costs;

[0017] 4) The present invention can achieve customized treatment of Prussian blue materials of different types and requirements by adjusting the heat treatment conditions. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0019] Figure 1 This is a SEM image of the Prussian blue sodium cathode material after treatment in Example 1;

[0020] Figure 2 This is a SEM image of the Prussian blue sodium cathode material after treatment in Example 2;

[0021] Figure 3 This is a SEM image of the Prussian blue sodium cathode material after treatment in Example 3;

[0022] Figure 4 This is a SEM image of the Prussian blue sodium cathode material after treatment in Example 4;

[0023] Figure 5 This is a SEM image of the Prussian blue sodium cathode material after treatment in Example 5;

[0024] Figure 6This is a SEM image of the Prussian blue sodium cathode material after treatment in Example 6;

[0025] Figure 7 This is a SEM image of the Prussian blue sodium cathode material after treatment in Example 7;

[0026] Figure 8 This is a SEM image of the Prussian blue sodium cathode material after treatment in Example 8;

[0027] Fig. 9 This is a SEM image of the Prussian blue sodium cathode material after treatment in Example 9;

[0028] Fig.10 This is the SEM image of the Prussian blue sodium cathode material after treatment in Comparative Example 3. DETAILED DESCRIPTION

[0029] The present invention will be more fully understood by reading the following specific embodiments. However, it should be understood that the specific embodiments disclosed below are only exemplary of the present invention, and the present invention can be embodied in various forms. Therefore, the specific functional details disclosed herein should not be interpreted as limiting, but only as the basis for the claims and as a representative basis for teaching those skilled in the art to adopt the present invention in different ways in any appropriate detailed embodiment.

[0030] As one aspect of the technical solution of the present invention, a continuously controllable heat treatment method of a Prussian blue material includes:

[0031] Provide a wet material matrix of Prussian blue type materials;

[0032] In a protective atmosphere, heat-treating the wet Prussian blue material matrix with a rotary device to obtain a heat-treated Prussian blue material;

[0033] The heat treatment includes a first heat treatment and a second heat treatment performed sequentially, and the temperature of the second heat treatment is higher than the temperature of the first heat treatment.

[0034] In some embodiments, the Prussian blue-based material includes a Prussian blue sodium cathode material synthesized by co-precipitation.

[0035] In some embodiments, the heat treatment method includes: pretreating the Prussian blue material to obtain a wet material matrix of the Prussian blue material.

[0036] Furthermore, the pretreatment includes: washing and filtering the Prussian blue material to obtain a wet material matrix of the Prussian blue material.

[0037] In some embodiments, the moisture content of the Prussian blue material wet matrix is ​​2%-20%, preferably 5%-15%.

[0038] In some embodiments, the first heat treatment is performed at a temperature of 70-150° C. and for a time of 4-15 hours.

[0039] In some preferred embodiments, the temperature of the first heat treatment is 80-130° C. and the time is 5-10 h.

[0040] In some embodiments, the second heat treatment is performed at a temperature of 170-300° C. and for a time of 5-30 h.

[0041] In some preferred embodiments, the second heat treatment is performed at a temperature of 170-280° C. for a time of 8-24 h.

[0042] In some embodiments, the protective atmosphere comprises a nitrogen atmosphere.

[0043] In some embodiments, the pressure within the rotary device is -15-30Pa.

[0044] In some preferred embodiments, the pressure inside the rotary device is -10-20Pa.

[0045] In some embodiments, the rotation speed of the rotary device is 1.5-3.5 r / min.

[0046] In some embodiments, the heat treatment method includes: transferring the wet matrix of the Prussian blue material to a rotary device via an automatic feeding device.

[0047] In some more specific embodiments, the heat treatment method includes:

[0048] S1. Pretreatment: washing and filtering the coprecipitated Prussian blue sodium cathode material to obtain a wet matrix of the Prussian blue sodium cathode material; the moisture content of the wet matrix of the Prussian blue sodium cathode material is controlled at 2%-20%;

[0049] S2. Loading: The pretreated Prussian blue sodium cathode material wet matrix is ​​transferred to the rotary kiln through an automatic feeding device;

[0050] S3. Heat treatment: a Prussian blue sodium cathode material wet material matrix is ​​subjected to a programmed temperature treatment in a rotary kiln, and the programmed temperature, time, protective atmosphere, rotary kiln furnace pressure, etc. are controlled during the programmed temperature treatment to obtain a heat-treated Prussian blue material; the programmed temperature treatment comprises a first stage of temperature treatment and a second stage of temperature treatment performed in sequence, the temperature of the first stage of temperature treatment is 70-150°C, the time is 4-15h; the temperature of the second stage of temperature treatment is 170-300°C, the time is 5-30h; the protective atmosphere is a nitrogen atmosphere; the rotary kiln furnace pressure is controlled at -15-30Pa; the rotation speed of the rotary kiln is 1.5-3.5r / min;

[0051] S4. Post-processing: batch, screen, demagnetize and package the materials after the rotary kiln is cooled to obtain the final product.

[0052] As another aspect of the technical solution of the present invention, it relates to a Prussian blue material obtained by the aforementioned heat treatment method, wherein the moisture content is below 1500ppm, the crystallinity is good, and the particles are intact without breakage. Conventional heat treatment methods use too high a temperature and too fast a dehydration rate, which may lead to particle crystal breakage. The Prussian blue material after heat treatment of the present invention is a complete cubic particle with no cracks or cracks on the surface.

[0053] As another aspect of the technical solution of the present invention, it also involves the application of the aforementioned Prussian blue materials in sodium ion batteries.

[0054] In some embodiments, the application includes: application of the Prussian blue-based material in a positive electrode material for a sodium ion battery.

[0055] In some preferred embodiments, the Prussian blue sodium cathode material subjected to rotary kiln heat treatment is subsequently applied to fields such as two-wheeled electric vehicles and power storage systems, especially two-wheeled low-speed electric vehicles and large-scale energy storage.

[0056] As another aspect of the technical solution of the present invention, it also relates to a sodium ion battery positive electrode material, which includes the aforementioned Prussian blue material.

[0057] The present invention is further described below by way of examples, but the present invention is not limited to the scope of the examples. The reagents and raw materials used in the following examples are commercially available, and the experimental methods without specific conditions are usually carried out under conventional conditions or under conditions recommended by the manufacturers.

[0058] Example 1

[0059] The method of the invention is adopted to post-treat Prussian blue materials. The specific steps include: washing and filtering the Prussian blue sodium positive electrode material synthesized by coprecipitation to obtain a Prussian blue positive electrode material wet material matrix with a water content of 5%, transferring the pretreated Prussian blue positive electrode material wet material matrix to a rotary kiln through an automatic feeding device, performing programmed heating and cooling on the wet material matrix in the rotary kiln, controlling the first stage temperature to be 110° C. for 8 hours and the second stage temperature to be 220° C. for 16 hours during the heat treatment process, introducing nitrogen as a protective gas, controlling the oxygen content in the furnace to drop below 0.2%, controlling the furnace pressure of the rotary kiln to be -10 Pa, and the rotating speed of the rotary kiln to be 2.5 r / min, starting the heat treatment, starting to cool after the heat treatment is completed, and performing batching, screening, demagnetization, packaging and other processes on the materials cooled in the rotary kiln to obtain the final product.

[0060] Example 2

[0061] Compared with Example 1, the difference is that the internal pressure of the rotary kiln furnace is adjusted to 10 Pa.

[0062] Example 3

[0063] Compared with Example 1, the difference is that the internal pressure of the rotary kiln furnace is adjusted to -15 Pa.

[0064] Example 4

[0065] Compared with Example 1, the difference is that the water content of the Prussian blue positive electrode material wet matrix is ​​10%, the first heat treatment temperature is adjusted to 150°C and the insulation time is 10 hours, the second heat treatment temperature is adjusted to 280°C and the insulation time is 24 hours, and the internal pressure of the rotary kiln furnace is 20 Pa.

[0066] Example 5

[0067] Compared with Example 1, the difference is that the first heat treatment temperature is adjusted to 80°C and the insulation time is 10 hours, and the second heat treatment temperature is adjusted to 170°C and the insulation time is 24 hours.

[0068] Example 6

[0069] Compared with Example 1, the difference is that the first heat treatment temperature is adjusted to 80°C and the insulation time is 10 hours, the second heat treatment temperature is adjusted to 170°C and the insulation time is 24 hours, and the internal pressure of the rotary kiln furnace is 30pa.

[0070] Example 7

[0071] The method of the invention is adopted to post-treat Prussian blue materials. The specific steps include: washing and filtering the Prussian blue sodium positive electrode material synthesized by coprecipitation to obtain a Prussian blue positive electrode material wet material matrix with a water content of 2%, transferring the pretreated Prussian blue positive electrode material wet material matrix to a rotary kiln through an automatic feeding device, performing programmed heating and cooling on the wet material matrix in the rotary kiln, controlling the first stage temperature to be 70°C for a heat preservation time of 4 hours and the second stage temperature to be 170°C for a heat preservation time of 30 hours during the heat treatment process, introducing nitrogen as a protective gas, controlling the oxygen content in the furnace to decrease below 0.2%, controlling the furnace pressure of the rotary kiln to be -15 Pa, and the rotating speed of the rotary kiln to be 1.5 r / min, starting the heat treatment, starting to cool after the heat treatment is completed, and performing batching, screening, demagnetization, packaging and other processes on the materials cooled in the rotary kiln to obtain the final product.

[0072] Example 8

[0073] The method of the invention is adopted to post-treat Prussian blue materials. The specific steps include: washing and filtering the Prussian blue sodium positive electrode material synthesized by coprecipitation to obtain a Prussian blue positive electrode material wet material matrix with a water content of 20%, transferring the pretreated Prussian blue positive electrode material wet material matrix to a rotary kiln through an automatic feeding device, performing programmed heating and cooling on the wet material matrix in the rotary kiln, controlling the first stage temperature to be 140°C for a heat preservation time of 15 hours and the second stage temperature to be 300°C for a heat preservation time of 5 hours during the heat treatment process, introducing nitrogen as a protective gas, controlling the oxygen content in the furnace to decrease below 0.2%, controlling the furnace pressure of the rotary kiln to be -15 Pa, and the rotating speed of the rotary kiln to be 3.5 r / min, starting the heat treatment, starting to cool after the heat treatment is completed, and performing batching, screening, demagnetization, packaging and other processes on the materials cooled in the rotary kiln to obtain the final product.

[0074] Example 9

[0075] The method of the invention is adopted to post-treat Prussian blue materials. The specific steps include: washing and filtering the Prussian blue sodium positive electrode material synthesized by coprecipitation to obtain a Prussian blue positive electrode material wet material matrix with a water content of 15%, transferring the pretreated Prussian blue positive electrode material wet material matrix to a rotary kiln through an automatic feeding device, performing programmed heating and cooling on the wet material matrix in the rotary kiln, controlling the first stage temperature to be 130°C for a heat preservation time of 5 hours and the second stage temperature to be 280°C for a heat preservation time of 8 hours during the heat treatment process, introducing nitrogen as a protective gas, controlling the oxygen content in the furnace to decrease below 0.2%, controlling the furnace pressure of the rotary kiln to be -10 Pa, and the rotating speed of the rotary kiln to be 3.5 r / min, starting the heat treatment, starting to cool after the heat treatment is completed, and performing batching, screening, demagnetization, packaging and other processes on the materials cooled in the rotary kiln to obtain the final product.

[0076] Comparative Example 1

[0077] Compared with Example 1, the difference is that the heat treatment equipment is a vacuum drying oven, 220° C., heat treatment is 8 hours, and the vacuum pressure is 20 Pa.

[0078] Comparative Example 2

[0079] Compared with Comparative Example 1, the difference is that the heat treatment time is 12 hours.

[0080] Comparative Example 3

[0081] Compared with Comparative Example 1, the difference is that the heat treatment time is 24 hours.

[0082] Comparative Example 4

[0083] Compared with Example 1, the difference is that only the second stage heat treatment is performed.

[0084] Comparative Example 5

[0085] Compared with Example 1, the difference is that only the first stage heat treatment is performed.

[0086] Comparative Example 6

[0087] Compared with Example 1, the difference is that the furnace pressure is adjusted to -20 Pa.

[0088] Comparative Example 7

[0089] Compared with Example 1, the difference is that the furnace pressure is adjusted to 40 Pa.

[0090] Performance Testing

[0091] The moisture content and electrical properties of the heat-treated materials of Examples 1-9 and Comparative Examples 1-7 were tested. The test results are shown in Tables 1 and 2.

[0092] Battery performance test: The heat-treated materials of Examples 1-9 and Comparative Examples 1-7 were used as positive electrodes and 1 mol / L NaClO 4 / PC∶EMC∶FEC (49∶49∶2) was used as the electrolyte to prepare a sodium ion battery, and the charge and discharge cycle test was carried out. The results are shown in Table 1.

[0093] Water content test: Samples were taken at four different locations on the heat-treated materials of Examples 1-9 and Comparative Examples 1-7, and a moisture test was performed at 250°C using a Karl Fischer titrator. The moisture content was obtained through the test data. The results are shown in Table 2.

[0094] Table 1:

[0095] 0.1c discharge mAh / g cycle Retention rate % Example 1 166.33 100 laps 94.76% Example 2 164.16 100 laps 93.65% Example 3 160.52 100 laps 91.11% Example 4 163.07 100 laps 92.32% Example 5 162.97 100 laps 92.25% Example 6 160.22 100 laps 90.67% Example 7 159.23 100 laps 90.24% Example 8 160.12 100 laps 90.84% Example 9 165.24 100 laps 94.54% Comparative Example 1 144.75 100 laps 84.55% Comparative Example 2 150.9 100 laps 87.35% Comparative Example 3 152.18 100 laps 88.12% Comparative Example 4 146.73 100 laps 80.78% Comparative Example 5 140.18 100 laps 83.23% Comparative Example 6 144.85 100 laps 84.36% Comparative Example 7 154.19 100 laps 81.36%

[0096] Table 2:

[0097]

[0098] SEM Testing

[0099] The SEM images of the materials treated in Examples 1-9 of the present invention and Comparative Example 3 were compared. Fig.10 As shown, it can be seen that when the water is quickly removed, the material treated in Comparative Example 3 has particle breakage, while the material treated by heat treatment of the present invention (such as Figures 1 to 9 The particles shown are complete cubic particles with no cracks or fissures on the surface.

[0100] In addition, the inventors of this case also referred to the aforementioned embodiments and conducted experiments with other raw materials, process operations, and process conditions described in this specification, and obtained relatively ideal results.

[0101] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A continuous and controllable heat treatment method for Prussian blue materials, It is characterized in that include: Provide a wet material matrix of Prussian blue type materials; In a protective atmosphere, heat-treating the wet Prussian blue material matrix with a rotary device to obtain a heat-treated Prussian blue material; The heat treatment includes a first heat treatment and a second heat treatment performed sequentially, and the temperature of the second heat treatment is higher than the temperature of the first heat treatment.

2. The continuous and controllable heat treatment method for Prussian blue materials according to claim 1, It is characterized in that The Prussian blue material includes a Prussian blue sodium positive electrode material synthesized by co-precipitation.

3. The continuous and controllable heat treatment method for Prussian blue materials according to claim 1, It is characterized in that include: Pre-treating the Prussian blue material to obtain a wet material matrix of the Prussian blue material; Preferably, the pretreatment comprises: washing and filtering the Prussian blue material to obtain a wet material matrix of the Prussian blue material; And / or, the moisture content of the Prussian blue material wet matrix is ​​2%-20%, preferably 5%-15%.

4. The continuous and controllable heat treatment method for Prussian blue materials according to claim 1, It is characterized in that The temperature of the first heat treatment is 70-150°C, preferably 80-130°C, and the time is 4-15h, preferably 5-10h; And / or, the temperature of the second heat treatment is 170-300°C, preferably 170-280°C, and the time is 5-30h, preferably 8-24h.

5. The continuous and controllable heat treatment method for Prussian blue materials according to claim 1, It is characterized in that The protective atmosphere includes a nitrogen atmosphere.

6. The continuous and controllable heat treatment method for Prussian blue materials according to claim 1, It is characterized in that The pressure in the rotary device is -15-30Pa, preferably -10-20Pa; And / or, the rotation speed of the rotary device is 1.5-3.5r / min.

7. The continuous and controllable heat treatment method for Prussian blue materials according to claim 1, It is characterized in that include: The wet material matrix of the Prussian blue material is transferred to the rotary equipment through an automatic feeding device.

8. A Prussian blue material obtained by the heat treatment method according to any one of claims 1 to 7, wherein the water content of the material is 1500 ppm or less.

9. Use of the Prussian blue material according to claim 8 in a sodium ion battery, preferably, the use include: Application of the Prussian blue material in positive electrode materials of sodium ion batteries; Preferably, the sodium ion battery is a battery for a two-wheeled electric vehicle or a power storage system.

10. A sodium ion battery cathode material, It is characterized in that The invention comprises the Prussian blue material as described in claim 9.

Citation Information

Patent Citations

  • Prussian blue analogue and preparation method, negative electrode material and application thereof

    CN112694104A

  • Dehydration system of lithium ion battery positive electrode material precursor and method for preparing positive electrode material precursor

    CN114695880A

  • Preparation method of sodium ion battery positive electrode Prussian blue material

    CN116375054A

  • Preparation method of Prussian blue analogue sodium ion battery positive electrode material

    CN116588953A

  • Baking method of Prussian blue positive plate

    CN118016821A

Cited By

  • Prussian blue analogue sodium ion positive electrode material and preparation method thereof

    CN121247841A