Method for preparing high-purity alpha-Al2O3 from supercritical boiler fly ash by aluminum sulfate salting-out method

Through the supercritical boiler aluminum sulfate salting method, combined with sulfuric acid method and hydrochloric acid method, the purification process was repeated, and the problems of low purity and high cost of alumina extraction in fly ash were solved, and the low purity of high α-Al2O3 was achieved Cost extraction simplifies process flow and reduces energy consumption.

CN118929716AActive Publication Date: 2024-11-12HAINAN UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411173683.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-12
Estimated Expiration
2044-08-26

AI Technical Summary

Technical Problem

The existing acid leaching method for extracting alumina from fly ash is dissolved in impurities such as sodium, magnesium and calcium, resulting in poor product purity, high cost and complex process, which limits market-oriented applications.

Method used

The supercritical boiler fly ash aluminum sulfate salting method was used to mix and leaching with sulfuric acid after ball milling, and perform multiple solid-liquid separations, hydrogen chloride gas precipitation, hydrochloric acid washing and pyrolysis. Combined with sulfuric acid and hydrochloric acid method, repeated purification was obtained to obtain high Pure α-Al2O3.

Benefits of technology

Low-cost and high-purity α-Al2O3 extraction is achieved, with simple process, low energy consumption and good safety, reducing production costs, and overcoming the problems of high leaching and large residue volume in the prior art.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929716A_ABST
    Figure CN118929716A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of coal-based solid waste high-value recycling, and particularly relates to a method for preparing high-purity alpha-Al2O3 through a supercritical boiler fly ash aluminum sulfate salting-out method. Research finds that in the precipitation reaction process, the yield of aluminum chloride hexahydrate crystals is in direct proportion to the concentration of Cl <-> in a reaction solution. According to the method, the properties of aluminum chloride hexahydrate are utilized, impurities in aluminum chloride are removed, and high-purity alpha-Al2O3 is obtained through repeated precipitation and purification. According to the method, the sulfuric acid method and the hydrochloric acid method are combined, the high-purity alpha-Al2O3 is extracted from the fly ash, and the method is low in cost, low in energy consumption, easy to operate, good in safety and high in product additional value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of high-value resource utilization of coal-based solid waste, and specifically relates to a method for preparing high-purity α-Al by a supercritical boiler fly ash aluminum sulfate salting method. 2 O 3 method. Background Art

[0002] During the combustion process of coal, a large amount of solid waste - fly ash - is generated. The fly ash produced has low activity and is difficult to use effectively. Therefore, most of it is directly discarded, and only a small part is used in low-value products such as fillers in construction and engineering. This not only makes the utilization rate of coal-based solid waste low, but also has low added value, resulting in a waste of resources. Later, researchers tried to extract residual metal minerals from fly ash, which not only can realize the resource utilization of fly ash, but also has significant economic and ecological benefits. At present, the main methods for extracting alumina from fly ash include activated sintering method, alkali method, acid leaching method and acid-base combined method.

[0003] Among them, the acid leaching method mainly uses hydrochloric acid or sulfuric acid leaching. This method has the advantages of simple process and mild conditions. However, metal components such as sodium, magnesium and calcium are dissolved at the same time during the acid leaching treatment, and these impurities need to be removed. However, leaching under acidic conditions is difficult and the amount of residue is large, resulting in poor product purity and high cost, which seriously limits the market application of the acid leaching method. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preparing high-purity α-Al by a supercritical boiler fly ash aluminum sulfate salting method. 2 O 3 The method provided by the present invention can extract high-purity α-Al from fly ash at low cost. 2 O 3 .

[0005] In order to achieve the above object, the present invention provides the following technical solutions:

[0006] The present invention provides a method for preparing high-purity α-Al by using aluminum sulfate salting out method of supercritical boiler fly ash. 2 O 3 The method comprises the following steps:

[0007] (1) mixing the ball-milled fly ash with sulfuric acid for acid leaching to obtain a dissolution slurry;

[0008] (2) separating the solid and liquid of the leached slurry to obtain circulating sulfuric acid and leached material, wherein the circulating sulfuric acid is used in step (1);

[0009] (3) heating and mixing the leached material and the dissolving agent, and then separating the solid and liquid while hot to obtain a dissolved liquid and silicon slag;

[0010] (4) introducing hydrogen chloride gas into the dissolved liquid to carry out a precipitation reaction and then perform solid-liquid separation to obtain primary aluminum chloride crystals and a primary mother liquor;

[0011] (5) washing the primary aluminum chloride crystals with hydrochloric acid to obtain acid-washed primary aluminum chloride crystals;

[0012] (6) first mixing the acid-washed primary aluminum chloride crystals with an acid solution to obtain a first aluminum chloride solution, wherein the acid solution is hydrochloric acid or a hydrochloric acid azeotropic solution, and the temperature of the first mixing is 20-30° C.; evaporating the primary mother liquor to obtain hydrogen chloride gas and a primary distilled liquid; introducing the obtained hydrogen chloride gas into the first aluminum chloride solution for precipitation reaction and then performing solid-liquid separation to obtain secondary aluminum chloride crystals and a secondary mother liquor; evaporating the primary distilled liquid to obtain a hydrochloric acid azeotropic solution and dilute sulfuric acid, using the hydrochloric acid azeotropic solution as an acid solution, and concentrating the dilute sulfuric acid to obtain sulfuric acid for step (1);

[0013] (7) repeating step (6) for more than 3 times to purify the secondary aluminum chloride crystals, and then pyrolyzing the obtained aluminum chloride crystals to obtain basic aluminum chloride;

[0014] (8) The basic aluminum chloride and the seed crystal are mixed, ground, and then calcined to obtain a high-purity α-Al 2 O 3 , the purity is more than 99.98%.

[0015] Preferably, in step (1), the rotation speed of the ball mill is 200 to 300 rpm, the ball-to-material ratio is 3 to 5:1, and the ball milling time is 1 to 3 hours.

[0016] Preferably, in step (1), the acid leaching temperature is 230-250° C., and the leaching time is 180-300 min.

[0017] Preferably, in step (2), the temperature of the solid-liquid separation is 120-160°C.

[0018] Preferably, in step (3), the temperature of the heating and mixing is 70 to 90° C., and the insulation time is 0.5 to 1.5 h.

[0019] Preferably, in step (4), the temperature of the precipitation reaction is greater than or equal to 60°C until H + The concentration is greater than 11mol / L.

[0020] Preferably, in step (6), the temperature of the precipitation reaction is 50-70°C until H + The concentration is greater than 11mol / L.

[0021] Preferably, in step (6), when the hydrogen chloride gas is insufficient, it is prepared by using an acidifying liquid; the acidifying liquid is sulfuric acid and hydrochloric acid; the concentration of the sulfuric acid is above 85%; and the concentration of the hydrochloric acid is 30-36%.

[0022] Preferably, in step (7), the pyrolysis temperature is 400-650° C., and the insulation time is 60-120 min.

[0023] Preferably, in step (8), the calcination temperature is 1200-1250° C., the holding time is 120-240 min; and the mass ratio of the basic aluminum chloride to the seed crystal is 100:4-7.

[0024] The present invention provides a method for preparing high-purity α-Al by using aluminum sulfate salting out method of supercritical boiler fly ash. 2 O 3 The present invention has found that during the precipitation reaction, the yield of aluminum chloride hexahydrate crystals is related to the Cl - The present invention utilizes AlCl 3 6H 2 The above properties of O are used to remove impurities in aluminum chloride, and high-purity α-Al 2 O 3 The present invention combines the sulfuric acid method with the hydrochloric acid method to extract high-purity α-Al from fly ash. 2 O 3 The method has low cost, low energy consumption, simple operation, good safety and high product added value. At the same time, in the entire process, all materials can be recycled after being processed, which reduces production costs and overcomes technical problems such as the difficulty of fly ash leaching and the large amount of residue in the prior art. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0026] Figure 1 The present invention uses fly ash to prepare high-purity α-Al 2 O 3 Process flow chart of

[0027] Figure 2 The high-purity α-Al prepared in Example 1 2 O 3 XRD spectrum of

[0028] Figure 3The high-purity α-Al prepared in Example 1 2 O 3 TEM image of. DETAILED DESCRIPTION

[0029] The present invention provides a method for preparing high-purity α-Al by using aluminum sulfate salting out method of supercritical boiler fly ash. 2 O 3 The method comprises the following steps:

[0030] (1) mixing the ball-milled fly ash with sulfuric acid for acid leaching to obtain a dissolution slurry;

[0031] (2) separating the solid and liquid of the leached slurry to obtain circulating sulfuric acid and leached material, wherein the circulating sulfuric acid is used in step (1);

[0032] (3) heating and mixing the leached material and the dissolving agent, and then separating the solid and liquid while hot to obtain a dissolved liquid and silicon slag;

[0033] (4) introducing hydrogen chloride gas into the dissolved liquid to carry out a precipitation reaction and then perform solid-liquid separation to obtain primary aluminum chloride crystals and a primary mother liquor;

[0034] (5) washing the primary aluminum chloride crystals with hydrochloric acid to obtain acid-washed primary aluminum chloride crystals;

[0035] (6) first mixing the acid-washed primary aluminum chloride crystals with an acid solution to obtain a first aluminum chloride solution, wherein the acid solution is hydrochloric acid or a hydrochloric acid azeotropic solution, and the temperature of the first mixing is 20-30° C.; evaporating the primary mother liquor to obtain hydrogen chloride gas and a primary distilled liquid; introducing the obtained hydrogen chloride gas into the first aluminum chloride solution for precipitation reaction and then performing solid-liquid separation to obtain secondary aluminum chloride crystals and a secondary mother liquor; evaporating the primary distilled liquid to obtain a hydrochloric acid azeotropic solution and dilute sulfuric acid, using the hydrochloric acid azeotropic solution as an acid solution, and concentrating the dilute sulfuric acid to obtain sulfuric acid for step (1);

[0036] (7) repeating step (6) for more than 3 times to purify the secondary aluminum chloride crystals, and then pyrolyzing the obtained aluminum chloride crystals to obtain basic aluminum chloride;

[0037] (8) The basic aluminum chloride and the seed crystal are mixed, ground, and then calcined to obtain a high-purity α-Al 2 O 3 , the purity is more than 99.98%.

[0038] The present invention mixes the fly ash after ball milling with sulfuric acid for acid leaching to obtain a dissolution slurry. In the present invention, the rotation speed of the ball mill is preferably 200-300 rpm, more preferably 240-260 rpm, the ball-to-material ratio is preferably 3-5:1, more preferably 4:1, and the ball milling time is preferably 1-3 hours, more preferably 2 hours. The present invention obtains activated fly ash by ball milling.

[0039] In the present invention, the particle size of the fly ash after ball milling is preferably less than 74 microns, more preferably 0.01 to 50 microns, further preferably 1 to 30 microns, and further preferably 5 to 15 microns. The fly ash in the above particle size range is used in the present invention to improve the leaching effect.

[0040] In the present invention, the concentration of the sulfuric acid is preferably 85 wt % or more, more preferably 85 to 95 wt %, further preferably 88 to 93 wt %, and further preferably 90 wt %.

[0041] In the present invention, the ratio of the mass of the fly ash after ball milling to the volume of sulfuric acid is preferably 1g:(3-5)mL, more preferably 1g:(3.3-4.6)mL, further preferably 1g:(3.7-4.3)mL, and further preferably 1g:4mL.

[0042] In the present invention, the acid leaching temperature is preferably 230-250° C., more preferably 235-245° C., and the leaching time is preferably 180-300 min, more preferably 210-250 min.

[0043] After obtaining the dissolution slurry, the present invention separates the dissolution slurry into solid and liquid to obtain circulating sulfuric acid and leaching material, and the circulating sulfuric acid is used in step (1). In the present invention, the solid-liquid separation is preferably filtration; the pore size of the filtration is preferably 3 to 15 μm, more preferably 4.5 to 9 μm; the filtration is preferably filter press; the temperature of the solid-liquid separation is preferably 120 to 160° C., more preferably 130 to 150° C. The circulating sulfuric acid obtained by the present invention can be directly used as acid leaching in the next step (1).

[0044] After obtaining the circulating sulfuric acid and the leaching material, the present invention heats and mixes the leaching material with the dissolving agent, and then separates the solid and liquid while hot to obtain a dissolved solution and silicon slag. In the present invention, the dissolving agent is preferably dilute hydrochloric acid or water; the mass concentration of the dilute hydrochloric acid is preferably 15-24%, more preferably 18-20%; the water is preferably deionized water. The present invention uses dilute hydrochloric acid or water to dissolve the leaching material, and while separating the silicon slag, the rare metals in the leaching material are leached out as much as possible, and the amount of hydrogen chloride used in the subsequent precipitation reaction can also be reduced.

[0045] In the present invention, the ratio of the mass of the fly ash after ball milling to the volume of the dissolving agent is preferably 1 g: (3-4) mL, more preferably 1 g: (3.2-3.8) mL, and further preferably 1 g: (3.4-3.6) mL.

[0046] In the present invention, the temperature of the heating and mixing is preferably 70 to 90°C, more preferably 75 to 85°C, the holding time is preferably 0.5 to 1.5 hours, more preferably 0.8 to 1.2 hours; the heating and mixing is preferably stirring and mixing; the speed of the stirring and mixing is preferably 200 to 500 rpm, more preferably 350 to 400 rpm. The present invention converts aluminum sulfate in the leached material into aluminum chloride by heating and mixing, thereby separating silicon slag.

[0047] In the present invention, the hot solid-liquid separation is preferably hot filtration; the pore size of the hot filtration is preferably 3-15 μm, more preferably 4.5-9 μm; the temperature of the hot solid-liquid separation is preferably 70-90°C, more preferably 75-85°C.

[0048] After obtaining the dissolved solution and silicon slag, the present invention introduces hydrogen chloride gas into the dissolved solution for precipitation reaction and then solid-liquid separation to obtain primary aluminum chloride crystals and primary mother liquor. In the present invention, the introduction time of the hydrogen chloride gas is preferably 2 to 5 hours, more preferably 4 hours; the hydrogen chloride gas is preferably prepared by evaporating the mother liquor (including the primary mother liquor, the secondary mother liquor, and the last mother liquor) or by evaporating the acidified liquid (i.e., acidification).

[0049] In the present invention, the acidifying liquid is preferably sulfuric acid and hydrochloric acid; the concentration of the sulfuric acid is preferably above 85%, more preferably 85-90%; the concentration of the hydrochloric acid is preferably 30-36%, more preferably 32-34%; the volume ratio of hydrochloric acid to sulfuric acid is preferably 2:1; the method for preparing the hydrogen chloride gas is preferably: sulfuric acid is dripped into hydrochloric acid and then heated to obtain hydrogen chloride gas and dilute sulfuric acid.

[0050] In the present invention, the temperature of the precipitation reaction (referred to as precipitation reaction Z) is preferably greater than or equal to 60°C, more preferably 60-70°C, preferably until H + The concentration is greater than 11 mol / L, more preferably 12 to 12.5 mol / L.

[0051] In the present invention, the solid-liquid separation is preferably filtration; the pore size of the filtration is preferably 3 to 15 μm, more preferably 4.5 to 9 μm.

[0052] After obtaining the primary aluminum chloride crystals and the primary mother liquor, the present invention washes the primary aluminum chloride crystals with hydrochloric acid to obtain acid-washed primary aluminum chloride crystals. In the present invention, the concentration of hydrochloric acid used in the hydrochloric acid washing is preferably 32-38%, more preferably 34-38%, further preferably 34-36%, and further preferably 36%.

[0053] In the present invention, the ratio of the mass of the fly ash after ball milling to the volume of hydrochloric acid is preferably (1-2) g: (1-2) mL, more preferably (1-2) g: 1 mL, and further preferably 2 g: 1 mL. During washing, the primary aluminum chloride crystals are compacted in a funnel, and hydrochloric acid is poured in for filtering and washing.

[0054] In the present invention, the hydrochloric acid washing is preferably carried out based on the observation that the aluminum chloride crystals are colorless or light yellow after being dissolved in hydrochloric acid. The present invention uses hydrochloric acid washing after a precipitation reaction to wash away a large amount of impurities attached to the surface, thereby reducing the number of subsequent precipitation reactions.

[0055] After obtaining the pickled primary aluminum chloride crystals, the present invention first mixes the pickled primary aluminum chloride crystals with an acid solution to obtain a first aluminum chloride solution, wherein the acid solution is hydrochloric acid or a hydrochloric acid azeotropic solution. In the present invention, the concentration of the acid solution is preferably 16 to 24 wt%, more preferably 18 to 20 wt%, and further preferably 20 wt%; the hydrochloric acid azeotropic solution is obtained by distillation after evaporation of the primary mother liquor and / or the secondary mother liquor.

[0056] In the present invention, the ratio of the mass of the acid-washed primary aluminum chloride crystals to the volume of the acid solution is preferably 1 g: (1.8-2.0) mL, more preferably 1 g: (1.85-1.95) mL, and further preferably 1 g: 1.9 mL.

[0057] In the present invention, the temperature of the first mixing is preferably 22 to 30°C, more preferably 22 to 28°C, and further preferably 24 to 26°C.

[0058] In the present invention, the primary mother liquor is evaporated to obtain hydrogen chloride gas and a primary evaporation liquid. In the present invention, the evaporation temperature is preferably 105-110° C., more preferably 108-110° C., and the insulation time is preferably 2-5 hours, more preferably 4 hours. In the present invention, the hydrogen chloride gas obtained by evaporating the primary mother liquor is used for the subsequent precipitation reaction.

[0059] After obtaining hydrogen chloride gas and primary evaporation liquid, the present invention introduces the obtained hydrogen chloride gas into the first aluminum chloride solution for precipitation reaction and solid-liquid separation to obtain secondary aluminum chloride crystals and secondary mother liquor. In the present invention, the temperature of the precipitation reaction (referred to as precipitation reaction A) is preferably 50 to 70°C, more preferably 55 to 65°C, preferably until H +The concentration is greater than 11 mol / L, more preferably 11 to 12 mol / L, and even more preferably 11.5 mol / L.

[0060] In the present invention, the time for introducing the obtained hydrogen chloride gas is preferably 2 to 5 hours, more preferably 4 hours.

[0061] In the present invention, when the hydrogen chloride gas is insufficient, it is preferably prepared by acidizing liquid (i.e., acidification); the acidizing liquid is preferably sulfuric acid and hydrochloric acid; the concentration of the sulfuric acid is preferably 85% or more, more preferably 85-90%; the concentration of the hydrochloric acid is preferably 30-36%, more preferably 32-34%; the volume ratio of the hydrochloric acid to the sulfuric acid is preferably 2:1; the method for preparing the hydrogen chloride gas is preferably: sulfuric acid is dripped into hydrochloric acid and then heated to obtain hydrogen chloride gas and dilute sulfuric acid, the hydrogen chloride gas is used for precipitation reaction, and the dilute sulfuric acid is concentrated to obtain sulfuric acid for the preparation of the acidizing liquid or the acid leaching in step (1); the heating temperature is preferably 120°C. The present invention can provide hydrogen chloride gas and dilute sulfuric acid by dripping sulfuric acid into hydrochloric acid to drive out the hydrogen chloride gas in the hydrochloric acid, and the dilute sulfuric acid is concentrated into sulfuric acid, which can be used for the circulation of sulfuric acid in the acidizing liquid used in this step or the acid leaching in step (1).

[0062] In the present invention, the solid-liquid separation is preferably filtration; the pore size of the filtration is preferably 3 to 15 μm, more preferably 4.5 to 9 μm.

[0063] The present invention evaporates the primary evaporation liquid to obtain a hydrochloric acid azeotropic liquid and dilute sulfuric acid, uses the hydrochloric acid azeotropic liquid as an acid solution, and concentrates the dilute sulfuric acid to obtain sulfuric acid for step (1). In the present invention, the evaporation temperature is preferably 120 to 130° C., more preferably 125 to 130° C., and the insulation time is preferably 2 to 5 hours, more preferably 4 hours.

[0064] In the present invention, the concentration is preferably evaporation concentration; the evaporation temperature of the evaporation concentration is preferably 230-260°C, more preferably 240-250°C.

[0065] The present invention repeats step (6) for more than 3 times to purify the secondary aluminum chloride crystals, and then pyrolyzes the obtained aluminum chloride crystals to obtain basic aluminum chloride. In the present invention, the step (6) is repeated for more than 3 times, preferably 4 to 6 times, and more preferably 5 times. In the process of repeating step (6), when the hydrogen chloride gas is insufficient, it is preferably prepared (i.e., acidified) using an acidifying liquid; the acidifying liquid is preferably the same as the acidifying liquid in the precipitation reaction A, and will not be repeated here.

[0066] In the present invention, repeating step (6) three times preferably includes: subjecting the first aluminum chloride solution to precipitation reaction A, precipitation reaction B and precipitation reaction C in sequence; performing solid-liquid separation on the products obtained from the precipitation reaction A, precipitation reaction B or precipitation reaction C to obtain a secondary mother liquor, a tertiary mother liquor or a quaternary mother liquor; evaporating the secondary mother liquor or the tertiary mother liquor to obtain a hydrochloric acid azeotropic liquid A or a tertiary evaporation liquid; recycling the hydrochloric acid azeotropic liquid A as the acid solution in step (6), recycling the tertiary evaporation liquid as the hydrochloric acid azeotropic liquid or the dissolving agent in step (3); evaporating the quaternary mother liquor to obtain hydrogen chloride gas for the precipitation reaction in step (4) or step (6).

[0067] In the present invention, repeating the step (6) 4 times preferably includes: subjecting the first aluminum chloride solution to precipitation reaction A, precipitation reaction B, precipitation reaction C and precipitation reaction D in sequence; subjecting the products obtained from the precipitation reaction A, precipitation reaction B, precipitation reaction C or precipitation reaction D to solid-liquid separation to obtain a secondary mother liquor, a tertiary mother liquor, a quaternary mother liquor or a quintic mother liquor; evaporating the secondary mother liquor, the tertiary mother liquor or the quaternary mother liquor to obtain a hydrochloric acid azeotropic liquid A, a hydrochloric acid azeotropic liquid B or a tertiary evaporation liquid; recycling the hydrochloric acid azeotropic liquid A, the hydrochloric acid azeotropic liquid B and the quintic mother liquor as the acid solution in step (6), and recycling the tertiary evaporation liquid as the hydrochloric acid azeotropic liquid or the dissolving agent in step (3).

[0068] In the present invention, repeating the step (6) 5 times preferably comprises: subjecting the first aluminum chloride solution to precipitation reaction A, precipitation reaction B, precipitation reaction C, precipitation reaction D and precipitation reaction E in sequence; subjecting the products obtained from the precipitation reaction A, precipitation reaction B, precipitation reaction C, precipitation reaction D or precipitation reaction E to solid-liquid separation to obtain a secondary mother liquor, a tertiary mother liquor, a quaternary mother liquor, a quinary mother liquor or a sextuple mother liquor; subjecting the secondary mother liquor, the tertiary mother liquor, the quaternary mother liquor or the sextuple mother liquor to a reaction mixture containing the products of the precipitation reaction A, the precipitation reaction B, the precipitation reaction C, the precipitation reaction D or the precipitation reaction E; and subjecting the products to solid-liquid separation to solid-liquid separation to obtain a secondary mother liquor, a tertiary mother liquor, a quaternary mother liquor, a quinary mother liquor or a sextuple mother liquor. The mother liquors are evaporated respectively to obtain hydrochloric acid azeotropic liquid A, hydrochloric acid azeotropic liquid B, tertiary distilled liquid or quaternary distilled liquid respectively; the hydrochloric acid azeotropic liquid A, the hydrochloric acid azeotropic liquid B and the quaternary distilled liquid are recycled as the acid liquid in step (6) (the quaternary distilled liquid can also be recycled as the dissolution agent in step (3)), and the tertiary distilled liquid is recycled as the hydrochloric acid azeotropic liquid or the dissolution agent in step (3); the quaternary mother liquor is evaporated to obtain hydrogen chloride gas, which is used for the precipitation reaction in step (4) or step (6).

[0069] In the present invention, the pyrolysis temperature is preferably 400-650°C, more preferably 500-600°C, and the holding time is preferably 60-120 min, more preferably 80-100 min. The present invention obtains basic aluminum chloride through pyrolysis, and the purity reaches 4N.

[0070] In the present invention, the pyrolysis obtains basic aluminum chloride and hydrogen chloride gas at the same time; the hydrogen chloride gas is preferably absorbed by water and then used in step (6) as acid solution for recycling.

[0071] After obtaining the basic aluminum chloride, the present invention mixes the basic aluminum chloride with seed crystals, grinds them, and then calcines them to obtain high-purity α-Al 2 O 3 , with a purity of 99.98% or more. In the present invention, the mass ratio of the basic aluminum chloride to the seed crystal is preferably 100:4-7, more preferably 100:4.5-6.5, and further preferably 100:5-6.

[0072] In the present invention, the grinding is preferably ball milling; the ball milling ratio of the ball milling is preferably 4:1, and the ball milling time is preferably 2 hours.

[0073] In the present invention, the calcination temperature is preferably 1200-1250°C, more preferably 1210-1240°C, and further preferably 1220-1230°C, and the holding time is preferably 120-240 min, more preferably 150-210 min, and further preferably 180-200 min. 2 O 3 The process flow is as follows Figure 1 shown.

[0074] In order to further illustrate the present invention, the scheme of the present invention is described in detail below in conjunction with the accompanying drawings and embodiments, but they should not be understood as limiting the protection scope of the present invention.

[0075] Example 1

[0076] (1) Ball milling: ball milling the fly ash to obtain activated fly ash with a particle size of less than 200 mesh;

[0077] (2) Acid leaching: 120 g of the activated fly ash obtained in step (1) was mixed with 600 mL of sulfuric acid (85% by mass), and leached at 240° C. for 3 h to obtain a leached slurry;

[0078] (3) Filtration: filtering and separating the leached slurry from step (2) to obtain circulating sulfuric acid and leached material;

[0079] (4) Dissolution: Add 480 mL of hydrochloric acid (mass fraction: 20%) to the leached material in step (3) to dissolve the leached material, react at 80° C. for 30 min, and filter while hot to obtain a solution V. 1 and silicon slag;

[0080] (5) Aluminum chloride crystallization: At a temperature of 70°C, 500 mL of hydrochloric acid (32% by mass) was introduced into the solution of step (4) and heated to 108°C to obtain hydrogen chloride gas. The H + After concentration, acidification was performed, and the final solution contained H + The concentration reaches 13 mol / L; filtering and washing to obtain 180.4 g of primary aluminum chloride crystals and primary mother liquor;

[0081] (6) Aluminum chloride purification: Repeat the crystallization process 4 times:

[0082] ① At room temperature, the primary aluminum chloride crystals of step (5) are washed with 32% hydrochloric acid and then dissolved in 360 mL of hydrochloric acid azeotropic solution (the hydrochloric acid azeotropic solution remaining from the previous implementation of the method of the present invention) to obtain a first aluminum chloride solution, and the primary mother liquor of step (5) is evaporated to 108° C. to obtain hydrogen chloride gas and a primary distilled liquid, and the obtained hydrogen chloride gas is introduced into the first aluminum chloride solution for precipitation, and the H + The concentration reaches 11 mol / L, and after filtering, 102.7 g of secondary aluminum chloride crystals and a secondary mother liquor are obtained; the primary distilled liquid is further evaporated to obtain a hydrochloric acid azeotropic solution, dilute sulfuric acid and aluminum chloride containing impurities, and the obtained dilute sulfuric acid is further concentrated for acid leaching in step (2);

[0083] ② At room temperature, dissolve the secondary aluminum chloride crystals in step ① in 205 mL of hydrochloric acid azeotropic solution to obtain a second aluminum chloride solution. Evaporate the secondary mother liquor in step ① to 108°C to obtain hydrogen chloride gas and secondary distilled liquid. Pass the obtained hydrogen chloride gas into the second aluminum chloride solution to precipitate. After acidification, H + The concentration reaches 11.2 mol / L, and after filtering, 91.6 g of tertiary aluminum chloride crystals and tertiary mother liquor are obtained; the secondary distilled liquid is further evaporated to obtain hydrochloric acid azeotropic liquid and aluminum chloride containing impurities;

[0084] ③ At room temperature, dissolve the three aluminum chloride crystals in step ② in 185mL hydrochloric acid azeotropic solution to obtain the third aluminum chloride solution, evaporate the three mother liquors in step ② to 108°C to obtain hydrogen chloride gas and three distilled liquids, pass the obtained hydrogen chloride gas into the third aluminum chloride solution to precipitate, acidify and + The concentration reaches 11.3 mol / L, and after filtration, 89.4 g of aluminum chloride crystals and four mother liquors are obtained; the three distilled liquids are used as hydrochloric acid dissolution in step (4);

[0085] ④ At room temperature, dissolve the aluminum chloride crystals in step ③ in 180 mL of hydrochloric acid azeotropic solution to obtain a fourth aluminum chloride solution. Evaporate the fourth mother liquor in step ③ to 108°C to obtain hydrogen chloride gas and a fourth distilled liquid. Pass the obtained hydrogen chloride gas into the fourth aluminum chloride solution to precipitate. After acidification, H +The concentration reaches 11.8 mol / L, and after filtering, 89 g of five times aluminum chloride crystals and five times mother liquor are obtained; the four times distilled liquid is used as hydrochloric acid azeotropic liquid; the five times mother liquor is evaporated and used as hydrochloric acid azeotropic liquid;

[0086] (7) Pyrolysis: Pyrolyze the quintic aluminum chloride crystals obtained in step ④ at 600° C. for 120 min to obtain 21.2 g of basic aluminum chloride and hydrogen chloride gas. The obtained hydrogen chloride gas is absorbed by water and used as a hydrochloric acid azeotropic liquid.

[0087] (8) Calcination: Add 5% of the basic aluminum chloride obtained in step (7) to the seed crystals and grind them, then calcine them at 1250° C. for 240 min to obtain high-purity α-Al 2 O 3 16.5 g, purity 99.98%.

[0088] Example 2

[0089] (1) Ball milling: ball milling the fly ash to obtain activated fly ash with a particle size of less than 200 mesh;

[0090] (2) Acid leaching: 120 g of the activated fly ash obtained in step (1) was mixed with 600 mL of sulfuric acid (85% by mass), and leached at 240° C. for 4 h to obtain a leached slurry;

[0091] (3) Filtration: filtering and separating the leached slurry from step (2) to obtain circulating sulfuric acid and leached material;

[0092] (4) Dissolving: adding 450 mL of hydrochloric acid (mass fraction: 20%) to the leached material in step (3) to dissolve the leached material, reacting at 90° C. for 30 min, filtering while hot, and obtaining a dissolved solution and silicon slag;

[0093] (5) Aluminum chloride crystallization: At a temperature of 70° C., the hydrogen chloride gas obtained by evaporating the five mother liquors (the five mother liquors obtained by the previous implementation of the method of the present invention) in the solution of step (4) was passed through the solution to measure the H + After concentration, acidification was performed, and the final solution contained H + The concentration reaches 13 mol / L; filtering and washing to obtain 127.8 g of primary aluminum chloride crystals and primary mother liquor;

[0094] (6) Aluminum chloride purification: Repeat the crystallization process 3 times:

[0095] ① At room temperature, the primary aluminum chloride crystals of step (5) are dissolved in 255 mL of hydrochloric acid azeotropic solution (the hydrochloric acid azeotropic solution remaining from the previous implementation of the method of the present invention) to obtain a first aluminum chloride solution, and the primary mother liquor of step (5) is evaporated to 108° C. to obtain hydrogen chloride gas and a primary distilled liquid, and the obtained hydrogen chloride gas is introduced into the first aluminum chloride solution for precipitation, and after acidification, H +The concentration reaches 11.4 mol / L, and after filtering, 127 g of secondary aluminum chloride crystals and a secondary mother liquor are obtained; the primary distilled liquid is further evaporated to obtain a hydrochloric acid azeotropic solution, dilute sulfuric acid and aluminum chloride containing impurities, and the obtained dilute sulfuric acid is further concentrated for acid leaching in step (2);

[0096] ② At room temperature, the secondary aluminum chloride crystals of step ① are dissolved in 255 mL of hydrochloric acid azeotrope (hydrochloric acid azeotrope obtained in step ①) to obtain a second aluminum chloride solution, and the secondary mother liquor of step ① is evaporated to 108°C to obtain hydrogen chloride gas and a secondary distilled liquid, and the obtained hydrogen chloride gas is passed into the second aluminum chloride solution for precipitation, and after acidification, H + The concentration reaches 11.2 mol / L, and after filtering, 121.3 g of tertiary aluminum chloride crystals and tertiary mother liquor are obtained; the secondary distilled liquid is further evaporated to obtain a hydrochloric acid azeotropic liquid and aluminum chloride containing impurities;

[0097] ③ At room temperature, dissolve the three aluminum chloride crystals in step ② in 242 mL of hydrochloric acid azeotropic solution to obtain a third aluminum chloride solution, evaporate the three mother liquors in step ② to 108 ° C to obtain hydrogen chloride gas and three distilled liquids, pass the obtained hydrogen chloride gas into the third aluminum chloride solution to precipitate, acidify, and + The concentration reaches 11.3 mol / L, and after filtration, 119.7 g of aluminum chloride crystals and four mother liquors are obtained; the three distilled liquids are used as hydrochloric acid dissolution in step (4);

[0098] (7) Pyrolysis: Pyrolyze the aluminum quaternary chloride crystals obtained in step ③ at 650° C. for 60 min to obtain 23.8 g of basic aluminum chloride and hydrogen chloride gas. The obtained hydrogen chloride gas is absorbed by water and used as a hydrochloric acid azeotrope.

[0099] (8) Calcination: Add 5% of the basic aluminum chloride obtained in step (7) to the seed crystals and grind them, then calcine them at 1250° C. for 240 min to obtain high-purity α-Al 2 O 3 18.6 g, purity 99.98%.

[0100] Example 3

[0101] (1) Ball milling: ball milling the fly ash to obtain activated fly ash with a particle size of less than 200 mesh;

[0102] (2) Acid leaching: 150 g of the activated fly ash obtained in step (1) was mixed with 600 mL of sulfuric acid (85% by mass), and leached at 250° C. for 4 h to obtain a leached slurry;

[0103] (3) Filtration: filtering and separating the leached slurry from step (2) to obtain circulating sulfuric acid and leached material;

[0104] (4) Dissolving: adding 600 mL of hydrochloric acid (mass fraction: 20%) to the leached material in step (3) to dissolve the leached material, reacting at 80° C. for 30 min, filtering while hot, and obtaining a dissolved solution and silicon slag;

[0105] (5) Aluminum chloride crystallization: At a temperature of 70° C., four mother liquors (the four mother liquors remaining from the previous implementation of the method of the present invention) were introduced into the solution of step (4) to evaporate the resulting hydrogen chloride gas, and the H + After concentration, acidification was performed, and the final solution contained H + The concentration reaches 13 mol / L; filtering and washing to obtain 161.3 g of primary aluminum chloride crystals and primary mother liquor;

[0106] (6) Aluminum chloride purification: Repeat the crystallization process 4 times:

[0107] ① At room temperature, the primary aluminum chloride crystals of step (5) are dissolved in 325 mL of hydrochloric acid azeotropic solution (the hydrochloric acid azeotropic solution remaining from the previous implementation of the method of the present invention) to obtain a first aluminum chloride solution, and the primary mother liquor is evaporated to 108° C. to obtain hydrogen chloride gas and a primary distilled liquid, and the obtained hydrogen chloride gas is introduced into the first aluminum chloride solution for precipitation, and the H + The concentration reaches 11.2 mol / L, and after filtering, 124.7 g of secondary aluminum chloride crystals and a secondary mother liquor are obtained; the primary distilled liquid is further evaporated to obtain a hydrochloric acid azeotropic solution, dilute sulfuric acid and aluminum chloride containing impurities, and the obtained dilute sulfuric acid is further concentrated for acid leaching in step (2);

[0108] ② At room temperature, dissolve the secondary aluminum chloride crystals in step ① in 250 mL of hydrochloric acid azeotropic solution to obtain a second aluminum chloride solution, evaporate the secondary mother liquor in step ① to 108°C to obtain hydrogen chloride gas and secondary distilled liquid, pass the obtained hydrogen chloride gas into the second aluminum chloride solution for precipitation, and acidify to obtain H + The concentration reaches 11.2 mol / L, and after filtering, 111.3 g of tertiary aluminum chloride crystals and tertiary mother liquor are obtained; the secondary distilled liquid is further evaporated to obtain a hydrochloric acid azeotropic liquid and aluminum chloride containing impurities;

[0109] ③ At room temperature, dissolve the three aluminum chloride crystals in step ② in 223 mL of hydrochloric acid azeotropic solution to obtain a third aluminum chloride solution. Evaporate the three mother liquors in step ② to 108 ° C to obtain hydrogen chloride gas and three distilled liquids. Pass the obtained hydrogen chloride gas into the third aluminum chloride solution to precipitate. After acidification, H + The concentration reaches 11.3 mol / L, and after filtration, 108.7 g of aluminum chloride crystals and four mother liquors are obtained; the three distilled liquids are used as hydrochloric acid dissolution in step (4);

[0110] ④ At room temperature, dissolve the aluminum chloride crystals in step ③ in 217 mL of hydrochloric acid azeotropic solution to obtain a fourth aluminum chloride solution. Evaporate the fourth mother liquor in step ③ to 108 ° C to obtain hydrogen chloride gas and a fourth distilled liquid. Pass the obtained hydrogen chloride gas into the fourth aluminum chloride solution to precipitate. After acidification, H + The concentration reaches 11.5 mol / L, and after filtering, 108 g of five times aluminum chloride crystals and five times mother liquor are obtained; the four times distilled liquid is used as a hydrochloric acid azeotropic liquid; the five times mother liquor is used as a hydrochloric acid azeotropic liquid after evaporation;

[0111] (7) Pyrolysis: Pyrolyze the quintic aluminum chloride crystals from step ④ at 600° C. for 120 min to obtain 22.6 g of basic aluminum chloride and hydrogen chloride gas, which is then absorbed by water and used as a hydrochloric acid azeotrope;

[0112] (8) Calcination: Add 5% of the basic aluminum chloride obtained in step (7) to the seed crystals and grind them, then calcine them at 1250° C. for 240 min to obtain high-purity α-Al 2 O 3 16.8 g, purity 99.98%.

[0113] The high-purity α-Al prepared in Example 1 2 O 3 ICP-OES test was carried out according to GB / T37248-2018. The results are shown in Table 1.

[0114] Table 1 ICP-OES test results of Example 1

[0115]

[0116]

[0117] It can be seen from Table 1 that the high-purity α-Al prepared by the present invention 2 O 3 Less impurities and high purity.

[0118] The high-purity α-Al prepared in Example 1 2 O 3 XRD test was performed, and the results were as follows Figure 2 As shown. Figure 2 It can be seen that the Al 2 O 3 Mainly α phase.

[0119] The high-purity α-Al prepared in Example 1 2 O 3 TEM test results are as follows Figure 3 As shown. Figure 3 It can be seen that Al2 O 3 The microscopic appearance of the product is mainly worm-shaped, accompanied by ellipsoidal shape, and the surface is smooth.

[0120] It can be seen from the above examples that the method provided by the present invention can extract high-purity α-Al 2 O 3 , low cost, simple operation, realizes the high-value resource utilization of fly ash, and has broad market prospects.

[0121] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.

Claims

1. A method for preparing high-purity α-Al2O3 from supercritical boiler fly ash by aluminum sulfate salting out method, characterized in that: The following steps are involved: (1) mixing the ball-milled fly ash with sulfuric acid for acid leaching to obtain a dissolution slurry; (2) separating the solid and liquid of the leached slurry to obtain circulating sulfuric acid and leached material, wherein the circulating sulfuric acid is used in step (1); (3) heating and mixing the leached material and the dissolving agent, and then separating the solid and liquid while hot to obtain a dissolved liquid and silicon slag; (4) introducing hydrogen chloride gas into the dissolved liquid to carry out a precipitation reaction and then perform solid-liquid separation to obtain primary aluminum chloride crystals and a primary mother liquor; (5) washing the primary aluminum chloride crystals with hydrochloric acid to obtain acid-washed primary aluminum chloride crystals; (6) first mixing the acid-washed primary aluminum chloride crystals with an acid solution to obtain a first aluminum chloride solution, wherein the acid solution is hydrochloric acid or a hydrochloric acid azeotropic solution, and the temperature of the first mixing is 20-30° C.; evaporating the primary mother liquor to obtain hydrogen chloride gas and a primary distilled liquid; introducing the obtained hydrogen chloride gas into the first aluminum chloride solution for precipitation reaction and then performing solid-liquid separation to obtain secondary aluminum chloride crystals and a secondary mother liquor; evaporating the primary distilled liquid to obtain a hydrochloric acid azeotropic solution and dilute sulfuric acid, using the hydrochloric acid azeotropic solution as an acid solution, and concentrating the dilute sulfuric acid to obtain sulfuric acid for step (1); (7) repeating step (6) for more than 3 times to purify the secondary aluminum chloride crystals, and then pyrolyzing the obtained aluminum chloride crystals to obtain basic aluminum chloride; (8) The basic aluminum chloride and seed crystals are mixed, ground, and then calcined to obtain high-purity α-Al2O3 with a purity of more than 99.98%.

2. The method according to claim 1, characterized in that: In step (1), the rotation speed of the ball mill is 200-300 rpm, the ball-to-material ratio is 3-5:1, and the ball milling time is 1-3 hours.

3. The method according to claim 1 or 2, characterized in that: In step (1), the acid leaching temperature is 230-250° C., and the leaching time is 180-300 min.

4. The method according to claim 1, characterized in that: In step (2), the temperature of the solid-liquid separation is 120-160°C.

5. The method according to claim 1 or 2, characterized in that: In step (3), the temperature of the heating and mixing is 70 to 90° C., and the insulation time is 0.5 to 1.5 h.

6. The method according to claim 1, characterized in that In step (4), the temperature of the precipitation reaction is greater than or equal to 60°C until H + The concentration is greater than 11mol / L.

7. The method according to claim 1 or 6, characterized in that: In step (6), the temperature of the precipitation reaction is 50-70°C until H + The concentration is greater than 11mol / L.

8. The method according to claim 1 or 6, characterized in that: In step (6), when the hydrogen chloride gas is insufficient, it is prepared by using an acidifying liquid; the acidifying liquid is sulfuric acid and hydrochloric acid; the concentration of the sulfuric acid is above 85%; and the concentration of the hydrochloric acid is 30-36%.

9. The method according to claim 1 or 2, characterized in that: In step (7), the pyrolysis temperature is 400-650° C., and the insulation time is 60-120 min.

10. The method according to claim 1, characterized in that In step (8), the calcination temperature is 1200-1250° C., and the holding time is 120-240 min; the mass ratio of the basic aluminum chloride to the seed crystal is 100:4-7.

Citation Information

Patent Citations

  • Method using sulfuric acid activating and HCl (hydrogen chloride) crystallizing to jointly produce high-purity aluminum oxide

    CN106745131A

  • Method for preparing high-purity aluminum oxide from coal gangue

    CN112897560A