Method for producing high-quality potassium chloride by utilizing low-grade potassium salt minerals

By combining cold decomposition-rough flotation with hot dissolution crystallization, the problems of high energy consumption and resource waste in the production of potassium chloride from low-grade potash minerals have been solved, achieving efficient and low-cost potassium chloride production and full utilization of resources.

CN118929699APending Publication Date: 2024-11-12GOLMUD ZANGGE POTASH FERTILIZER CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411205551.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing technologies for producing potassium chloride from low-grade potash minerals suffer from high energy consumption, high costs, and complex processes, and also result in insufficient utilization of potassium resources.

Method used

The method employs a combination of cold decomposition-rough flotation and hot dissolution crystallization, which improves the grade of potassium chloride and reduces energy consumption through steps such as hydrolysis, flotation, hot dissolution, concentration and crystallization. It also utilizes natural energy for evaporation, reducing the number of equipment and the floor space required.

Benefits of technology

This technology enables the production of high-quality potassium chloride, reduces production energy consumption and costs, minimizes potassium resource waste, meets the requirements of circular economy and resource utilization, and has broad application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929699A_ABST
    Figure CN118929699A_ABST
Patent Text Reader

Abstract

The invention provides a method for producing high-quality potassium chloride by using low-grade potassium salt minerals, and relates to the technical field of salt lake resource synthesis, and the method comprises the following steps: taking low-grade carnallite or low-grade sylvite as a raw material, crushing the carnallite, and performing ball milling and crushing on the sylvite; carnallite or sylvinite ore pulp is fed into a stirring crystallizer to be hydrolyzed or decomposed; flotation treatment: adding a flotation agent into the underflow ore pulp of the stirring crystallizer, carrying out flotation, and carrying out solid-liquid separation on flotation froth to obtain crude potassium ore; the method comprises the following steps: putting crude potassium ore into a hot melting tank, adding fresh water and mother liquor, heating hot melting slurry through steam, and enabling the dissolved slurry to overflow to a thickener; solid particles are settled in the concentrator, the potassium clear liquid overflows to a crystallizer for cooling crystallization, and potassium chloride crystals are obtained; and dehydrating the potassium chloride slurry through a belt filter and a centrifugal machine to finally obtain a high-quality potassium chloride product. According to the method, production energy consumption is remarkably reduced, and the recovery rate and product quality of potassium chloride are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of comprehensive salt lake resources, in particular to a method for producing high-quality potassium chloride by utilizing low-grade potassium salt minerals. Background Art

[0002] Potassium fertilizer is one of the important factors related to my country's agricultural security. The Qarhan Salt Lake is the main production base of potassium fertilizer in my country. However, in the process of drying carnallite for many years, it is inevitable that a large amount of low-grade carnallite products will accumulate. In addition, when the flotation tailings are added to the brine to produce potassium chloride, when the flotation tailings are introduced into the evaporation pond and dried to the brine at point E, a large amount of potassium salt ore will be produced in the evaporation pond. When this type of ore is produced by cold decomposition positive flotation method, the workshop recovery rate and product grade cannot meet the national standards. In order to avoid wasting these resources and further utilize these potassium resources, the hot solution crystallization method is used to produce potassium chloride products, but this method has the problems of high production energy consumption, high cost and complex process.

[0003] Therefore, it is necessary to provide a method for producing potassium chloride using low-grade potassium salt minerals, which can not only reduce economic investment but also provide an efficient method for recovering potassium chloride. Summary of the invention

[0004] Based on the above problems, the present invention proposes a method for producing high-quality potassium chloride using low-grade potassium salt minerals. The specific technical scheme is as follows:

[0005] A method for producing high-quality potassium chloride using low-grade potassium salt minerals comprises the following steps:

[0006] (1) The low-grade potassium salt mineral used in the technical solution is used as a raw material to produce high-quality potassium chloride, wherein the potassium salt mineral is low-grade carnallite or low-grade sylvite.

[0007] (2) If the raw material is low-grade carnallite, the low-grade carnallite is crushed into small pieces and sent to a stirred crystallizer for hydrolysis.

[0008] (3) If the raw material is low-grade sylvite, the sylvite is directly put into a ball mill for crushing to obtain a slurry with a particle size of less than 0.2 mm. The crushed sylvite is then put into a stirred crystallizer for decomposition.

[0009] (4) Add octadecylamine, No. 2 oil and hydrochloric acid to the underflow pulp of the stirred crystallizer in step (2) or (3), send it to the flotation tank, and perform flotation in the flotation tank. The roughing foam passes through a belt filter to obtain a crude potash ore.

[0010] (5) The crude potassium ore obtained in step (4) is placed in a hot melt tank, and fresh water and mother liquor are added. The hot melt tank heats the hot melt slurry by hot water or steam. In the hot melt tank, potassium chloride dissolves into the liquid phase, while most of the sodium chloride and insoluble matter remain in the solid phase. The dissolved slurry overflows to the concentrator.

[0011] (6) In the concentrator, the solid particles in the slurry settle to the bottom of the concentrator to form a slurry layer. The liquid on the upper layer becomes the supernatant (potassium clear liquid). The supernatant overflows into the potassium clear liquid tank and is then pumped to the crystallizer for further processing.

[0012] (7) The potassium clear liquid is cooled and crystallized in a crystallizer to precipitate potassium chloride crystals to obtain potassium chloride slurry. The unprecipitated portion of the solution after cooling and crystallization is collected in a low-temperature mother liquor tank and reused as the mother liquor in step (5).

[0013] (8) The potassium chloride slurry at the bottom of the crystallizer is transported to a belt filter and a centrifuge through a slurry pump to remove a large amount of water. The potassium chloride crystals after centrifugation are sent to a drying drum and a fluidized bed for drying and dehydration, and finally a high-quality potassium chloride product is obtained.

[0014] Furthermore, in the above step (2), the content of KCl in the low-grade carnallite is 5.29-13.62%, the content of NaCl is 10.23-77.39%, the content of MgCl2 is 3.89-36.11%, the content of CaSO4 is 0.57-9.43%, and the content of H2O is 0.6-46.72%;

[0015] Furthermore, in the above step (3), the content of KCl in the low-grade sylvite is 6.81-19.91%, the content of NaCl is 38.33-77.12%, the content of MgCl2 is 1.51-17.66%, the content of CaSO4 is 0.97-10.90%, and the content of H2O is 7.14-31.12%.

[0016] Furthermore, in the stirred crystallizer underflow slurry in the above step (2) or step (3), the KCl content in the liquid phase is less than 4.2%, and the MgCl2 content is less than 4.0%; the KCl content in the solid phase is less than 1.2%.

[0017] Furthermore, in the crude potassium ore after flotation dehydration in the above step (4), the content of KCl is 19.92-52.5%, the content of NaCl is 31.57-67.78%, the content of MgCl2 is 0.48-5.98%, the content of CaSO4 is 0.36-14.95%, and the content of H2O is 1.1-19.71%.

[0018] Furthermore, the liquid separated by the belt filter in the above step (4) is collected in a mother liquid tank for reflux to the ball mill, stirred crystallizer and flotation tank for recycling.

[0019] Furthermore, in the above step (5), the heat source for heating the hot melt slurry in the hot melt tank is steam from the boiler room, which heats the material temperature to 95° C. and the heating steam pressure is 0.40 MPa.

[0020] Furthermore, the crystallizer in the above step (7) is a three-stage vacuum flash crystallizer, and a DTB crystallizer is used throughout the three-stage flash crystallization process.

[0021] Furthermore, in the potassium chloride product in the above step (8), the content of KCl is greater than 97%, the content of NaCl is not higher than 2%, the content of MgCl2 is not higher than 0.3%, the content of CaSO4 is not higher than 0.3%, and the content of H2O is not higher than 1.5%.

[0022] On the other hand, the present invention also provides a system for preparing high-quality potassium chloride using the above method, comprising:

[0023] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0024] (1) The present invention adds cold decomposition-rough flotation before the hot melt crystallization method to improve the grade of potassium chloride used as the raw material of the hot melt method. By improving the grade of potassium chloride, the energy consumption of the hot melt process is reduced, which is a technology for energy saving and consumption reduction;

[0025] (2) The present invention adds cold decomposition-coarse flotation to increase the processing capacity of a single unit of potassium chloride produced by the hot solution method, reduce the number of the same equipment, reduce the equipment footprint, and thus reduce investment. At the same time, it can also solve the environmental protection problem. When the present invention is used in the Chaerhan Salt Lake area in Qinghai, it can make full use of natural energy for evaporation without consuming other energy, thus reducing the production cost and being a green technology;

[0026] (3) The present invention utilizes the carnallite ore which cannot be used by cold decomposition positive flotation, which not only reduces the waste of potassium resources, but also meets the requirements of reduction, reuse and resource utilization of circular economy. Potassium resources can be fully utilized, and has broad application prospects in the development of salt lake potassium resources. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 It is a process flow chart in an embodiment of the present invention. DETAILED DESCRIPTION

[0028] The present invention provides a method for producing high-quality potassium chloride by using low-grade carnallite, comprising the following steps:

[0029] (1) Low-grade carnallite is first hydrolyzed, and then octadecylamine No. 2 oil and hydrochloric acid are added for flotation. The rough selected foam is separated and dehydrated by a belt filter. The dehydrated potassium salt is conveyed to the hot melt system by a belt conveyor;

[0030] (2) If the raw material is potassium salt, it is crushed to less than 0.2 mm by a ball mill, and then octadecylamine oil No. 2 and hydrochloric acid are added for flotation. The coarsely selected foam is separated and dehydrated by a belt filter, and the potassium salt obtained after dehydration is conveyed to the hot melt system by a belt conveyor.

[0031] (3) The potassium salt after flotation dehydration is put into a hot melt tank and dissolved with fresh water and mother liquor, so that potassium chloride is dissolved in the liquid phase, and most of the sodium chloride and insoluble matter are present in the solid phase. The hot melt tank slurry overflows to the concentrator.

[0032] (4) The bottom flow slurry of the concentrator is transported to the salt centrifuge for solid-liquid separation. The solid tail salt is transported to the tail salt pile by a belt, and the liquid phase returns to the concentrator. The potassium clear liquid in the concentrator overflows into the potassium clear liquid tank and is then pumped to the crystallizer for flash crystallization to precipitate potassium chloride crystals.

[0033] (5) The potassium chloride slurry at the bottom of the crystallizer is transported to a belt filter and a centrifuge through a slurry pump to remove a large amount of water, and then sent to a drying drum and a fluidized bed for drying and dehydration to obtain high-quality potassium chloride.

[0034] Preferably, the low-grade carnallite in step (1) has a KCl content of 5.29-13.62%, a NaCl content of 10.23-77.39%, a MgCl2 content of 3.89-36.11%, a CaSO4 content of 0.57-9.43%, and a H2O content of 0.6-46.72%.

[0035] Preferably, the low-grade sylvite in step (2) has a KCl content of 6.81-19.91%, a NaCl content of 38.33-77.12%, a MgCl2 content of 1.51-17.66%, a CaSO4 content of 0.97-10.90%, and a H2O content of 7.14-31.12%;

[0036] Preferably, the crude potassium ore after flotation dehydration in step (3) has a KCl content of 19.92-52.5%, a NaCl content of 31.57-67.78%, a MgCl2 content of 0.48-5.98%, a CaSO4 content of 0.36-14.95%, and a H2O content of 1.1-19.71%;

[0037] Preferably, in step (3), after the sylvite enters the hot dissolution tank, the material temperature needs to be heated to above 95°C.

[0038] Preferably, in step (5), the outlet temperature of the potassium chloride slurry at the bottom of the crystallizer is ≤36°C.

[0039] Preferably, the high-quality potassium chloride in step (5) is characterized by: a KCl content of greater than 97%, a NaCl content of ≤2%, a MgCl2 content of ≤0.3%, a CaSO4 content of ≤0.3%, and a H2O content of ≤1.5%;

[0040] Example 1

[0041] This embodiment is a method for producing high-quality potassium chloride using low-grade carnallite in the Chaerhan Salt Lake area of ​​Qinghai. The specific process flow is shown in Figure 1 , including the following steps:

[0042] (1) The content of KCl in low-grade carnallite is 13.78%, the content of NaCl is 21.27%, the content of MgCl2 is 34.74%, the content of CaSO4 is 1.19%, and the content of H2O is 29.02%. The low-grade carnallite is crushed in the ore loading bin and transported to the crystallizer via a belt conveyor. The crystallizer tank is provided with a stirrer. Fresh water is added to the crystallizer for mixing to obtain a mixed slurry, which is stirred and decomposed for crystallization for more than 2 hours;

[0043] (2) After decomposition, the liquid phase composition of the crystallizer underflow slurry is 3.85% KCl, 19.34% NaCl, 3.97% MgCl2, 0.91% CaSO4, and 71.83% H2O. The solid phase composition is 1.14% KCl, 69.85% NaCl, 21.22% MgCl2, 0.75% CaSO4, and 7.04% H2O;

[0044] (3) transferring the mixed slurry after stirring, decomposing and crystallizing to a flotation tank, adding octadecylamine, No. 2 oil and hydrochloric acid for flotation, separating and dehydrating the coarsely selected foam by a belt filter, and conveying the dehydrated sylvite to a hot melt system via a belt conveyor; the dehydrated sylvite has a KCl content of 52.5%, a NaCl content of 31.57%, a MgCl2 content of 2.91%, a CaSO4 content of 3.02%, and a H2O content of 10%;

[0045] (4) The potassium salt ore from the belt conveyor enters the potassium dissolving tank. The potassium salt ore is dissolved in the hot dissolving tank at a controlled rate using fresh water and mother liquor, so that potassium chloride is dissolved into the liquid phase, sodium chloride and insoluble matter enter the solid phase, and the hot dissolving tank overflows to the concentrator.

[0046] (5) The potassium clear liquid in the concentrator overflows into the potassium clear liquid tank and is then pumped to the crystallizer. After cooling and crystallization in the three-stage crystallizer, potassium chloride crystals are obtained. The bottom flow solid phase is pumped into the centrifuge for dehydration by a slurry pump. The solid phase after centrifugation is conveyed to the outside of the system by a belt, and the liquid phase after centrifugation returns to the concentrator.

[0047] (6) The potassium chloride crystals at the bottom of the crystallizer are pumped onto a belt filter through a slurry pump to remove a large amount of water, and then sent to a wet refined potassium centrifuge to obtain refined potassium through centrifugal separation. The refined potassium is sent to a drying drum for drying and dehydration to obtain high-quality potassium chloride.

[0048] According to Example 1, in the process of producing 1 ton of high-purity potassium chloride, the hot dissolution time in the hot dissolution tank is 2.25 hours, and the natural gas consumption is 198.4m 3 The electricity consumption is 497.3kWh, and the total energy consumption is equivalent to 325.67kg of standard coal, showing a high energy utilization efficiency.

[0049] The chemical composition of the final product of this embodiment is shown in Table 1.

[0050] Example 2

[0051] This embodiment is a method for producing high-quality potassium chloride using low-grade carnallite in the Chaerhan Salt Lake area of ​​Qinghai, comprising the following steps:

[0052] (1) The content of KCl in low-grade carnallite is 5.29%, the content of NaCl is 32.047%, the content of MgCl2 is 36.11%, the content of CaSO4 is 0.57%, and the content of H2O is 25.99%. The low-grade carnallite is crushed in the ore loading bin and transported to the crystallizer via a belt conveyor. The crystallizer tank is provided with a stirrer. Fresh water is added to the crystallizer for mixing to obtain a mixed slurry, which is stirred for decomposition and crystallization for more than 2 hours;

[0053] (2) After decomposition, the liquid phase composition of the crystallizer underflow slurry is 3.75% KCl, 20.87% NaCl, 3.62% MgCl2, 0.64% CaSO4, and 71.12% H2O. The solid phase composition is 0.79% KCl, 69.34% NaCl, 19.53% MgCl2, 0.81% CaSO4, and 9.53% H2O;

[0054] (3) The mixed slurry after stirring, decomposing and crystallizing is transferred to a flotation tank, and octadecylamine, No. 2 oil and hydrochloric acid are added for flotation. The coarsely selected foam is separated and dehydrated by a belt filter, and the sylvite obtained after dehydration is conveyed to a hot melt system by a belt conveyor; the content of KCl in the dehydrated sylvite is 19.92%, the content of NaCl is 67.78%, the content of MgCl2 is 1.78%, the content of CaSO4 is 2.2%, and the content of H2O is 8.32%.

[0055] (4) The potassium salt ore from the belt conveyor enters the potassium dissolving tank. The potassium salt ore is dissolved in the hot dissolving tank at a controlled rate using fresh water and mother liquor, so that potassium chloride is dissolved into the liquid phase, sodium chloride and insoluble matter enter the solid phase, and the hot dissolving tank overflows to the concentrator.

[0056] (5) The potassium clear liquid in the concentrator overflows into the potassium clear liquid tank and is then pumped to the crystallizer. After cooling and crystallization in the three-stage crystallizer, potassium chloride crystals are obtained. The bottom flow solid phase is pumped into the centrifuge for dehydration by a slurry pump. The solid phase after centrifugation is conveyed to the outside of the system by a belt, and the liquid phase after centrifugation returns to the concentrator.

[0057] (6) The potassium chloride crystals at the bottom of the crystallizer are pumped onto a belt filter through a slurry pump to remove a large amount of water, and then sent to a wet refined potassium centrifuge to obtain refined potassium through centrifugal separation. The refined potassium is sent to a drying drum for drying and dehydration to obtain high-quality potassium chloride.

[0058] In Example 2, the hot dissolution time in the hot dissolution tank during the production of 1 ton of high-purity potassium chloride is 2.25 hours, and the energy consumption is: natural gas consumption is 202.7m 3 The electricity consumption is 502.1kWh, and the total energy consumption is equivalent to 330.15kg of standard coal.

[0059] The chemical composition of the final product of this embodiment is shown in Table 1.

[0060] Example 3

[0061] This embodiment is a method for preparing carnallite raw material by using flotation tailings and salt pan brine in the Chaerhan Salt Lake area of ​​Qinghai, comprising the following steps:

[0062] (1) The content of KCl in low-grade carnallite is 9.59%, the content of NaCl is 17.03%, the content of MgCl2 is 45.43%, the content of CaSO4 is 2.56%, and the content of H2O is 25.39%. The low-grade carnallite is crushed in the ore loading bin and transported to the crystallizer via a belt conveyor. The crystallizer tank is provided with a stirrer. Fresh water is added to the crystallizer for mixing to obtain a mixed slurry, which is stirred and decomposed for crystallization for more than 2 hours;

[0063] (2) After decomposition, the crystallizer underflow slurry was taken, and the liquid phase composition had a KCl content of 3.69%, a NaCl content of 20.11%, a MgCl2 content of 3.16%, a CaSO4 content of 0.79%, and a H2O content of 72.25%; the solid phase composition had a KCl content of 1.2%, a NaCl content of 70.09%, a MgCl2 content of 20.09%, a CaSO4 content of 0.65%, and a H2O content of 7.92%;

[0064] (3) The mixed slurry after stirring, decomposing and crystallizing is transferred to a flotation tank, and octadecylamine, No. 2 oil and hydrochloric acid are added for flotation. The coarsely selected foam is separated and dehydrated by a belt filter, and the sylvite obtained after dehydration is conveyed to a hot melt system by a belt conveyor; the content of KCl in the dehydrated sylvite is 27.54%, the content of NaCl is 55.85%, the content of MgCl2 is 2.77%, the content of CaSO4 is 2.36%, and the content of H2O is 11.48%.

[0065] (4) The potassium salt ore from the belt conveyor enters the potassium dissolving tank. The potassium salt ore is dissolved in the hot dissolving tank at a controlled rate using fresh water and mother liquor, so that potassium chloride is dissolved into the liquid phase, sodium chloride and insoluble matter enter the solid phase, and the hot dissolving tank overflows to the concentrator.

[0066] (5) The potassium clear liquid in the concentrator overflows into the potassium clear liquid tank and is then pumped to the crystallizer. After cooling and crystallization in the three-stage crystallizer, potassium chloride crystals are obtained. The bottom flow solid phase is pumped into the centrifuge for dehydration by a slurry pump. The solid phase after centrifugation is conveyed to the outside of the system by a belt, and the liquid phase after centrifugation returns to the concentrator.

[0067] (6) The potassium chloride crystals at the bottom of the crystallizer are pumped onto a belt filter through a slurry pump to remove a large amount of water, and then sent to a wet refined potassium centrifuge to obtain refined potassium through centrifugal separation. The refined potassium is sent to a drying drum for drying and dehydration to obtain high-quality potassium chloride.

[0068] In Example 3, the hot dissolution time in the hot dissolution tank during the production of 1 ton of high-purity potassium chloride is 2.25 hours, and the energy consumption is: natural gas consumption is 205.9m 3 The electricity consumption is 509.8kWh, and the total energy consumption is equivalent to 337.11kg standard coal.

[0069] The chemical composition of the final product of this embodiment is shown in Table 1.

[0070] Example 4

[0071] This embodiment is a method for preparing high-quality potassium chloride using low-grade sylvite, comprising the following steps:

[0072] (1) The content of KCl in low-grade sylvite is 15.32%, the content of NaCl is 49.78%, the content of MgCl2 is 10.21%, the content of CaSO4 is 5.09%, and the content of H2O is 19.60%. The low-grade sylvite is directly put into a ball mill for crushing to obtain a slurry with a particle size of less than 0.20 mm. The crushed sylvite slurry is sent to a stirred crystallizer for decomposition. Fresh water is added to the stirred crystallizer, and the stirring decomposition crystallization is performed for more than 2 hours;

[0073] (2) After decomposition, the liquid phase composition of the crystallizer underflow slurry is 3.85% KCl, 19.34% NaCl, 3.97% MgCl2, 0.91% CaSO4, and 71.83% H2O. The solid phase composition is 1.14% KCl, 69.85% NaCl, 21.22% MgCl2, 0.75% CaSO4, and 7.04% H2O;

[0074] (3) The mixed slurry after stirring, decomposing and crystallizing is transferred to a flotation tank, and octadecylamine, No. 2 oil and hydrochloric acid are added for flotation. The coarsely selected foam is separated and dehydrated by a belt filter, and the sylvite obtained after dehydration is conveyed to a hot melt system by a belt conveyor; the content of KCl in the dehydrated sylvite is 45.25%, the content of NaCl is 30.57%, the content of MgCl2 is 5.02%, the content of CaSO4 is 4.95%, and the content of H2O is 14.21%.

[0075] (4) The potassium salt ore from the belt conveyor enters the potassium dissolving tank. The potassium salt ore is dissolved in the hot dissolving tank at a controlled rate using fresh water and mother liquor, so that potassium chloride is dissolved into the liquid phase, sodium chloride and insoluble matter enter the solid phase, and the hot dissolving tank overflows to the concentrator.

[0076] (5) The potassium clear liquid in the concentrator overflows into the potassium clear liquid tank and is then pumped to the crystallizer. After cooling and crystallization in the three-stage crystallizer, potassium chloride crystals are obtained. The bottom flow solid phase is pumped into the centrifuge for dehydration by a slurry pump. The solid phase after centrifugation is conveyed to the outside of the system by a belt, and the liquid phase after centrifugation returns to the concentrator.

[0077] (6) The potassium chloride crystals at the bottom of the crystallizer are pumped onto a belt filter through a slurry pump to remove a large amount of water, and then sent to a wet refined potassium centrifuge to obtain refined potassium through centrifugal separation. The refined potassium is sent to a drying drum for drying and dehydration to obtain high-quality potassium chloride.

[0078] In Example 4, the hot dissolution time in the hot dissolution tank during the production of 1 ton of high-purity potassium chloride is 2.25 hours, and the energy consumption is: natural gas consumption is 208.6m 3 The electricity consumption is 514.5kWh, and the total energy consumption is equivalent to 341.98kg of standard coal.

[0079] The chemical composition of the final product of this embodiment is shown in Table 1.

[0080] Comparative Example 1

[0081] This comparative example is a method for preparing high-quality potassium chloride using low-grade sylvite, comprising the following steps:

[0082] The content of KCl in low-grade sylvite is 15.32%, the content of NaCl is 49.78%, the content of MgCl2 is 10.21%, the content of CaSO4 is 5.09%, and the content of H2O is 19.60%. The low-grade sylvite is directly put into a ball mill for crushing to obtain a slurry with a particle size of less than 0.20 mm;

[0083] The crushed potassium salt slurry is directly placed in the hot dissolution tank for hot dissolution treatment. Fresh water and steam are added to the hot dissolution tank, and the material is heated to 95°C with a steam pressure of 0.40MPa. During the hot dissolution process, potassium chloride dissolves into the liquid phase, while most of the sodium chloride and insoluble matter remain in the solid phase. The dissolved slurry overflows to the concentrator.

[0084] In the concentrator, the solid particles in the slurry settle to the bottom of the concentrator to form a slurry layer. The liquid on the upper layer becomes the supernatant (potassium clear liquid). The supernatant overflows into the potassium clear liquid tank and is then pumped to the crystallizer for further processing.

[0085] The potassium clear liquid is cooled and crystallized in a crystallizer to precipitate potassium chloride crystals to obtain potassium chloride slurry.

[0086] The potassium chloride slurry at the bottom of the crystallizer is passed through a belt filter and a centrifuge to remove a large amount of water. The potassium chloride crystals after centrifugation are sent to a drying drum for drying and dehydration to finally obtain potassium chloride products.

[0087] In this comparative example 1, the conventional process is used to directly process low-grade potassium salt. The melting time of the hot melting tank is 4 hours in the process of producing 1 ton of high-purity potassium chloride. The energy consumption is: natural gas consumption is 398.2m 3 The electricity consumption is 998.4kWh, and the total energy consumption is equivalent to 695.45kg standard coal.

[0088] Table 1 Chemical composition of the final products of each embodiment

[0089]

[0090] By comparing Examples 1 to 4 with Comparative Example 1, it can be seen that to produce one ton of 97% KCl product: the thermal dissolution time of Examples 1 to 4 is 2.25 hours, while Comparative Example 1 requires 4 hours, showing the advantage of the present invention in time efficiency; by comparing the energy consumption, it is shown that the present invention significantly reduces energy consumption.

Claims

1. A method for producing high-quality potassium chloride using low-grade potassium salt minerals, characterized in that: The following steps are involved: (1) The low-grade potassium salt mineral is low-grade carnallite or low-grade sylvite; (2) When the low-grade potassium salt mineral is low-grade carnallite, the low-grade carnallite is crushed into small pieces, and the pieces are sent into a stirred crystallizer for hydrolysis to obtain a stirred crystallizer underflow slurry; (3) When the low-grade potassium salt mineral is low-grade potassium rock salt, the potassium rock salt is ground by a ball mill to obtain a slurry with a particle size of less than 0.2 mm, and the slurry is introduced into a stirred crystallizer for decomposition to obtain a stirred crystallizer underflow slurry; (4) adding octadecylamine, No. 2 oil and hydrochloric acid to the underflow slurry of the stirred crystallizer described in step (2) or step (3), feeding the slurry into a flotation tank, performing flotation in the flotation tank to obtain a roughing foam, and dehydrating the roughing foam through a belt filter to obtain a crude potash ore; (5) placing the crude potassium ore described in step (4) into a hot dissolution tank, and adding fresh water and mother liquor, the hot dissolution tank heats the hot dissolution slurry by hot water or steam, and the dissolved slurry overflows to the concentrator; (6) In the concentrator, the solid particles in the slurry settle to the bottom of the concentrator to form a slurry layer, and the liquid on the upper layer is the supernatant, which overflows into the potassium clear liquid tank and is then pumped to the crystallizer for further processing; (7) the potassium clear liquid is cooled and crystallized in a crystallizer to precipitate potassium chloride crystals to obtain potassium chloride slurry, and the unprecipitated portion of the solution after cooling and crystallization is collected into a low-temperature mother liquor tank and reused as the mother liquor in step (5); (8) The potassium chloride slurry at the bottom of the crystallizer is transported to a belt filter and a centrifuge through a slurry pump, and the obtained potassium chloride crystals are dried and dehydrated to finally obtain a potassium chloride product.

2. The method for producing high-quality potassium chloride using low-grade potassium salt minerals according to claim 1, characterized in that: The low-grade carnallite described in step (2) has a KCl content of 5.29-13.62%, a NaCl content of 10.23-77.39%, a MgCl2 content of 3.89-36.11%, a CaSO4 content of 0.57-9.43%, and a H2O content of 0.6-46.72%.

3. The method for producing high-quality potassium chloride using low-grade potassium salt minerals according to claim 1, characterized in that: In the above step (3), the content of KCl in the low-grade sylvite is 6.81-19.91%, the content of NaCl is 38.33-77.12%, the content of MgCl2 is 1.51-17.66%, the content of CaSO4 is 0.97-10.90%, and the content of H2O is 7.14-31.12%.

4. The method for producing high-quality potassium chloride using low-grade potassium salt minerals according to claim 1, characterized in that: The stirred crystallizer underflow slurry described in step (2) or step (3) has a KCl content in the liquid phase of less than 4.2%, a MgCl2 content of less than 4.0%; and a KCl content in the solid phase of less than 1.2%.

5. The method for producing high-quality potassium chloride using low-grade potassium salt minerals according to claim 1, characterized in that: The crude potassium ore in step (4) has a KCl content of 19.92-52.5%, a NaCl content of 31.57-67.78%, a MgCl2 content of 0.48-5.98%, a CaSO4 content of 0.36-14.95%, and a H2O content of 1.1-19.71%.

6. The method for producing high-quality potassium chloride using low-grade potassium salt minerals according to claim 1, characterized in that: The liquid separated by the belt filter in step (4) is collected in a mother liquor tank for reflux to the ball mill, stirred crystallizer and flotation tank for recycling.

7. The method for producing high-quality potassium chloride using low-grade potassium salt minerals according to claim 1, characterized in that: In step (5), the heat source for heating the hot melt slurry in the hot melt tank is steam from the boiler room, which heats the material temperature to 95° C. and the heating steam pressure is 0.40 MPa.

8. The method for producing high-quality potassium chloride using low-grade potassium salt minerals according to claim 1, characterized in that: The crystallizer in step (7) is a three-stage vacuum flash crystallizer, and a DTB crystallizer is used throughout the three-stage flash crystallization process.

9. The method for producing high-quality potassium chloride using low-grade potassium salt minerals according to claim 1, characterized in that: The potassium chloride product in step (8) has a KCl content greater than 97%, a NaCl content not higher than 2%, a MgCl2 content not higher than 0.3%, a CaSO4 content not higher than 0.3%, and a H2O content not higher than 1.5%.

10. A system for producing high-quality potassium chloride using low-grade potassium salt minerals according to any one of claims 1 to 9, characterized in that: The following equipments are connected in sequence: a stirring crystallizer, a blending tank, a flotation tank, a crude potassium ore belt filter, a crude potassium ore feeding belt, a hot dissolution tank, a concentrator, a potassium clear liquid tank, a crystallizer, a potassium chloride crystal belt filter, a centrifuge, a drying drum, and a fluidized bed; Among them, a ball mill is also provided at the front end of the stirred crystallizer, a mother liquor tank is provided at the rear end of the crude potassium ore belt filter, and a low-temperature mother liquor tank and a steam heat exchanger are also provided between the crystallizer and the hot dissolution tank.

Citation Information

Cited By

  • Process for producing high-quality potassium chloride by using carnallite ore

    CN121181011A